Prepreg yarn, resin system for preparing prepreg yarn, preparation method and application thereof

By using epoxy resin, diluent, amino group curing agent and liquid dicyandiamide in the resin system of prepreg yarn, the problems of resin migration, uneven distribution and harsh storage conditions are solved, and the quality of prepreg yarn is improved. Excellent mechanical properties and storage stability, achieving a product effect that is non-sticky.

CN118638301BActive Publication Date: 2024-10-25SHENYANG OUSHIDUN NEW MATERIAL TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411117370.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-10-25
Estimated Expiration
2044-08-15

AI Technical Summary

Technical Problem

Existing prepreg yarns have problems with resin migration, uneven distribution, harsh storage conditions, and insufficient mechanical properties. In particular, the dry preparation method has problems such as discontinuous resin distribution, insufficient fiber penetration, and high low-temperature storage requirements.

Method used

A resin system is used, including epoxy resin, epoxy diluent, curing agent containing at least 2 amino groups and resin migration inhibitor B-liquid dicyandiamide, and is prepared through a specific process flow and component ratio. Pre-impregnated yarns that do not stick to your hands, have even resin distribution and strong mechanical properties can be stored at room temperature for a long time and remain stable in use.

Benefits of technology

The resin distribution of the prepreg yarn is even, the mechanical properties are improved, and the storage conditions are relaxed. The product is not sticky and can be stored for a long time at room temperature. The resin does not migrate, ensuring product quality and use effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118638301B_ABST
    Figure CN118638301B_ABST
Patent Text Reader

Abstract

The present application discloses a prepreg yarn, a resin system for preparing the prepreg yarn, and a preparation method and application thereof, and belongs to the technical field of composite materials for winding process. The resin system includes the following raw materials by weight: 140-190 parts of epoxy resin; 5-20 parts of epoxy diluent; 5-16 parts of curing agent containing at least 2 amino groups; resin migration inhibitor B; liquid dicyandiamide is prepared by the following method: after heating 11-20 parts of liquefaction agent, 7-12 parts of powdered dicyandiamide are added under high temperature conditions, and liquid dicyandiamide is obtained by high temperature stirring and reaction; the liquefaction agent is a compound containing an ether bond and an epoxy group in the molecular chain. The prepreg yarn obtained by impregnation with the resin is not sticky / wet, and the product experience is good; it can also be stored for a long time at room temperature; and whether it is stored at room temperature, thawed at low temperature, or transported or used, the resin in the prepreg yarn will not migrate, and the quality is high and the product has strong mechanical properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the technical field of composite materials for winding process, and relates to a prepreg yarn, a resin system for preparing the prepreg yarn, and a preparation method and application thereof. Background Art

[0002] Prepreg yarn is made of carbon fiber yarn that has been pre-impregnated and has been widely used in transportation, new energy, leisure and other fields. At present, the preparation of prepreg yarn at home and abroad adopts the method of cutting prepreg tape: the dry unidirectional prepreg narrow tape (yarn width 3.2mm and 6.3mm) used for laying silk is all unidirectional tape (width>1m) cut after melt coating. After cutting and winding, the continuous length of unidirectional fiber is less than 500m, and the process also requires isolation film separation protection. At present, all monofilament yarns on the market are obtained by wet preparation. They are sticky / wet when touched by hand, and the product experience is poor.

[0003] In addition, the prepreg yarn prepared by the wet method has the following shortcomings: 1) The resin system contains organic solvents such as acetone, which pollutes the environment and harms human health; 2) The storage conditions are more stringent: it must be stored at low temperature when not in use to ensure the stability of the resin in the prepreg yarn, and the low temperature requirements are high, and it must be below -18°C to be well stable; 3) The resin in the wet prepreg yarn is fluid, and it is easy to cause resin migration during transportation, room temperature, thawing after low-temperature storage, etc., and uneven distribution in the prepreg yarn, affecting product quality; 4) The mechanical properties need to be improved.

[0004] In the prior art, the dry preparation methods of prepreg yarn include hot melt resin method and powder method. Compared with wet prepreg, dry prepreg does not produce volatile gases during the production process, the process is environmentally friendly, reduces the maintenance time of production equipment, and improves process efficiency. However, there are the following shortcomings: 1) The powder method causes uneven and discontinuous distribution of resin in the prepreg yarn, and the fiber is not fully impregnated with resin, making it difficult to ensure product quality; the hot melt resin method is cumbersome and inefficient. 2) Currently, carbon fiber prepregs mainly use thermosetting materials-epoxy resins. The higher the temperature, the shorter the reaction and curing time. Therefore, the wound prepreg needs to be stored in a low temperature environment. Although the current low-temperature storage conditions of dry prepreg yarns are wider than those of wet prepreg yarns, they still need to be improved.

[0005] Therefore, the present application aims to solve the problems of resin migration, uneven distribution and harsh storage conditions in prepreg yarns, while improving its mechanical properties and ensuring that the obtained prepreg yarns are not sticky. At present, it is necessary to improve the process of dry-process prepreg yarn preparation to overcome the above technical problems. Summary of the invention

[0006] In order to solve the above problems, the present application provides a prepreg yarn, a resin system for preparing the prepreg yarn, and a preparation method and application thereof. The prepreg yarn obtained after the resin is impregnated is not sticky / wet, and the product experience is good; the continuous length of a single roll of prepreg yarn is greater than 4000mm (the specific length depends on the length of the raw material carbon fiber dry yarn), and no isolation film is required for separation and protection during the winding process; the storage conditions are low, and it can be stored for a long time at room temperature; and whether it is stored at room temperature, thawed at low temperature, or transported or used, the resin in the prepreg yarn will not migrate, and the distribution is uniform, the quality is high, and the product has strong mechanical properties.

[0007] The specific technical solutions of this application are as follows:

[0008] In one aspect, the present application provides a resin system for preparing prepreg yarn, which comprises the following raw materials in parts by weight:

[0009] Epoxy resin, 140-190 parts;

[0010] Epoxy diluent, 5-20 parts;

[0011] 5-16 parts of a curing agent containing at least 2 amino groups;

[0012] A resin migration inhibitor B, wherein the resin migration inhibitor B is liquid dicyandiamide;

[0013] The liquid dicyandiamide is prepared by the following method:

[0014] After heating 11 to 20 parts of a liquefaction agent, 7 to 12 parts of powdered dicyandiamide are added under high temperature conditions, and stirred and reacted at high temperature to obtain liquid dicyandiamide;

[0015] The liquefaction agent is a compound whose molecular chain contains an ether bond and an epoxy group.

[0016] The carbon fiber yarn includes large tow carbon fiber, such as 24k and 36k carbon fiber; small tow carbon fiber, such as 6k and 12k carbon fiber; high strength carbon fiber, such as T800-12k, T800-24K, T1000-12K; high modulus carbon fiber, such as 6k, 12k, and 24k of M46J and M50J. The yarn used is single-strand, and the rubber content of the single-strand yarn is precisely controlled.

[0017] Optionally, the epoxy resin includes bisphenol A epoxy resin.

[0018] Furthermore, the epoxy value of the bisphenol A epoxy resin is 0.51 to 0.53 eq / 100 g; the epoxy value of the butyl glycidyl ether is ≥ 0.60 eq / 100 g; and the epoxy value range of the resin system is 0.28 to 0.31 eq / 100 g.

[0019] Optionally, the liquefaction agent includes butyl glycidyl ether, phenyl glycidyl ether, benzyl glycidyl ether, and alkylene glycidyl ether.

[0020] Optionally, the curing agent includes alicyclic amine and polyether amine. Preferably, the alicyclic amine is at least one of 3,3'-dimethyl-4,4'-diamino-dicyclohexylmethane, methylcyclohexanediamine, and 5-amino-1,3,3-trimethylcyclohexylmethylamine;

[0021] Optionally, the epoxy diluent is at least one of 1,4-butanediol diglycidyl ether, polyethylene glycol diglycidyl ether, trimethylolpropane triglycidyl ether, propylene oxide phenyl ether, neopentyl glycol diglycidyl ether, and 4,5-epoxyhexane-1,2-dicarboxylic acid diglycidyl ether;

[0022] Optionally, dicyandiamide is added at 90-140° C., and then stirred and reacted at 140-170° C. for 1.5-3 hours to obtain liquid dicyandiamide.

[0023] On the other hand, the present application also provides a method for preparing the above resin system, comprising the following steps:

[0024] Step 1, after heating 11 to 20 parts of a liquefaction agent, add 7 to 12 parts of powdered dicyandiamide at 90 to 140° C., and then stir and react at 140 to 170° C. for 1.5 to 3 hours to obtain liquid dicyandiamide;

[0025] Step 2: After cooling the liquid dicyandiamide to room temperature, add 5 to 16 parts of accelerator, 140 to 190 parts of epoxy resin, 5 to 20 parts of epoxy diluent and 5 to 16 parts of curing agent, stir well to obtain a resin system.

[0026] Optionally, the accelerator is at least one of imidazoles, tertiary amines and hydrazides;

[0027] The imidazole is any one of 2-ethyl-4-methylimidazole and 1-aminoethyl-2-methylimidazole; the tertiary amine includes DMP-30; and the hydrazide is any one of succinic acid dihydrazide and adipic acid dihydrazide.

[0028] On the other hand, the present application also provides the use of the above resin system in a dry prepreg yarn process.

[0029] On the other hand, the present application also provides a prepreg yarn prepared using the resin system obtained above, wherein the prepreg yarn is prepared by the following steps:

[0030] Step 1: Pour the resin system into the glue tank of the prepreg equipment;

[0031] Step 2, roll the carbon fiber yarn onto the air expansion shaft of the tension machine, and the carbon fiber yarn passes through the tension control frame of the tension machine, the first high-aluminum porcelain tube of the first oven, and the yarn spreading roller assembly at a speed of 8-10 meters per minute, and then transitions to the yarn guide roller. The rubber roller arranged above the rubber groove is driven by the carbon fiber yarn to move clockwise, and drives the pressure rubber roller arranged above the rubber roller to move counterclockwise. The rubber roller brings out the resin glue in the glue groove and concentrates it between the rubber roller and the pressure rubber roller. The rear carbon fiber yarn will be coated with resin glue when passing through this area; the rubber roller coats and infiltrates the resin glue into the surface layer of the carbon fiber yarn; the pressure rubber roller and the rubber roller jointly fully infiltrate the resin glue into the carbon fiber yarn, and then enter the second high-aluminum porcelain tube in the second oven in turn for B-stage treatment, and then the carbon fiber yarn enters the refrigeration box for cooling to obtain pre-impregnated yarn, and then goes to the winding machine for winding, and the winding speed is 8-10 meters per minute;

[0032] Among them, the resin mass proportion in the carbon fiber yarn composite layer after impregnation is between 21 and 24%; during use, the heating temperature of the glue tank is 35 to 40°C, and the viscosity of the glue is controlled between 900 and 1100 MPa·s.

[0033] The temperature in the first oven is 68-73° C., the temperature in the second oven is 60-65° C., and the winding speed is maintained at 8-10 m / min within the temperature range of the second oven.

[0034] A temperature control detection component capable of detecting the temperature value in the second oven is arranged at the end of the second oven.

[0035] On the one hand, the epoxy diluent added in the present application can reduce the viscosity of the system and improve the wettability; on the other hand, the toughening group - ether bond (flexible group) contained in the diluent of the present application will make the entire cured system have good toughness after compounding, and this toughness will improve the strength of the entire composite material.

[0036] In the production practice, the resin system needs a storage period to meet the demand for preparing prepreg yarn at any time. And the mechanical properties of the prepreg yarn obtained after prepreg during the storage period must be 100% exerted, that is, the strength of the fiber can be 100% exerted. The present application combines a curing agent containing at least 2 amino groups with B-dicyandiamide, an inhibitor of resin migration. It not only ensures the potential (storage period) of the prepreg yarn, which can be stored in a semi-cured state at room temperature, but also ensures that the prepreg yarn has good strength.

[0037] The beneficial effects of this application include but are not limited to:

[0038] 1. The present application combines liquid dicyandiamide and a curing agent containing at least two amino groups in the resin system, which not only ensures the latent property (storage period) of the prepreg yarn, but also ensures that the prepreg yarn has good mechanical properties; and the obtained prepreg yarn is not sticky. The reason is that, on the one hand, after adding dicyandiamide, the curing effect between the epoxy resin and the curing agent can be inhibited at room temperature, and the obtained resin system has a certain latent property; on the other hand, the combination of liquid dicyandiamide and a curing agent containing at least two amino groups can increase the molecular weight of components such as bisphenol A epoxy resin and diluent, so that the resin system reaches a semi-solid state, thereby achieving the prepreg yarn that feels dry to the touch, is in a semi-solid state, and is not sticky to the touch.

[0039] The addition of another curing agent containing at least two amino groups can enable the yarn to complete the B-stage conversion at a faster speed during the winding process after the dipping is completed (i.e., semi-curing is completed in the second oven process, and cooling and winding are completed after coming out), so that the prepreg yarn feels dry and does not stick to the hands.

[0040] 2. The present application further limits the epoxy value of the epoxy resin. On the one hand, the epoxy resin under a specific epoxy value can be fully mixed with other components to achieve better pre-impregnation of the yarn; on the other hand, the yarn is controlled to have a suitable residual epoxy value after the B-stage treatment after the dipping is completed, thereby ensuring that the pre-impregnated yarn can successfully complete semi-curing in the second oven to obtain a non-stick pre-impregnated yarn.

[0041] 3. In the present application, dicyandiamide is liquefied and added to the resin system, so that the resin can be 100% filled during the curing and cross-linking reaction without causing defects. The surface of the obtained resin system will be very transparent and the strength will be better.

[0042] Furthermore, a specific medium - a compound whose molecular chain contains an ether bond and an epoxy group - is selected to prepare liquefied dicyandiamide, which reacts with dicyandiamide to form an intermediate with a suitable viscosity, can be fully mixed with the epoxy system, and has a good effect of wetting the yarn. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] The drawings described herein are used to provide a further understanding of the present application and constitute a part of the present application. The illustrative embodiments of the present application and their descriptions are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:

[0044] Figure 1 This is the process flow diagram of this application;

[0045] Figure 2 for Figure 1 Enlarged view of part A.

[0046] List of parts and reference numerals:

[0047] 1 tension machine air expansion shaft, 2 tension machine, 3 tension control frame, 4 first high aluminum porcelain tube, 5 first oven, 6 yarn spreading roller assembly, 7 glue tank, 8 resin glue, 9 rubber roller, 10 second oven, 11 second high aluminum porcelain tube, 12 temperature control detection assembly, 13 refrigeration box, 14 winder, 15 winder air expansion shaft, 16 rubber pressure roller, 17 carbon fiber yarn, 18 yarn guide roller. DETAILED DESCRIPTION

[0048] The present application is described in detail below with reference to embodiments, but the present application is not limited to these embodiments.

[0049] The resin obtained in the embodiment is used to impregnate the yarn in the following process flow device:

[0050] like Figure 1 As shown, the process flow device includes a tension machine 2, a first oven 5, an impregnation machine, a second oven 10, a refrigeration box 13, and a winding machine 14 connected in sequence by a conveyor belt; the tension machine 2 includes a tension machine air expansion shaft 1 and a tension control frame 3; a first high-aluminum porcelain tube 4 is arranged inside the first oven 5; the impregnation machine includes a yarn spreading roller assembly 6, a glue tank 7 for holding resin glue 8, a rubber roller 9, and a rubber pressing roller 16; a second high-aluminum porcelain tube 11 and a temperature control detection assembly 12 are arranged inside the second oven 10; and a winding machine air expansion shaft 15 is arranged in the winding machine 14. A temperature control detection assembly 12 that can detect the temperature value in the second oven 10 is arranged at the end of the second oven 10.

[0051] The operating principles of the local components of the device that are not expanded in detail are well known in the art and will not be described in detail.

[0052] Example 1

[0053] The resin system for preparing the prepreg yarn comprises the following raw materials in parts by weight:

[0054] 140 parts of bisphenol A epoxy resin; 20 parts of epoxy diluent (1,4-butanediol diglycidyl ether); 5 parts of curing agent (methylcyclohexanediamine); Resin migration inhibitor B: liquid dicyandiamide;

[0055] The liquid dicyandiamide is prepared by the following method:

[0056] After heating 20 parts of butyl glycidyl ether, 12 parts of powdered dicyandiamide were added at 90°C, and then stirred and reacted at 140°C for 1.5 hours to obtain liquid dicyandiamide.

[0057] Among them, the epoxy value of bisphenol A epoxy resin is 0.51eq / 100g; the epoxy value of butyl glycidyl ether is ≥0.60eq / 100g.

[0058] The resin system for preparing the prepreg yarn is prepared by the following method:

[0059] According to the above formula, after the liquid dicyandiamide is cooled to room temperature, an accelerator (2-ethyl-4-methylimidazole), bisphenol A epoxy resin, epoxy diluent (1,4-butanediol diglycidyl ether) and a curing agent (methylcyclohexanediamine) are added, and the mixture is fully stirred to obtain a resin system.

[0060] A dry prepreg yarn is prepared by the following method:

[0061] Step 1: Pour the resin system (about 700 g) into the glue tank 7 of the prepreg equipment;

[0062] Step 2: Roll the T700 grade 12k small-tow carbon fiber yarn 17 (original yarn) onto the tension machine air expansion shaft 1 of the tension machine 2. The carbon fiber yarn 17 passes through the tension control frame 3 of the tension machine 2, the first high-aluminum porcelain tube 4 of the first oven 5, and the yarn spreading roller assembly 6 at a speed of 8 meters per minute, and then transitions to the yarn guide roller 18. The rubber roller 9 arranged above the glue groove 7 is driven by the carbon fiber yarn 17 to move clockwise, driving the rubber pressure roller 16 arranged above the rubber roller 9 to move counterclockwise, and the rubber roller 9 brings out the resin glue 8 in the glue groove 7 and concentrates it on the belt. Between the rubber roller 9 and the pressure rubber roller 16, the rear carbon fiber yarn 17 will be coated with resin glue 8 when passing through this area; the rubber roller 9 coats and impregnates the resin glue 8 into the surface of the carbon fiber yarn 17; the pressure rubber roller 16 and the rubber roller 9 jointly fully impregnate the resin glue 8 into the carbon fiber yarn 17, and then successively enter the second high-aluminum porcelain tube 11 in the second oven 10 for B-stage treatment, and then the carbon fiber yarn 17 enters the refrigeration box 13 for cooling to obtain pre-impregnated yarn, and then goes to the winding machine 14 for winding, and the winding speed is 8 to 10 meters / minute.

[0063] Among them, the resin mass proportion in the composite layer of the carbon fiber yarn 17 after impregnation is 23%; during use, the heating temperature of the glue tank 7 is 35° C., and the viscosity of the glue is controlled to be around 1000 mpa·s.

[0064] The temperature in the first oven 55 is 70° C., the temperature in the second oven 1010 is 60° C., and the winding speed is maintained at 8 m / min within the temperature of the second oven 1010.

[0065] Principle: The purpose of drying the carbon fiber yarn 17 for the first time is to dry the carbon fiber yarn 17 and remove moisture absorbed by the carbon fiber yarn 17 during storage. The dried carbon fiber yarn 17 has good surface bonding with the resin after curing. Figure 2 As shown, after the carbon fiber yarn 17 comes out of the drying box, it reaches the yarn spreading roller assembly 6 (as shown in FIG. Figure 2The yarn spreading roller assembly 6 is composed of 5 yarn spreading rollers. By adjusting a single yarn spreading roller on the yarn spreading roller assembly 6 structure, the yarn spreading roller assembly 6 structure can fully spread the carbon fiber yarn 17 under tension, so that the several strands of carbon fiber yarn 17 can be dispersed, which is convenient for the subsequent transition to the yarn guide roller 18 (the yarn guide roller 18 is for transmission). After that, the resin is fully infiltrated between the several strands, so that the carbon fiber yarn 17 is fully impregnated. Figure 2 The carbon fiber yarn 17 is shown to be located between the rubber roller 9 and the rubber pressure roller 16; the carbon fiber yarn 17 is transmitted to the right, and under the action of tension and friction, the carbon fiber yarn 17 will drive the rubber roller 9 to move clockwise. At this moment, the rubber pressure roller 16 above will be driven to rotate counterclockwise, and the rubber roller 9 will bring out the resin in the glue tank 7 and concentrate it between the rubber roller 9 and the rubber pressure roller 16. The carbon fiber yarn 17 behind will be coated with resin glue 8 when passing through this area. Cylinders are also provided at both ends of the glue pressing to control the gap between the rubber pressure roller 16 and the rubber roller 9 and also apply downward force to press the resin into the carbon fiber yarn 17, and then pass through the yarn guide roller 18 to exit the glue dipping tank 7.

[0066] Example 2

[0067] The resin system for preparing the prepreg yarn comprises the following raw materials in parts by weight:

[0068] 190 parts of bisphenol A epoxy resin; 5 parts of epoxy diluent (polyethylene glycol diglycidyl ether and trimethylolpropane triglycidyl ether are compounded in a weight ratio of 1:1); 16 parts of curing agent (5-amino-1,3,3-trimethylcyclohexylmethylamine); resin migration inhibitor B: liquid dicyandiamide;

[0069] The liquid dicyandiamide is prepared by the following method:

[0070] After heating 11 parts of butyl glycidyl ether, 7 parts of powdered dicyandiamide were added at 140°C, and then stirred and reacted at 170°C for 3 hours to obtain liquid dicyandiamide.

[0071] Among them, the epoxy value of bisphenol A epoxy resin is 0.53eq / 100g; the epoxy value of butyl glycidyl ether is ≥0.60eq / 100g.

[0072] The resin system for preparing the prepreg yarn is prepared by the following method:

[0073] According to the above formula, after the liquid dicyandiamide is cooled to room temperature, an accelerator (2-ethyl-4-methylimidazole), bisphenol A epoxy resin, epoxy diluent and curing agent are added, and the mixture is fully stirred to obtain a resin system.

[0074] A dry prepreg yarn is prepared by the following method:

[0075] Step 1: Pour the resin system into the glue tank 7 of the prepreg equipment;

[0076] Step 2: The resin mass ratio in the yarn composite layer after impregnation is 21%, and the rest is the same as in Example 1.

[0077] Example 3

[0078] The resin system for preparing the prepreg yarn comprises the following raw materials in parts by weight:

[0079] 172 parts of bisphenol A epoxy resin; 16 parts of epoxy diluent (1,4-butanediol diglycidyl ether); 10 parts of curing agent (5-amino-1,3,3-trimethylcyclohexylmethylamine); resin migration inhibitor B: liquid dicyandiamide;

[0080] The liquid dicyandiamide is prepared by the following method:

[0081] After heating 17 parts of butyl glycidyl ether, 10 parts of powdered dicyandiamide were added at 123°C, and then stirred and reacted at 166°C for 2 hours to obtain liquid dicyandiamide.

[0082] Among them, the epoxy value of bisphenol A epoxy resin is 0.52eq / 100g; the epoxy value of butyl glycidyl ether is ≥0.60eq / 100g.

[0083] The resin system for preparing the prepreg yarn is prepared by the following method:

[0084] According to the above formula, after the liquid dicyandiamide is cooled to room temperature, an accelerator (2-ethyl-4-methylimidazole), bisphenol A epoxy resin, epoxy diluent and curing agent are added, and the mixture is fully stirred to obtain a resin system.

[0085] A dry prepreg yarn is prepared by the following method:

[0086] Step 1: Pour the resin system into the glue tank 7 of the prepreg equipment;

[0087] Step 2: Step 2: The resin mass proportion in the yarn composite layer after impregnation is 24%, and the rest is the same as Example 1.

[0088] Example 4

[0089] The resin system used to prepare the prepreg yarn is different from that in Example 1 in that the epoxy value of the bisphenol A epoxy resin is 0.65 eq / 100 g. The rest is the same as in Example 1.

[0090] The preparation method of the resin system is the same as that of Example 1.

[0091] A dry prepreg yarn, the preparation method is the same as that of Example 1.

[0092] Example 5

[0093] The resin system used to prepare the prepreg yarn is different from that in Example 1 in that the epoxy value of the bisphenol A epoxy resin is 0.4 eq / 100 g. The rest is the same as in Example 1.

[0094] The preparation method of the resin system is the same as that of Example 1.

[0095] A dry prepreg yarn, the preparation method is the same as that of Example 1.

[0096] Example 6

[0097] The resin system used to prepare the prepreg yarn is the same as that in Example 1. The preparation method of the resin system is the same as that in Example 1.

[0098] A dry prepreg yarn, which differs from Example 1 in that the mass proportion of resin in the composite layer is 26%.

[0099] Example 7

[0100] The resin system used to prepare the prepreg yarn is different from that in Example 1 in that the epoxy resin is different from that in Example 1 and is bisphenol H epoxy resin. The preparation method of the resin system is the same as that in Example 1.

[0101] Example 8

[0102] The resin system used to prepare the prepreg yarn is different from that in Example 1 in that the epoxy resin is 4,4-diaminodiphenylmethane tetraglycidylamine. The preparation method of the resin system is the same as that in Example 1.

[0103] Comparative Example 1

[0104] The resin system used to prepare the prepreg yarn is different from that in Example 1 in that only bisphenol A epoxy resin, epoxy diluent, and curing agent are added to the resin system, and B-dicyandiamide, a resin migration inhibitor, is not added. The rest is the same as in Example 1.

[0105] The preparation method of the resin system is the same as that of Example 1.

[0106] A dry prepreg yarn, the preparation method is the same as that of Example 1.

[0107] Comparative Example 2

[0108] The resin system used to prepare the prepreg yarn is different from that in Example 1 in that the liquid dicyandiamide is replaced by 4,4-diaminodiphenyl sulfone. The rest is the same as in Example 1.

[0109] The preparation method of the resin system is the same as that of Example 1.

[0110] A dry prepreg yarn, the preparation method is the same as that of Example 1.

[0111] Comparative Example 3

[0112] The resin system used to prepare the prepreg yarn is different from that in Example 1 in that no curing agent is added to the resin system. The rest is the same as in Example 1.

[0113] The preparation method of the resin system is the same as that of Example 1.

[0114] A dry prepreg yarn, the preparation method is the same as that of Example 1.

[0115] Comparative Example 4

[0116] The resin system used to prepare the prepreg yarn is different from that in Example 1 in that the added curing agent is 3,3'-diethyl-4,4'-diaminodiphenylmethane. The rest is the same as in Example 1.

[0117] The preparation method of the resin system is the same as that of Example 1.

[0118] A dry prepreg yarn, the preparation method is the same as that of Example 1.

[0119] Comparative Example 5

[0120] The resin system used to prepare the prepreg yarn is different from that in Example 1 in that butyl glycidyl ether is replaced with 4,5-epoxyhexane-1,2-dicarboxylic acid diglycidyl ester. The rest is the same as in Example 1.

[0121] The preparation method of the resin system is the same as that of Example 1.

[0122] A dry prepreg yarn, the preparation method is the same as that of Example 1.

[0123] Comparative Example 6

[0124] The resin system used to prepare the prepreg yarn is different from that in Example 1 in that powdered solid dicyandiamide is added. The rest is the same as in Example 1.

[0125] The preparation method of the resin system is the same as that of Example 1.

[0126] A dry prepreg yarn, the preparation method is the same as that of Example 1.

[0127] The prepreg yarns prepared in the above embodiments and comparative examples were tested for indicators, and the results are shown in Table 1:

[0128] The following method is used to determine whether the resin in the prepreg yarn has migrated: a 300 mm long fiber bundle is taken from the upper, middle and lower parts of the prepreg yarn roll, and the weight is measured. If the upper part is light and the lower part is heavy, it is determined that the resin has migrated; if the weight of the upper, middle and lower parts is the same (with almost no difference), it is determined that the resin is stable and no migration has occurred.

[0129]

[0130]

[0131] Conclusion analysis: According to the above table, the dry prepreg obtained in the embodiment can be stored for a long time at room temperature. In order to further increase the storage period, it is refrigerated at low temperature. The low temperature refrigeration condition is wider than that of the dry prepreg, -8 to 20 ° C. Whether at room temperature or during thawing, the resin in the prepreg will not sink or migrate, and it is always in a semi-solid state. At the same time, it has higher mechanical properties.

[0132] The Nohl ring of T700 carbon fiber yarn 17 (not pre-impregnated) and the resin system has a Nohl ring tensile strength of 2350MPa and a Nohl ring shear strength of 38MPa. Under this condition, the bursting strength of the cylinder after winding will meet the design requirements. The T700 carbon fiber yarn 17 pre-impregnated yarn wrapped Nohl ring prepared in this embodiment 1 of the present application has a Nohl ring tensile strength of 2475MPa and a Nohl ring shear strength of 52MPa. Therefore, it is believed that the mechanical properties of the pre-impregnated yarn obtained after pre-impregnation during the storage period can be 100% exerted.

[0133] Compared with Comparative Example 1, the prepreg in the embodiment can have a storage period / buffer period because dicyandiamide contains a cyano structure and has a relatively low activity. It is not easy to react at room temperature, which inhibits the curing effect between the epoxy resin and the curing agent. The resin and the curing agent are cured and cross-linked in a short time, and the resin system will harden in a short time, and it is impossible to have a storage period / buffer period to meet the needs of preparing prepreg at any time.

[0134] Compared with Comparative Example 2, the prepreg in the embodiment has a longer shelf life and better mechanical properties. The reason is that: the structure of dicyandiamide contains three isocyanate structures, which makes dicyandiamide highly stable. During the reaction, its stable structure must be broken first before the reaction can proceed; although 4,4-diaminodiphenyl sulfone (a sulfonyl diamide curing agent) is also a low-activity substance, it has been found in practice that the long-term storage stability of the primary amine group in its molecular structure is lower than that of dicyandiamide. In addition, 4,4-diaminodiphenyl sulfone is a crystalline powder that cannot be liquefied. After mixing with the epoxy resin system, it is unevenly dispersed, the system viscosity is high, and the curing cross-linking density is high, which is manifested as brittle resin and poor toughness, resulting in poor structural mechanical properties of the composite material product after curing.

[0135] The combined results of Comparative Examples 1 and 2 indicate that not all resin systems prepared with low-activity substances can produce prepregs with long storage life and strong mechanical properties after impregnating carbon fiber yarns 17.

[0136] Compared with comparative example 3, the prepreg in the embodiment is not sticky / wet when touched by hand, and the resin does not migrate in the prepreg and is evenly distributed. The reason is that after the addition of alicyclic amine, the molecular weight of components such as bisphenol A epoxy resin and diluent increases, so that the resin system reaches a semi-solid state, which makes the prepreg feel dry, a semi-solid state, and non-sticky when touched by hand. This semi-solid state prevents the prepreg in the embodiment of the present application from dripping under the action of gravity at room temperature, and the resin of the entire material is evenly distributed, so that room temperature storage is achieved. When directly heated during later use, it will become a molten state, showing a viscous flow state, with low and limited fluidity, and uniform glue content in the composite layer, so that the prepreg obtained after solidification with the increase of temperature will have a better fitting effect between the interfaces of several layers when in use.

[0137] Compared with comparative example 4, the prepreg in the embodiment can achieve the effect of not getting your hands dirty on the surface and has a longer storage period. The reason is that the curing agent 3,3'-diethyl-4,4'-diaminodiphenylmethane has a slightly lower activity and cannot complete the B-stage conversion within the process temperature range and winding speed, resulting in the fiber surface still being dirty when winding; and during the storage stage after winding, the curing agent 3,3'-diethyl-4,4'-diaminodiphenylmethane has no latency and will slowly react and cure until the system reaches a semi-solid state, while the winding has been completed at this time, resulting in the prepreg yarn being unable to be unwound and becoming ineffective.

[0138] Based on Comparative Examples 3 and 4, it is shown that not all combinations of curing agents and dicyandiamide can produce a semi-cured resin system.

[0139] Compared with Examples 4-5, the mechanical properties and quality of the prepreg in Examples 1-3 are better, because the viscosity of the resin system under this epoxy value is appropriate, and it can be fully mixed with other components, and the obtained resin system has a better wetting effect on the yarn. If the epoxy value of the original resin is too large, the remaining epoxy value in the B-stage treatment of the prepreg is large, and the prepreg will be sticky and cannot reach a semi-solid state; if the epoxy value of the original resin is small, the viscosity of the mixed resin system is too large during the dipping stage, which is not conducive to uniform and sufficient dipping of the prepreg.

[0140] Compared with Comparative Example 5, the dicyandiamide in the embodiment can be liquefied and can be used for the subsequent preparation of prepreg yarn. The reason is that the glycidyl ether with multiple epoxy functional groups used in Comparative Example 7 often has a large degree of structural crosslinking in the process of reacting with dicyandiamide to form an intermediate, which will cause the viscosity of the intermediate of the polyepoxy glycidyl ether / ester and dicyandiamide to be too high, and may be semi-solid or even solid, which loses the purpose of convenient use of dicyandiamide after liquefaction and mixing with the epoxy system and impregnating the fiber. The applicant has found that the above problem can be overcome / does not exist in the process of reacting with dicyandiamide to form an intermediate.

[0141] Compared with Comparative Example 6, the prepreg in the embodiment has better mechanical properties and lower viscosity of the resin system. The reason is that liquid dicyandiamide is easy to mix with epoxy resin, and can better reduce the viscosity of the system, better infiltrate, and disperse more evenly than powdered dicyandiamide; in the process of curing and cross-linking reaction, the resin can be 100% filled without causing defects, and the surface of the obtained resin system will be very transparent and the strength will be better. However, after mixing powdered dicyandiamide with liquid resin, there will be an electrostatic effect, which is easy to agglomerate and unevenly dispersed. In the process of curing and cross-linking reaction, residual particles in the system will cause pore defects, thereby reducing the strength of the body.

[0142] Example 8

[0143] Based on the above results, epoxy resin, epoxy diluent, curing agent containing at least 2 amino groups, and resin migration inhibitor B (liquid dicyandiamide) were selected as components of the resin system for preparation. However, it is difficult for the applicant to control the stability of the resin in the prepreg in a good semi-cured state (i.e., it is not sticky and can be rolled up) during the preparation of the prepreg, which is unstable.

[0144] The applicant has found in practice that when the epoxy value of the resin system is controlled within a specific range, it will show a better semi-cured state (i.e., it is not sticky and can be rolled up). See the screening test results in Table 2 for details:

[0145] Table 2 Epoxy value of mixed resin system

[0146]

[0147] According to Table 2 above, when the epoxy value in the resin system is in the range of 0.28 to 0.31 eq / 100 g, the semi-solid state of the entire system is most suitable, and the prepared prepreg will not stick to your hands at room temperature of 25°C. If the epoxy value is greater than 0.31 eq / 100 g, it will stick to your hands. If the epoxy value is less than 0.28 eq / 100 g, the prepreg will be relatively brittle. During the winding process of the prepreg for storage, there will be a phenomenon of localized slag / fragments (resin slag or slag / fragments of the composite material after fiber dipping).

[0148] The resin system after the epoxy resin and the diluent are mixed in the present application has a certain range of epoxy value, and the resin system at this time is relatively dilute, about 0.58eq / 100g. The applicant has found that adding alicyclic amine can consume part of the epoxy value, and when adding dicyandiamide consumes the epoxy value in the system, the remaining range is 0.28 to 0.31eq / 100g, and the semi-solid state of the entire system is the most suitable.

[0149] In practice, it is found that when the weight ratio of epoxy diluent: epoxy diluent: curing agent: liquefaction agent: powdered dicyandiamide in the resin system is 140-190: 5-20: 5-16: 11-20: 7-12, the epoxy value of the resin system can be controlled in the range of 0.28-0.31eq / 100g.

[0150] It is not easy for a technician in this field to think of controlling the epoxy value of the mixed resin system within a specific range of 0.28 to 0.31 eq / 100g by adding specific components in a specific ratio to achieve a better curing state (ie, not sticky and able to be rolled up).

[0151] Example 5

[0152] Regarding the influence of the pre-impregnation process on the pre-impregnation effect, the present application conducted the following screening experiment on the yarn at the B stage after pre-impregnation (the process in the second oven 10 after the completion of the glue tank 7 dipping), and the results are shown in Table 3:

[0153] Table 3 Effect of prepreg yarn heating path length and temperature on prepreg yarn quality

[0154]

[0155] According to the above table, when the temperature of the second oven 10 is between 60 and 65°C (the oven temperature determines the B-stage temperature of the prepreg yarn), the oven length is 2m (i.e., the length of the prepreg yarn heating path), and the winding speed is 8 to 10 m / min (the winding speed and the oven length determine the B-stage treatment time of the prepreg yarn), the semi-solid prepreg yarn after cooling has the best effect. At this time, it is not sticky and can be wound up; otherwise, in this oven temperature range, if the winding speed is fast, the process is incomplete, and the surface of the cooled prepreg yarn is still sticky.

[0156] The above is only the embodiment of the present application, and the protection scope of the present application is not limited by these specific embodiments, but is determined by the claims of the present application. For those skilled in the art, the present application can have various changes and variations. Any modification, equivalent replacement, improvement, etc. made within the technical ideas and principles of the present application should be included in the protection scope of the present application.

Claims

1. A resin system for preparing prepreg yarn, characterized in that: By weight, it includes the following raw materials: Epoxy resin, 140-190 parts; Epoxy diluent, 5-20 parts; 5 to 16 parts of a curing agent containing at least 2 amino groups; A resin migration inhibitor B, wherein the resin migration inhibitor B is liquid dicyandiamide; The liquid dicyandiamide is prepared by the following method: After heating 11 to 20 parts of a liquefaction agent, add 7 to 12 parts of powdered dicyandiamide at 90 to 140° C., and react at 140 to 170° C. with stirring for 1.5 to 3 hours to obtain liquid dicyandiamide; The liquefaction agent is butyl glycidyl ether; the epoxy value of the butyl glycidyl ether is ≥ 0.60eq / 100g; The epoxy resin is bisphenol A epoxy resin; The epoxy value of the bisphenol A epoxy resin is 0.51-0.53 eq / 100 g; the epoxy value of the resin system is in the range of 0.28-0.31 eq / 100 g; The curing agent is an alicyclic amine; the alicyclic amine is at least one of 3,3'-dimethyl-4,4'-diamino-dicyclohexylmethane, methylcyclohexanediamine, and 5-amino-1,3,3-trimethylcyclohexylmethylamine; The epoxy diluent is at least one of 1,4-butanediol diglycidyl ether, polyethylene glycol diglycidyl ether, trimethylolpropane triglycidyl ether, propylene oxide phenyl ether, neopentyl glycol diglycidyl ether, and 4,5-epoxyhexane-1,2-dicarboxylic acid diglycidyl ether.

2. A method for preparing a resin system as claimed in claim 1, characterized in that: The steps include: Step 1, after heating 11 to 20 parts of a liquefaction agent, add 7 to 12 parts of powdered dicyandiamide at 90 to 140° C., and then stir and react at 140 to 170° C. for 1.5 to 3 hours to obtain liquid dicyandiamide; Step 2: After cooling the liquid dicyandiamide to room temperature, add 5 to 16 parts of accelerator, 140 to 190 parts of epoxy resin, 5 to 20 parts of epoxy diluent and 5 to 16 parts of curing agent, stir well to obtain a resin system.

3. Use of the resin system as claimed in claim 1 in a dry prepreg process.

4. A prepreg yarn prepared using the resin system as claimed in claim 1, characterized in that: The prepreg yarn is prepared by the following steps: Step 1, pouring the resin system into the glue tank (7) of the prepreg equipment; Step 2: Roll the carbon fiber yarn (17) onto the tension machine air expansion shaft (1), and the carbon fiber yarn (17) passes through the tension control frame (3) of the tension machine (2), the first high-aluminum porcelain tube (4) of the first oven (5), and the yarn spreading roller assembly (6) at a speed of 8-10 m / min, and then transitions to the yarn guide roller (18). The rubber roller (9) arranged above the glue groove (7) is driven by the carbon fiber yarn (17) to move clockwise, driving the rubber pressure roller (16) arranged above the rubber roller (9) to move counterclockwise, and the rubber roller (9) brings out the resin glue (8) in the glue groove (7) and concentrates it on the rubber roller (9) and the pressure glue. The carbon fiber yarn (17) behind is coated with resin glue (8) when passing through this area; the adhesive roller (9) coats and impregnates the surface of the carbon fiber yarn (17) with the resin glue (8); the pressure roller (16) and the adhesive roller (9) jointly fully impregnate the carbon fiber yarn (17) with the resin glue (8), and then successively enter the second high-aluminum porcelain tube (11) in the second oven (10) for B-stage treatment, and then the carbon fiber yarn (17) enters the refrigeration box (13) for cooling to obtain pre-impregnated yarn, and then enters the winding machine (14) for winding, and the winding speed is 8 to 10 meters per minute; The resin mass proportion in the composite layer of the impregnated carbon fiber yarn (17) is between 21% and 24%. During use, the heating temperature of the glue tank (7) is 35 to 40°C, and the viscosity of the glue is controlled to be between 900 and 1100 mPa·s. The temperature in the first oven (5) is 68 to 73°C, and the temperature in the second oven (10) is 60 to 65°C. The winding speed is maintained at 8 to 10 m / min within the temperature range of the second oven (10), and the length of the second oven (10) is 1.8 to 2.3 m.