A high-performance modified PET culture medium bottle and preparation method thereof
By combining polyvinyl chloride resin with PET resin and chemically reacting with additives, a porous foam carbon layer and an inorganic heat insulation layer are formed, which solves the barrier and flammability problems of PET materials and achieves PET culture medium bottles with high barrier, flame retardancy and oxidation resistance.
Patent Information
- Application Number
- CN202410666538.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-28
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-05-28
AI Technical Summary
Existing PET resin materials have insufficient barrier properties, are flammable, and antioxidants are easily lost, affecting the transparency and performance of the materials.
It uses polyvinyl chloride resin and PET resin composite, and adds additives containing nitrogen, phosphorus and silicon elements. Through chemical reaction, a porous foam carbon layer and an inorganic heat insulation layer are formed to improve barrier and flame retardancy. At the same time, hindered phenol and hindered amine structures provide antioxidant properties.
It achieves high barrier properties, excellent flame retardancy and oxidation resistance in PET culture medium bottles, while maintaining the transparency and stable mechanical properties of the material.
Smart Images

Figure BDA0004861266450000032 
Figure BDA0004861266450000033 
Figure BDA0004861266450000041
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polymer materials, and in particular, relates to a high-performance modified PET culture medium bottle and a preparation method thereof. Background Art
[0002] PET resin is made by polycondensation of terephthalic acid and ethylene glycol. It has excellent performance and its share in packaging materials for food, beverage, chemical, pharmaceutical, cosmetics and other industries is on a straight upward trend. It accounts for 37% of all materials in the global beverage packaging market. The reason why PET has been so widely developed as a packaging material is that it has the following excellent properties: (1) Stable chemical properties: good corrosion resistance; (2) High mechanical strength: no damage when dropped, high compression and shock resistance. (3) Light weight: can significantly reduce transportation and circulation costs; (4) Good hygienic properties: it is a green and environmentally friendly product that meets FDA hygienic standards; (5) Good transparency: because the light transmittance can reach 90%; (6) Recyclable: As people's environmental awareness is increasing, whether the material can be recycled and reused has become one of the important bases for material selection in the industry.
[0003] At present, PET has gradually begun to replace traditional packaging materials and become an important packaging material. PET culture medium bottle packaging materials can be prepared from PET resin, but the barrier property of PET resin is not high enough and cannot meet the requirements of high barrier packaging materials such as PET culture medium bottles. To further expand its use, its barrier property must be improved. Patent CN116063832A discloses a method for increasing the barrier property of PET. The scheme is to blend 70-80 parts of PET, 20-30 parts of polylactic acid, 1-5 parts of nano titanium dioxide, 3-5 parts of antioxidant, 1-2 parts of nano calcium carbonate, 1-1.5 parts of silane coupling agent, and 0.1-0.5 parts of graphene oxide composite. The barrier reason is that graphene oxide, calcium carbonate and titanium dioxide are used as fillers, which cooperate with each other and are evenly distributed in the material, extending the permeation path of water and oxygen molecules and improving the barrier performance of the product. However, inorganic fillers are non-transparent and transparent PET materials cannot be obtained, thus limiting its application.
[0004] PET resin materials are flammable, and when burning, they produce serious dripping and harmful smoke, and the dripping can cause secondary hazards, which limits its application range. In addition, in the prior art, the antioxidant in the PET material is only physically mixed in the raw materials, and there is no chemical reaction between the antioxidant and the other raw materials. Therefore, the antioxidant is easily affected by the external environment and gradually lost, and loses its function, so that the PET material will gradually turn yellow and become brittle, which will not only affect the appearance effect, but also have a serious impact on the use. Summary of the invention
[0005] The purpose of the present invention is to overcome the defects of the prior art and provide a high-performance modified PET culture medium bottle and a preparation method thereof.
[0006] The purpose of the present invention can be achieved through the following technical solutions:
[0007] A high-performance modified PET culture medium bottle, comprising the following raw materials in parts by weight: 70-80 parts of PET resin, 10-15 parts of polyvinyl chloride resin, 2-6 parts of amino silicone oil, 2-4 parts of auxiliary agent, 2-5 parts of plasticizer, and 0.02-0.04 parts of initiator;
[0008] Polyvinyl chloride is a polymer formed by the polymerization of vinyl chloride monomers according to the free radical polymerization mechanism. Polyvinyl chloride has the advantage of effectively blocking water vapor, oxygen, odor and grease. Compounding polyvinyl chloride resin with PET resin can effectively improve the barrier properties of PET culture medium bottles.
[0009] Furthermore, the auxiliary agent is prepared by the following steps:
[0010] S1. Blow nitrogen gas into a dry three-necked flask for 30 minutes to drive away the air in the flask, then add 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane, triethylamine and methanol under nitrogen protection, stir and dissolve, slowly add 4-chloro-1-butene, heat to 80°C and react for 3 hours. After the reaction is completed, cool to room temperature and distill under reduced pressure to obtain intermediate 1; the dosage ratio of 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane, 4-chloro-1-butene, triethylamine and methanol is 13.8mL:5.6mL:11.5mL:120mL;
[0011] Under the action of triethylamine, the molar ratio of 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane to 4-chloro-1-butene is controlled to be 1:1.05-1.1. One -NH 2 It undergoes a nucleophilic substitution reaction with the -Cl of 4-chloro-1-butene. The reaction process is as follows:
[0012]
[0013] S2. Add flame retardant FRC-2 (3-[(hydroxymethyl)amino]-3-oxopropylphosphonic acid-dimethyl ester) and DMSO (dimethyl sulfoxide) to a dry three-necked flask under nitrogen protection, stir thoroughly, and then slowly add a mixed solution of intermediate 1 and DMSO. After the addition is completed, heat to 120° C. and react for 2 h. After the reaction is completed, cool to room temperature and distill under reduced pressure to obtain intermediate 2. The amount ratio of flame retardant FRC-2, intermediate 1 and DMSO is 10.1 mL:19.8 g:200 mL.
[0014] Under heating conditions, the molar ratio of flame retardant FRC-2 and intermediate 1 is controlled to be 1:1.05-1.1, then flame retardant FRC-2 and intermediate 1 undergo the following chemical reaction, and the reaction equation is as follows:
[0015]
[0016] S3, under nitrogen protection, add intermediate 2, 2-(2,2,6,6-tetramethylpiperidin-4-yl)acetic acid and DMSO into a four-necked flask, stir until completely dissolved, then slowly add concentrated sulfuric acid, stir and heat to 110°C for reaction for 3h, cool to room temperature after the reaction, add sodium bicarbonate solution for neutralization, shake and stand for stratification, take the organic phase, dry it with anhydrous magnesium sulfate, filter, and distill the filtrate under reduced pressure to obtain intermediate 3; the amount ratio of intermediate 2, 2-(2,2,6,6-tetramethylpiperidin-4-yl)acetic acid, concentrated sulfuric acid and DMSO is 16.9g:8.2g:2.5mL:220mL;
[0017] Under concentrated sulfuric acid and heating conditions, the molar ratio of intermediate 2 and 2-(2,2,6,6-tetramethylpiperidin-4-yl)acetic acid is controlled to be 1:1.1-1.2, then -OH of intermediate 2 and -COOH of 2-(2,2,6,6-tetramethylpiperidin-4-yl)acetic acid undergo esterification reaction, and the reaction process is as follows:
[0018]
[0019] S4. Add intermediate 3, triethylamine and DMF (N,N-dimethylformamide) to a dry three-necked flask under nitrogen protection, stir and dissolve, slowly add a mixed solution of 2,6-di-tert-butyl-4-bromomethylphenol and DMF, heat to 90°C and react for 4 hours, cool to room temperature after the reaction, and distill under reduced pressure to obtain an auxiliary agent. The dosage ratio of intermediate 3, 2,6-di-tert-butyl-4-bromomethylphenol, triethylamine and DMF is 16.6g:8.2g:5.5mL:200mL.
[0020] Under the action of triethylamine, the molar ratio of intermediate 3 to 2,6-di-tert-butyl-4-bromomethylphenol is controlled to be 1:1.05-1.1, and -NH- of intermediate 3 and -Br of 2,6-di-tert-butyl-4-bromomethylphenol undergo nucleophilic substitution reaction. The reaction process is as follows:
[0021]
[0022] The phosphorus element in the additive provides an acid source, reacts with the polymer resin, and promotes the formation of carbonized products; the nitrogen element provides a gas source, which can make the system expand and foam, and also promotes the formation of the carbonized layer to form porous foam carbon; the silicon element generates an inorganic heat-insulating and insulating protective layer containing -Si-O bonds and -Si-C- bonds during combustion, which not only prevents the decomposition products generated by combustion from escaping, but also inhibits the thermal decomposition of the polymer material, achieving the purpose of high flame retardancy, low smoke emission, and low harmfulness. The additive of the present invention exerts an efficient and safe flame retardant effect through the synergistic effect of the halogen-free flame retardant elements nitrogen, phosphorus, and silicon, thereby making the PET culture medium bottle of the present invention have excellent flame retardancy.
[0023] The hindered phenol structure in the additive can provide hydrogen atoms to the free radicals to terminate the chain reaction, or directly combine with the active free radicals to form new relatively stable free radicals, thereby destroying any step in the free radical reaction process, playing a protective role, and maintaining the stability of the appearance and mechanical properties of the material. The hindered amine structure in the additive can decompose hydroperoxides and convert them into harmless substances; the hindered amine structure also has a very strong free radical capture ability, can neutralize and stabilize free radicals, and prevent polymer chain breakage reactions caused by free radicals; in addition, the hindered amine structure also has regeneration ability, that is, it can restore its own stability after the free radical capture reaction, so as to continue to play a role. The additive of the present invention exerts an antioxidant effect through the synergistic effect of the hindered phenol structure and the hindered amine structure, thereby making the PET culture medium bottle of the present invention have excellent antioxidant properties.
[0024] According to similar compatibility, the benzene ring, heterocyclic ring, ester group, amide group and the like in the additive promote the compatibility between the additive and the other raw materials; the carbon-carbon double bonds in the additive can produce a chemical reaction with the unreacted carbon-carbon double bonds at the end of the polyvinyl chloride resin under the action of the initiator, so that the additive is further dispersed in the raw materials, and at the same time, the additive is grafted into the polyvinyl chloride macromolecular chain through chemical action, so that it is stably present in the PET culture medium bottle, not easy to migrate and fall out, and thus fully and stably plays its role, so that the PET culture medium bottle of the present invention has a long-lasting, efficient and safe flame retardant effect and excellent and stable antioxidant properties.
[0025] Furthermore, the plasticizer is a compound of diisononyl cyclohexane 1,2-dicarboxylate and dioctyl sebacate.
[0026] Furthermore, the weight ratio of diisononyl cyclohexane-1,2-dicarboxylate to dioctyl sebacate is 2-3:1.
[0027] The plasticizer obtained by compounding diisononyl cyclohexane 1,2-dicarboxylate and dioctyl sebacate has good compatibility with polyvinyl chloride resin and PET resin, high plasticizing efficiency, low volatility, and excellent low temperature resistance.
[0028] Furthermore, the initiator is one or more of dibenzoyl peroxide, diisopropylbenzene peroxide, and azobisisobutyronitrile.
[0029] A method for preparing a high-performance modified PET culture medium bottle comprises the following steps:
[0030] Weigh each raw material by weight, add PET resin, polyvinyl chloride resin, and amino silicone oil into a high-speed mixer, mix at high speed, add auxiliary agent, initiator, and plasticizer in sequence after the material temperature reaches 100° C. and mix evenly, heat to 150° C., mix evenly to obtain a mixture, fill the mixture into a granulator, and cut it through the granulator to obtain pellets;
[0031] The pellets are transported to the bottle blowing machine through the feeding pipeline; they are melted and injected into the preform mold; after cooling for 32 seconds, the preform is demoulded and transferred to the temperature adjustment station simultaneously; the temperature of the preform is adjusted at 120℃ by the temperature adjustment barrel and 110℃ by the temperature adjustment core rod, so that the temperature of the preform reaches 90-95℃ when it enters the film blowing cavity; the preform enters the bottle cavity mold to prepare for bottle blowing, pre-blowing, strong blowing, pressure holding, and after passing the inspection, a PET culture medium bottle is obtained.
[0032] Furthermore, the pre-blowing pressure is 0.8 MPa, and the pre-blowing time is 0.3-0.35 s.
[0033] Furthermore, the strong blowing pressure is 3.2 MPa, and the strong blowing time is 0.5-0.6 s.
[0034] Furthermore, the holding pressure is 1.5 MPa.
[0035] The beneficial effects of the present invention are as follows: the additives containing nitrogen, phosphorus, silicon elements and hindered phenol structures and hindered amine structures have good compatibility with other raw materials, and there is a chemical reaction between the additives and the polyvinyl chloride resin. Therefore, the additives are highly dispersed and stably present in the PET culture medium bottle, and are not easy to migrate and escape. In addition, due to the synergistic effect with other raw materials, the PET culture medium bottle of the present invention has excellent and stable antioxidant properties, high barrier properties, and long-lasting, efficient and safe flame retardant effects and other properties. DETAILED DESCRIPTION
[0036] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0037] Example 1
[0038] Preparation of auxiliary agent, the specific steps are as follows:
[0039] S1. A dry 250 mL three-necked flask was purged with nitrogen for 30 min to drive away the air in the flask, and then 13.8 mL of 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane, 11.5 mL of triethylamine and 120 mL of methanol were added under nitrogen protection. After stirring and dissolving, 5.6 mL of 4-chloro-1-butene was slowly added, and the temperature was raised to 80 ° C for reaction for 3 h. After the reaction was completed, it was cooled to room temperature and distilled under reduced pressure to obtain intermediate 1;
[0040] S2. Add 10.1 mL of flame retardant FRC-2 and 120 mL of DMSO to a dry 500 mL three-necked flask under nitrogen protection, stir thoroughly, and then slowly add a mixed solution of 19.8 g of intermediate 1 and 80 mL of DMSO. After the addition is complete, heat to 120 ° C and react for 2 h. After the reaction is completed, cool to room temperature and distill under reduced pressure to obtain intermediate 2;
[0041] S3, under nitrogen protection, add 16.9g of intermediate 2, 8.2g of 2-(2,2,6,6-tetramethylpiperidin-4-yl)acetic acid and 220mL of DMSO into a 500mL four-necked flask, stir until completely dissolved, then slowly add 2.5mL of concentrated sulfuric acid, stir and heat to 110°C for 3h, cool to room temperature after the reaction, add sodium bicarbonate solution for neutralization, shake and stand for stratification, take the organic phase, dry it with anhydrous magnesium sulfate, filter, and distill the filtrate under reduced pressure to obtain intermediate 3;
[0042] S4. Under nitrogen protection, add 16.6 g of intermediate 3, 5.5 mL of triethylamine and 160 mL of DMF into a dry 500 mL three-necked flask. After stirring to dissolve, slowly add a mixed solution of 8.2 g of 2,6-di-tert-butyl-4-bromomethylphenol and 40 mL of DMF. Heat to 90 °C and react for 4 h. After the reaction is completed, cool to room temperature and distill under reduced pressure to obtain an auxiliary agent.
[0043] Example 2
[0044] Prepare PET culture medium bottles, the specific steps are as follows:
[0045] Weigh each raw material by weight, add 70 parts of PET resin, 10 parts of polyvinyl chloride resin, and 2 parts of amino silicone oil into a high-speed mixer, mix at high speed, and after the material temperature reaches 100° C., add 2 parts of the auxiliary agent prepared in Example 1, 0.02 parts of azobisisobutyronitrile, and 1.34 parts of cyclohexane 1,2-dicarboxylic acid diisononyl ester in sequence and mix evenly, heat to 150° C., mix evenly to obtain a mixture, fill the mixture into a granulator, and cut it through the granulator to obtain pellets;
[0046] The pellets are transported to the bottle blowing machine through the feeding pipeline; they are melted and injected into the preform mold; after cooling for 32 seconds, the preform is demoulded and synchronously transferred to the temperature adjustment station; the temperature of the preform is adjusted at 120℃ by the temperature adjustment barrel and 110℃ by the temperature adjustment core rod, so that the temperature of the preform enters the film blowing cavity to meet 90-95℃; the preform enters the bottle cavity mold to prepare for bottle blowing, the pre-blowing pressure is 0.8MPa, the pre-blowing time is 0.3s, the transfer pressure is 3.2MPa for strong blowing, the strong blowing time is 0.5s, and the transfer pressure is 1.5MPa for pressure maintenance. After passing the inspection, a PET culture medium bottle is obtained.
[0047] Example 3
[0048] Prepare PET culture medium bottles, the specific steps are as follows:
[0049] Weigh each raw material by weight, add 78 parts of PET resin, 13 parts of polyvinyl chloride resin, and 5 parts of amino silicone oil into a high-speed mixer, mix at high speed, and after the material temperature reaches 100° C., add 3 parts of the additive prepared in Example 1, 0.03 parts of dibenzoyl peroxide, 2 parts of cyclohexane 1,2-dicarboxylic acid diisononyl ester, and 1 part of dioctyl sebacate in sequence and mix evenly, heat to 150° C., mix evenly to obtain a mixture, fill the mixture into a granulator, and cut it with the granulator to obtain pellets;
[0050] The pellets are transported to the bottle blowing machine through the feeding pipeline; they are melted and injected into the preform mold; after cooling for 32 seconds, the preform is demoulded and synchronously transferred to the temperature adjustment station; the temperature of the preform is adjusted at 120℃ by the temperature adjustment barrel and 110℃ by the temperature adjustment core rod, so that the temperature of the preform enters the film blowing cavity to meet 90-95℃; the preform enters the bottle cavity mold to prepare for bottle blowing, the pre-blowing pressure is 0.8MPa, the pre-blowing time is 0.32s, the transfer pressure is 3.2MPa for strong blowing, the strong blowing time is 0.55s, and the transfer pressure is 1.5MPa for pressure maintenance. After passing the inspection, a PET culture medium bottle is obtained.
[0051] Example 4
[0052] Prepare PET culture medium bottles, the specific steps are as follows:
[0053] Weigh each raw material by weight, add 80 parts of PET resin, 15 parts of polyvinyl chloride resin, and 6 parts of amino silicone oil into a high-speed mixer, mix at high speed, and after the material temperature reaches 100° C., add 4 parts of the auxiliary agent prepared in Example 1, 0.04 parts of diisopropylbenzene peroxide, 3.75 parts of cyclohexane 1,2-dicarboxylic acid diisononyl ester, and 1.25 parts of dioctyl sebacate in sequence and mix evenly, heat to 150° C., mix evenly to obtain a mixture, fill the mixture into a granulator, and cut it through the granulator to obtain pellets;
[0054] The pellets are transported to the bottle blowing machine through the feeding pipeline; they are melted and injected into the preform mold; after cooling for 32 seconds, the preform is demoulded and synchronously transferred to the temperature adjustment station; the temperature of the preform is adjusted at 120℃ by the temperature adjustment barrel and 110℃ by the temperature adjustment core rod, so that the temperature of the preform enters the film blowing cavity to meet 90-95℃; the preform enters the bottle cavity mold to prepare for bottle blowing, the pre-blowing pressure is 0.8MPa, the pre-blowing time is 0.35s, the transfer pressure is 3.2MPa for strong blowing, the strong blowing time is 0.6s, the transfer pressure is 1.5MPa for pressure maintenance, and after passing the inspection, a PET culture medium bottle is obtained.
[0055] Comparative Example 1
[0056] Prepare PET culture medium bottles, the specific steps are as follows:
[0057] The remaining steps remain unchanged, and the auxiliary agent in Example 4 is removed to prepare a PET culture medium bottle.
[0058] Comparative Example 2
[0059] Prepare PET culture medium bottles, the specific steps are as follows:
[0060] The remaining steps remained unchanged, and the auxiliary agent in Example 4 was replaced by 1 part of antioxidant 1010, 1 part of light stabilizer 744 and 2 parts of flame retardant DDP to prepare a PET culture medium bottle.
[0061] Comparative Example 3
[0062] Prepare PET culture medium bottles, the specific steps are as follows:
[0063] The remaining steps remain unchanged, and the polyvinyl chloride resin, diisononyl cyclohexane 1,2-dicarboxylate and dioctyl sebacate of Example 4 are removed to prepare a PET culture medium bottle.
[0064] Performance Testing
[0065] The following Table 1 shows the technical indicators of the PET culture medium bottles prepared in Examples 2-4:
[0066] Table 1
[0067]
[0068]
[0069] The PET culture medium bottles prepared in Examples 2-4 and Comparative Examples 1-3 were made into corresponding samples according to different test items and subjected to the following performance tests:
[0070] According to GB / T16928-1997 "Test Method for Water Vapor Permeability of Packaging Materials", a constant temperature and humidity chamber was used to test the water vapor permeability; according to GB / T31354-2014 "Test Method for Oxygen Permeability of Packages and Containers - Coulometer Test Method", an oxygen permeability tester was used to test the oxygen permeability; according to UL-94 standard, the flame retardant performance was tested; according to ASTMD2843-2016 standard, the total smoke release (TSR) was tested. The test results are shown in Table 2 below:
[0071] Table 2
[0072]
[0073] “-” indicates no flame retardant rating.
[0074] It can be seen from the test results in Table 2 that the PET culture medium bottles prepared in Examples 2-4 of the present invention have excellent flame retardancy, high barrier properties and high light transmittance.
[0075] The PET culture medium bottles of Examples 2-4 and Comparative Examples 1-3 were made into corresponding specimens according to GB / T1040-2006 for tensile strength testing, and the change rate of tensile strength before and after aging was tested. The test results are shown in Table 3 below:
[0076] Table 3
[0077]
[0078] From the test results in Table 3, it can be seen that the PET culture medium bottles prepared in Examples 2-4 of the present invention have excellent antioxidant properties. From the data of Examples 2-4 and Comparative Example 2, it can be seen that when the additives of the present invention are replaced with existing antioxidants and light stabilizers, the anti-aging property of the PET culture medium bottles is reduced; from the data of Examples 2-4 and Comparative Example 3, it can be seen that when the polyvinyl chloride resin is removed, there is no chemical reaction between the additives of the present invention and the raw materials, and therefore, its anti-aging property is also reduced.
[0079] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0080] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.
Claims
1. A high-performance modified PET culture medium bottle, characterized in that: The raw materials include the following parts by weight: 70-80 parts of PET resin, 10-15 parts of polyvinyl chloride resin, 2-6 parts of amino silicone oil, 2-4 parts of auxiliary agent, 2-5 parts of plasticizer, and 0.02-0.04 parts of initiator; Wherein, the auxiliary agent is prepared by the following steps: S1, after nitrogen blowing into the flask, add 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane, triethylamine and methanol, stir and add 4-chloro-1-butene, react at 80°C for 3h, cool and distill under reduced pressure to obtain intermediate 1; S2. Add flame retardant FRC-2 and DMSO to a flask under nitrogen protection, add intermediate 1 and DMSO after stirring, heat to 120°C for 2h, cool, and distill under reduced pressure to obtain intermediate 2; S3, under nitrogen protection, add intermediate 2, 2-(2,2,6,6-tetramethylpiperidin-4-yl)acetic acid and DMSO into a flask, stir and add concentrated sulfuric acid, react at 110°C for 3h, cool, add sodium bicarbonate solution, separate, take the organic phase, dry, filter, and distill the filtrate under reduced pressure to obtain intermediate 3; S4. Under nitrogen protection, add intermediate 3, triethylamine and DMF into a flask, then add 2,6-di-tert-butyl-4-bromomethylphenol and DMF, react at 90° C. for 4 h, and distill under reduced pressure to obtain an auxiliary agent.
2. A high performance modified PET culture medium bottle according to claim 1, characterized in that: The usage ratio of 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane, 4-chloro-1-butene, triethylamine and methanol in step S1 is 13.8 mL:5.6 mL:11.5 mL:120 mL.
3. A high performance modified PET culture medium bottle according to claim 1, characterized in that: The usage ratio of the flame retardant FRC-2, the intermediate 1 and DMSO in step S2 is 10.1 mL:19.8 g:200 mL.
4. A high performance modified PET culture medium bottle according to claim 1, characterized in that: The usage ratio of intermediate 2 in step S3, 2-(2,2,6,6-tetramethylpiperidin-4-yl)acetic acid, concentrated sulfuric acid and DMSO is 16.9 g:8.2 g:2.5 mL:220 mL.
5. A high performance modified PET culture medium bottle according to claim 1, characterized in that: The usage ratio of intermediate 3, 2,6-di-tert-butyl-4-bromomethylphenol, triethylamine and DMF in step S4 is 16.6 g:8.2 g:5.5 mL:200 mL.
6. A high performance modified PET culture medium bottle according to claim 1, characterized in that: The plasticizer is a compound of diisononyl cyclohexane 1,2-dicarboxylate and dioctyl sebacate; the weight ratio of diisononyl cyclohexane 1,2-dicarboxylate to dioctyl sebacate is 2-3:
1.
7. A high performance modified PET culture medium bottle according to claim 1, characterized in that: The initiator is one or more of dibenzoyl peroxide, diisopropylbenzene peroxide and azobisisobutyronitrile.
8. The method for preparing a high-performance modified PET culture medium bottle according to claim 1, characterized in that: The following steps are involved: Add PET resin, polyvinyl chloride resin and amino silicone oil into a high-speed mixer according to weight, and mix them. After reaching 100°C, add auxiliary agent, initiator and plasticizer and mix them evenly. Heat to 150°C, mix evenly to obtain a mixture, fill the mixture into a granulator, cut and obtain granules. The pellets are transported to the bottle blowing machine through the feeding pipeline; they are melted and injected into the preform mold; after cooling for 32 seconds, the preform is demoulded and transferred to the temperature adjustment station simultaneously; The temperature of the preform is adjusted at 120℃ by the temperature-adjusting barrel and 110℃ by the temperature-adjusting core rod, so that the temperature of the preform reaches 90-95℃ when it enters the film blowing cavity; the preform enters the bottle cavity mold to prepare for bottle blowing, pre-blowing, strong blowing, and pressure holding. After passing the inspection, the PET culture medium bottle is obtained.
9. The method for preparing a high-performance modified PET culture medium bottle according to claim 8, characterized in that: The pre-blowing pressure is 0.8 MPa, and the pre-blowing time is 0.3-0.35 s.
10. The method for preparing a high-performance modified PET culture medium bottle according to claim 8, characterized in that: The strong blowing pressure is 3.2MPa, the strong blowing time is 0.5-0.6s; and the holding pressure is 1.5MPa.
Citation Information
Patent Citations
PET (Polyethylene Terephthalate) material with high barrier property, preparation method and packaging bottle
CN116063832A
Novel high-barrier-property PET bottle and preparation method thereof
CN107216622A
Novel high-barrier PET bottle and production method thereof
CN109929223A