A treatment method and application of tungsten smelting dephosphorization slag

By treating tungsten smelting phosphorus removal slag through high-concentration alkali leaching and concentrated sulfuric acid activation, it solves the problems of high-temperature equipment and solid hazardous waste in the existing technology, achieves efficient phosphorus removal and secondary resource utilization of sodium tungstate solution, and reduces enterprise costs. and environmental pressure.

CN118637664BActive Publication Date: 2024-10-29CHONGYI ZHANGYUAN TUNGSTEN

Patent Information

Application Number
CN202411115038.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-10-29
Estimated Expiration
2044-08-14

AI Technical Summary

Technical Problem

The existing tungsten smelting phosphorus removal slag treatment method requires high-temperature equipment, requires additional phosphoric acid, and produces a large amount of solid hazardous waste, which increases enterprise costs and environmental pressure.

Method used

High-concentration alkali is used to leach WO3 from tungsten smelting phosphorus removal slag, and the activated slag is added to concentrated sulfuric acid for treatment. The activated slag is then used to remove phosphorus from sodium tungstate solution to achieve secondary resource utilization and reduce solid hazards. Waste emissions and cost of purchasing phosphorus removal reagents.

Benefits of technology

It achieves efficient recovery of sodium tungstate with low equipment requirements, reduces solid hazardous waste emissions and procurement costs, and the leached sodium tungstate solution can be directly used in the next process, which meets the requirements of the sodium tungstate phosphorus removal process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present invention belongs to the technical field of waste residue recycling, and specifically relates to a treatment method and application of tungsten smelting dephosphorization slag, wherein WO3 in tungsten smelting dephosphorization slag is directly recovered by high-concentration alkali leaching, and the leached sodium tungstate can be directly used without further dephosphorization operation; the dephosphorization slag after leaching WO3 is activated by adding concentrated sulfuric acid, and the activated dephosphorization slag can be used for dephosphorization with sodium tungstate solution. The present invention realizes the efficient utilization of secondary resources, reduces the emission of solid hazardous wastes of enterprises, is friendly to the social environment, and can save the cost of enterprises purchasing dephosphorization reagents.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of waste slag recycling, and specifically relates to a treatment method and application of tungsten smelting dephosphorization slag. Background Art

[0002] With the exhaustion of wolframite mining, scheelite has been widely used in the tungsten smelting industry. At present, the APT production process commonly used in China with tungsten concentrate as raw material is alkaline pressure cooking + ion exchange process. In order to solve the "calcium reversion phenomenon" that occurs during the alkaline decomposition of scheelite, which leads to high tungsten content in the slag, the alkaline decomposition process of tungsten concentrate has gradually developed into a phosphate decomposition process or a sodium hydroxide + phosphate combined decomposition process. In order to make the reaction fully proceed, the added phosphate generally needs to be excessive, which leads to excessive phosphate in the sodium tungstate solution obtained by decomposition. In order to ensure the phosphorus removal effect of the subsequent ion exchange process and the qualified P element of the ammonium paratungstate product finally produced, the general method used in industrial production is to directly add calcium salts (such as light calcium carbonate, calcium sulfate, calcium hydroxide, etc.) to the obtained sodium tungstate solution for phosphorus removal, so that the excess phosphate in the sodium tungstate solution is removed in the form of calcium phosphate or hydroxy calcium phosphate. The general process requires the tungsten-phosphorus ratio in the sodium tungstate to be greater than 1500. In order to ensure the dephosphorization effect, the addition coefficient of dephosphorization reagent is generally large, and a large amount of dephosphorization reagent is in excess in the dephosphorization slag. At the same time, in the dephosphorization process, some tungstates inevitably react with calcium salts to form calcium tungstate, which leads to 30-40wt% WO3 in the dephosphorization slag. This part of WO3 in the dephosphorization slag needs to be recycled. In addition, a lot of dephosphorization slag is produced. For example, a tungsten smelting plant with an annual output of 10,000 tons of ammonium paratungstate produces up to 600-800 tons of dephosphorization slag each year. As more scheelite is used, more dephosphorization slag will be produced. Since 2016, alkali decomposition tungsten smelting slag has been listed as hazardous waste, and it is stipulated that alkali decomposition tungsten smelting slag must be harmlessly treated, which undoubtedly increases the smelting cost of tungsten enterprises. The Chinese patent with announcement number CN103451434B proposes to immerse the dephosphorization slag produced by the dephosphorization process in the production process of ammonium paratungstate in water, with a liquid-solid ratio of water to dephosphorization slag of 4:1; then add caustic soda flakes and phosphoric acid, the reaction temperature is 170-190°C, and the temperature is kept for 0.5-2 hours after reaching the temperature. After the leached slag is washed, WO3≤1.5wt%. This method has a high reaction temperature for recovering WO3 from the dephosphorization slag, has high requirements for equipment, and requires additional addition of phosphoric acid, which will cause the leached sodium tungstate solution to continue the dephosphorization operation before it can be used. The dephosphorization slag after recovering WO3 is directly discarded for harmless treatment, which also increases the processing cost of the enterprise. Therefore, the existing method for treating tungsten smelting dephosphorization slag needs to be further improved. Summary of the invention

[0003] In order to solve the problems existing in the prior art, the main purpose of the present invention is to provide a treatment method and application of tungsten smelting dephosphorization slag.

[0004] To solve the above technical problems, according to one aspect of the present invention, the present invention provides the following technical solutions:

[0005] A method for treating tungsten smelting dephosphorization slag, comprising the following steps:

[0006] S1. Add water to the tungsten smelting dephosphorization slag and sodium hydroxide to make a slurry for leaching, filter and wash after cooling, and the slag after washing contains WO3 <1.0wt%;

[0007] S2. The washed slag is slurried with water, and then concentrated sulfuric acid is added for activation, followed by cooling and filtration. The activated slag is washed with water and then dried.

[0008] As a preferred embodiment of the method for treating tungsten smelting dephosphorization slag described in the present invention, wherein: in the step S1, the mass ratio of tungsten smelting dephosphorization slag to sodium hydroxide is 1:(0.4-0.6).

[0009] As a preferred embodiment of the method for treating tungsten smelting dephosphorization slag described in the present invention, wherein: in the step S1, the solid-liquid ratio of tungsten smelting dephosphorization slag to water is 1g: (0.8-1.2)mL.

[0010] As a preferred embodiment of the method for treating tungsten smelting dephosphorization slag described in the present invention, wherein: in the step S1, the leaching temperature is 110-130°C, and the leaching time is 1-2 hours.

[0011] As a preferred embodiment of the method for treating tungsten smelting dephosphorization slag described in the present invention, in step S2, the solid-liquid ratio of the washed slag to water is 1 g: (3-5) mL.

[0012] As a preferred embodiment of the method for treating tungsten smelting dephosphorization slag described in the present invention, in step S2, the concentration of concentrated sulfuric acid is 98wt%, and the liquid-solid ratio of concentrated sulfuric acid to the washed slag is (0.2-0.3)mL:1g.

[0013] As a preferred embodiment of the method for treating tungsten smelting dephosphorization slag described in the present invention, in step S2, the activation temperature is 60-90°C and the activation time is 1-3h.

[0014] To solve the above technical problem, according to another aspect of the present invention, the present invention provides the following technical solution:

[0015] A method for removing phosphorus from a sodium tungstate solution is disclosed. The activated slag obtained by the above treatment method is added into the sodium tungstate solution for removing phosphorus. The tungsten-phosphorus ratio in the sodium tungstate solution after the removal of phosphorus is greater than 1500.

[0016] As a preferred embodiment of the method for removing phosphorus from a sodium tungstate solution of the present invention, the amount of calcium sulfate dihydrate added is 3 to 5 times the theoretical consumption of the sodium tungstate solution for removing phosphorus, based on the calcium sulfate dihydrate in the activated slag.

[0017] As a preferred embodiment of the method for removing phosphorus from a sodium tungstate solution described in the present invention, the phosphorus removal temperature is 60 to 90° C., and the phosphorus removal time is 0.5 to 2.0 h.

[0018] The beneficial effects of the present invention are as follows:

[0019] The present invention proposes a treatment method and application of tungsten smelting dephosphorization slag, which directly uses a high-concentration alkali leaching method to recover WO3 in the tungsten smelting dephosphorization slag, and the leached sodium tungstate can be used directly without further dephosphorization operation; the dephosphorization slag after leaching WO3 is activated by adding concentrated sulfuric acid, and the activated dephosphorization slag can be used for dephosphorization in sodium tungstate solution. The present invention realizes the efficient utilization of secondary resources, reduces the emission of solid hazardous wastes of enterprises, is friendly to the social environment, and can save the cost of enterprises purchasing dephosphorization reagents. DETAILED DESCRIPTION

[0020] The following will be described clearly and completely in conjunction with the technical solutions in the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0021] The present invention proposes a treatment method and application of tungsten smelting dephosphorization slag, which has the following advantages:

[0022] (1) The method of the present invention is used to recover and treat tungsten trioxide in tungsten smelting dephosphorization slag. The equipment requirements are low, the metal recovery rate is high, and the recovered leached sodium tungstate solution has a low phosphorus content and can be directly used in the next process.

[0023] (2) After activation, the dephosphorization slag from tungsten smelting can continue to be used for dephosphorization, turning waste into treasure, achieving efficient utilization of secondary resources, reducing the emission of solid hazardous waste from enterprises, and being friendly to the social environment; at the same time, it can save the cost of enterprises purchasing dephosphorization reagents.

[0024] (3) Using concentrated sulfuric acid as an activator can fully utilize the principle of heat release during dilution of concentrated sulfuric acid, which can save energy and basically no additional heating is required during the reaction process.

[0025] According to one aspect of the present invention, the present invention provides the following technical solution:

[0026] A method for treating tungsten smelting dephosphorization slag, comprising the following steps:

[0027] S1. Add water to the tungsten smelting dephosphorization slag and sodium hydroxide to make a slurry for leaching, filter and wash after cooling, and the slag after washing contains WO3 <1.0wt%;

[0028] S2. The washed slag is slurried with water, and then concentrated sulfuric acid is added for activation, followed by cooling and filtration. The activated slag is washed with water and then dried.

[0029] Preferably, in step S1, the mass ratio of tungsten smelting dephosphorization slag to sodium hydroxide is 1:(0.4-0.6). Specifically, the mass ratio of tungsten smelting dephosphorization slag to sodium hydroxide can be, for example, any one of 1:0.4, 1:0.45, 1:0.5, 1:0.55, 1:0.6 or a range between any two thereof.

[0030] Preferably, in step S1, the solid-liquid ratio of tungsten smelting dephosphorization slag to water is 1g: (0.8-1.2)mL. Specifically, the solid-liquid ratio of tungsten smelting dephosphorization slag to water can be, for example, any one of 1g: 0.8mL, 1g: 0.9mL, 1g: 1mL, 1g: 1.1mL, 1g: 1.2mL, or a range between any two of them.

[0031] Preferably, in step S1, the leaching temperature is 110-130°C, and the leaching time is 1-2 hours. Specifically, the leaching temperature can be, for example, any one of 110°C, 115°C, 120°C, 125°C, 130°C, or a range between any two thereof.

[0032] Preferably, in step S2, the solid-liquid ratio of the washed residue to water is 1 g: (3-5) mL. Specifically, the solid-liquid ratio of water slurry can be, for example, any one of 1 g: 3 mL, 1 g: 3.5 mL, 1 g: 4 mL, 1 g: 4.5 mL, 1 g: 5 mL, or a range between any two of them.

[0033] Preferably, in step S2, the concentration of concentrated sulfuric acid is 98wt%, and the liquid-solid ratio of concentrated sulfuric acid to the washed slag is (0.2-0.3)mL:1g. Specifically, the liquid-solid ratio of concentrated sulfuric acid to the washed slag can be, for example, any one of 0.2mL:1g, 0.25mL:1g, 0.3mL:1g, or a range between any two of them.

[0034] Preferably, in step S2, the activation temperature is 60-90°C and the activation time is 1-3h. Specifically, the activation temperature can be, for example, any one of 60°C, 65°C, 70°C, 75°C, 80°C, 85°C, 90°C or a range between any two thereof.

[0035] According to another aspect of the present invention, the present invention provides the following technical solution:

[0036] A method for removing phosphorus from a sodium tungstate solution is disclosed. The activated slag obtained by the above treatment method is added into the sodium tungstate solution for removing phosphorus. The tungsten-phosphorus ratio in the sodium tungstate solution after the removal of phosphorus is greater than 1500.

[0037] Preferably, the amount of calcium sulfate dihydrate added is 3 to 5 times the theoretical consumption of sodium tungstate solution for phosphorus removal, based on the calcium sulfate dihydrate in the activated slag. The theoretical consumption of sodium tungstate solution for phosphorus removal is calculated by the reaction of phosphate in the sodium tungstate solution with calcium sulfate dihydrate to form calcium phosphate.

[0038] Specifically, based on the calcium sulfate dihydrate in the activated slag, the added amount can be, for example, 3 times, 3.5 times, 4 times, 4.5 times, 5 times, or any two of the theoretical consumption of sodium tungstate solution for phosphorus removal.

[0039] Preferably, the dephosphorization temperature is 60-90°C, and the dephosphorization time is 0.5-2.0 hours. Specifically, the dephosphorization temperature can be, for example, any one of 60°C, 70°C, 80°C, 90°C, or a range between any two thereof.

[0040] The technical solution of the present invention is further described below in conjunction with specific embodiments.

[0041] The composition of the tungsten smelting dephosphorization slag treated in each embodiment and comparative example is shown in the following table:

[0042]

[0043] Example 1

[0044] A method for treating tungsten smelting dephosphorization slag, comprising the following steps:

[0045] S1. 400g of tungsten smelting dephosphorization slag and 200g of sodium hydroxide were added to 400mL of water for slurry leaching. The leaching temperature was 120℃ and the leaching time was 2h. After cooling, the slag was filtered and washed. The slag after washing contained WO3: 0.62wt%;

[0046] S2, take 100g of washed slag and add 400mL of water to make slurry, then add 27mL of 98wt% concentrated sulfuric acid for activation, the activation temperature is 80℃, the activation time is 2h; then cool and filter, wash the activated slag with water, and then dry. The content of calcium sulfate dihydrate in the activated slag is 85wt%.

[0047] The activated slag obtained by the treatment method of this embodiment is subjected to phosphorus removal treatment with sodium tungstate solution:

[0048] Take 500mL sodium tungstate solution (P: 0.240g / L), and the amount added is 4 times the theoretical consumption of sodium tungstate solution for phosphorus removal, based on the calcium sulfate dihydrate in the activated slag, that is, add 4.70g of activated slag, the phosphorus removal temperature is 80℃, and the phosphorus removal time is 1.0h; filter, measure WO3:168.5g / L, P:0.025g / L in sodium tungstate solution, WO3:P=6740 in sodium tungstate, tungsten-phosphorus ratio>1500, which meets the requirements of sodium tungstate phosphorus removal process.

[0049] Example 2

[0050] A method for treating tungsten smelting dephosphorization slag, comprising the following steps:

[0051] S1. 400g of tungsten smelting dephosphorization slag and 200g of sodium hydroxide were added to 400mL of water for slurry leaching. The leaching temperature was 120℃ and the leaching time was 2h. After cooling, the slag was filtered and washed. The slag after washing contained WO3: 0.62wt%;

[0052] S2, take 100g of washed slag and add 500mL of water to make slurry, then add 27mL of 98wt% concentrated sulfuric acid for activation, the activation temperature is 90℃, the activation time is 3h; then cool and filter, wash the activated slag with water, and then dry. The content of calcium sulfate dihydrate in the activated slag is 85wt%.

[0053] The activated slag obtained by the treatment method of this embodiment is subjected to phosphorus removal treatment with sodium tungstate solution:

[0054] Take 500mL sodium tungstate solution (P: 0.240g / L), and the amount added is 5 times the theoretical consumption of sodium tungstate solution for phosphorus removal, based on the calcium sulfate dihydrate in the activated slag, that is, add 5.87g of activated slag, the phosphorus removal temperature is 80℃, and the phosphorus removal time is 1.0h; filter, measure WO3 in sodium tungstate solution: 166.5g / L, P: 0.019g / L, WO3 in sodium tungstate: P=8763, tungsten-phosphorus ratio>1500, which meets the requirements of sodium tungstate phosphorus removal process.

[0055] Example 3

[0056] A method for treating tungsten smelting dephosphorization slag, comprising the following steps:

[0057] S1. 400g of tungsten smelting dephosphorization slag and 160g of sodium hydroxide were added to 320mL of water for slurry leaching. The leaching temperature was 130℃ and the leaching time was 1h. After cooling, the slag was filtered and washed. The slag after washing contained WO3: 0.72wt%;

[0058] S2, take 100g of washed slag and add 300mL of water to make slurry, then add 22mL of 98wt% concentrated sulfuric acid for activation, the activation temperature is 60℃, the activation time is 3h; then cool and filter, wash the activated slag with water, and then dry. The content of calcium sulfate dihydrate in the activated slag is 82wt%.

[0059] The activated slag obtained by the treatment method of this embodiment is subjected to phosphorus removal treatment with sodium tungstate solution:

[0060] Take 500mL sodium tungstate solution (P: 0.240g / L), and the amount added is 3 times the theoretical consumption of sodium tungstate solution for phosphorus removal, based on the calcium sulfate dihydrate in the activated slag, that is, add 3.65g of activated slag, the phosphorus removal temperature is 80℃, and the phosphorus removal time is 0.5h; filter, measure WO3:170.2g / L, P:0.068g / L in sodium tungstate solution, WO3:P=2502 in sodium tungstate, tungsten-phosphorus ratio>1500, which meets the requirements of sodium tungstate phosphorus removal process.

[0061] Example 4

[0062] A method for treating tungsten smelting dephosphorization slag, comprising the following steps:

[0063] S1. 400g of tungsten smelting dephosphorization slag and 240g of sodium hydroxide were added to 480mL of water for slurry leaching. The leaching temperature was 120℃ and the leaching time was 2h. After cooling, the slag was filtered and washed. The slag after washing contained WO3: 0.65wt%;

[0064] S2, take 100g of washed slag and add 500mL of water to make slurry, then add 22mL of 98wt% concentrated sulfuric acid for activation, the activation temperature is 70℃, the activation time is 3h; then cool and filter, wash the activated slag with water, and then dry. The content of calcium sulfate dihydrate in the activated slag is 83wt%.

[0065] The activated slag obtained by the treatment method of this embodiment is subjected to phosphorus removal treatment with sodium tungstate solution:

[0066] Take 500mL sodium tungstate solution (P: 0.240g / L), and the amount added is 3 times the theoretical consumption of sodium tungstate solution for phosphorus removal, based on the calcium sulfate dihydrate in the activated slag, that is, add 3.61g of activated slag, the phosphorus removal temperature is 80℃, and the phosphorus removal time is 0.5h; filter, measure WO3:169.5g / L, P:0.058g / L in sodium tungstate solution, WO3:P=2955 in sodium tungstate, tungsten-phosphorus ratio>1500, which meets the requirements of sodium tungstate phosphorus removal process.

[0067] Comparative Example 1

[0068] The difference from Embodiment 1 is that step S2 is not performed.

[0069] The slag obtained by the comparative example treatment method is subjected to a sodium tungstate solution dephosphorization treatment:

[0070] Take 500mL sodium tungstate solution (P: 0.240g / L), add 4.70g of washed slag, the dephosphorization temperature is 80℃, and the dephosphorization time is 1.0h; filter, measure WO3:169.6g / L, P:0.225g / L in sodium tungstate solution, WO3:P=753 in sodium tungstate, tungsten-phosphorus ratio <1500, which does not meet the requirements of sodium tungstate dephosphorization process.

[0071] Comparative Example 2

[0072] The difference from Example 1 is that the activation temperature in step S2 is room temperature, and the content of calcium sulfate dihydrate in the activated slag is 40wt%.

[0073] The slag obtained by the treatment method of this comparative example is subjected to phosphorus removal treatment with sodium tungstate solution:

[0074] Take 500mL sodium tungstate solution (P: 0.240g / L), and the amount added is 4 times the theoretical consumption of sodium tungstate solution for phosphorus removal, based on the calcium sulfate dihydrate in the activated slag, that is, add 10.0g of activated slag, the phosphorus removal temperature is 80℃, and the phosphorus removal time is 1.0h; filter, measure WO3:154.6g / L, P:0.115g / L in sodium tungstate solution, WO3:P=1344 in sodium tungstate, tungsten-phosphorus ratio <1500, which does not meet the requirements of sodium tungstate phosphorus removal process.

[0075] Comparative Example 3

[0076] The difference from Example 1 is that the amount of sodium hydroxide in step S1 is 100 g.

[0077] The slag after washing in this comparative example contains WO3: 9.65wt%, and the slag contains high tungsten, and the purpose of recovering tungsten trioxide in the slag is not achieved.

[0078] Comparative Example 4

[0079] The difference from Example 1 is that the leaching temperature in step S1 is 90°C.

[0080] The slag after washing in this comparative example contains WO3: 15.6wt%, and the slag contains high tungsten, and the purpose of recovering tungsten trioxide in the slag is not achieved.

[0081] It can be seen from the above embodiments and comparative examples that the present invention directly uses a high-concentration alkali leaching method to recover WO3 from the tungsten smelting dephosphorization slag, and the leached sodium tungstate can be used directly without further dephosphorization operation; the dephosphorization slag after leaching WO3 is activated by adding concentrated sulfuric acid, and the activated dephosphorization slag can be used for dephosphorization in sodium tungstate solution. The present invention realizes the efficient utilization of secondary resources, reduces the emission of solid hazardous wastes of enterprises, is friendly to the social environment, and can save the cost of enterprises purchasing dephosphorization reagents.

[0082] The above description is only a preferred embodiment of the present invention, and does not limit the patent scope of the present invention. All equivalent structural changes made by using the contents of the present invention specification under the inventive concept of the present invention, or directly / indirectly applied in other related technical fields are included in the patent protection scope of the present invention.

Claims

1. A method for treating tungsten smelting dephosphorization slag, characterized in that: The steps include: S1. Add water to the tungsten smelting dephosphorization slag and sodium hydroxide to make a slurry for leaching, the leaching temperature is 110-130°C, and the leaching time is 1-2h; after cooling, filter and wash, the slag after washing contains WO3 <1.0wt%; S2. The washed slag is slurried with water, and then concentrated sulfuric acid is added for activation. The concentration of the concentrated sulfuric acid is 98wt%, and the liquid-solid ratio of the concentrated sulfuric acid to the washed slag is (0.2-0.3)mL:1g; the activation temperature is 60-90°C, followed by cooling and filtration, washing the activated slag with water, and then drying.

2. The method for treating tungsten smelting dephosphorization slag according to claim 1, characterized in that: In the step S1, the mass ratio of tungsten smelting dephosphorization slag to sodium hydroxide is 1: (0.4-0.6).

3. The method for treating tungsten smelting dephosphorization slag according to claim 1, characterized in that: In the step S1, the solid-liquid ratio of tungsten smelting dephosphorization slag to water is 1 g: (0.8-1.2) mL.

4. The method for treating tungsten smelting dephosphorization slag according to claim 1, characterized in that: In the step S2, the solid-liquid ratio of the washed residue to water is 1 g: (3-5) mL.

5. The method for treating tungsten smelting dephosphorization slag according to claim 1, characterized in that: In the step S2, the activation time is 1 to 3 hours.

6. A method for removing phosphorus from a sodium tungstate solution, characterized in that: The activated slag obtained by the treatment method according to any one of claims 1 to 5 is added into a sodium tungstate solution for dephosphorization, and the tungsten-phosphorus ratio in the sodium tungstate solution after dephosphorization is greater than 1500.

7. The method for removing phosphorus from a sodium tungstate solution according to claim 6, characterized in that: Calculated based on the calcium sulfate dihydrate in the activated slag, the added amount is 3 to 5 times the theoretical consumption of sodium tungstate solution for phosphorus removal.

8. The method for removing phosphorus from a sodium tungstate solution according to claim 6, characterized in that: The dephosphorization temperature is 60-90℃, and the dephosphorization time is 0.5-2.0h.

Citation Information

Patent Citations

  • A treatment method for tungsten smelting phosphorus removal slag

    CN103451434B

  • Treatment method for dephosphorized slag in tungsten metallurgy

    CN103451434A

  • Method for preparing white and high-purity anhydrous calcium sulfate by phosphogypsum

    CN105859167A

  • Method for efficiently leaching WO3 and MO in tungsten smelting dephosphorization slag

    CN114774717A

  • Method for leaching scheelite

    CN116121566A

Cited By

  • Method for recovering tungsten from aluminum salt phosphorus removal slag of sodium tungstate solution

    CN121294889A