A degradable plastic product and preparation method thereof
Through the blending preparation of PBAT, corn yellow powder and calcium carbonate, and modification with coupling agent and plasticizer, the aging problem of biodegradable plastic in water vapor and air is solved, and its mechanical strength and thermal stability are improved. Achieved high-performance biodegradable plastic products.
Patent Information
- Application Number
- CN202411122331.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-08-15
AI Technical Summary
Traditional biodegradable plastics have poor mechanical properties and heat resistance after contacting water vapor and air, resulting in rapid aging and reduced strength, and are unable to be effectively used.
PBAT, pretreated cornmeal powder and calcium carbonate are blended and prepared. It can be modified by coupling agent and plasticizer to enhance the compatibility and thermal processing properties of the plastic, improve the tensile strength and thermal stability, and through The combination of pectinase and cellulase enhances biodegradation performance.
Degradable plastic products with high mechanical strength, thermal processing properties and hydrophobicity are obtained, extending their service life and improving biodegradability.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present application relates to the field of plastic material technology, and in particular to a degradable plastic product and a preparation method thereof. Background Art
[0002] Plastics are widely used in various fields of the national economy due to their advantages such as low density, easy processing, high specific strength, and easy multi-function. However, the durability and anti-degradation of traditional plastics make it difficult to degrade when discarded in the environment, causing serious waste of energy resources and environmental pollution. Biodegradable plastics are green and environmentally friendly materials that can be decomposed by microorganisms into environmentally friendly substances such as CO2 and water under the conditions of light, heat, and microorganisms within a certain period of time. From the perspective of sustainable development, biodegradable plastics have favorable characteristics such as renewability, biocompatibility, and non-toxicity. Promoting biodegradable plastic alternatives is one of the important ways to solve the problem of plastic pollution. Researchers from various countries have used various materials, such as starch, protein, plant fiber and other natural polymers to produce various completely biodegradable plastics, but there are still few products that can be used in practice. A key problem restricting their application is the high production cost. Corn yellow powder is a by-product of starch production. Its market price is much lower than starch and other natural materials. Therefore, there is a broad prospect for using corn yellow powder to produce biodegradable plastics.
[0003] However, this type of natural biodegradable material has very poor water vapor resistance, heat resistance, mechanical properties, etc. After being manufactured, it will be oxidized and the polymer connection bonds will break due to direct contact with the surrounding water vapor, air, etc. within a short period of time, resulting in rapid aging of the packaging material, reduced strength, and unusable. Therefore, it is urgent to provide a degradable plastic product and its preparation method to solve the above technical problems. Summary of the invention
[0004] In order to solve the performance problems of degradable plastic products such as poor mechanical properties and poor heat resistance, the present application provides a degradable plastic product and a preparation method thereof.
[0005] The present application provides a degradable plastic product, which adopts the following technical solution:
[0006] A degradable plastic product is made from a degradable plastic material; the degradable plastic material comprises, by weight, 60-100 parts of PBAT, 3-5 parts of pretreated corn yellow powder, 40-60 parts of calcium carbonate, 1-2 parts of a plasticizer, 1-2 parts of a coupling agent, 5-10 parts of anhydrous ethanol, and 0.5-1 part of a heat stabilizer.
[0007] By adopting the above technical scheme, PBAT, corn yellow powder and calcium carbonate are blended to prepare degradable plastic products, and degradable plastics with high mechanical strength and thermal processing properties can be obtained. The addition of calcium carbonate can effectively improve the mechanical properties and thermal processing properties of PBAT and corn yellow powder. At the same time, during the preparation process, the surface of calcium carbonate and corn yellow powder is modified by a coupling agent, which can effectively enhance the compatibility between the PBAT matrix, corn yellow powder and calcium carbonate filler, and effectively enhance the tensile strength and thermal stability of the plastic; the corn yellow powder is modified by a plasticizer, which effectively improves the thermal processing properties of the corn yellow powder, making it thermoplastic.
[0008] Preferably, the pretreated corn yellow powder is prepared from the following raw materials in parts by weight: 10-20 parts of corn yellow powder, 0.15-0.3 parts of complex enzyme, and 5-10 parts of water.
[0009] Preferably, the complex enzyme includes pectinase and cellulase, and the mass ratio of the two is 1:0.1-0.15.
[0010] By adopting the above technical scheme, the combined use of pectinase and cellulase can exert a synergistic effect. Pectinase mainly degrades pectin components to loosen the cell walls; while cellulase further degrades cellulose components to improve the biodegradability of plastics. This treatment can not only improve the utilization rate and processing efficiency of corn yellow powder raw materials, but also improve the performance and quality of the final plastic products.
[0011] Preferably, the plasticizer is a mixture of glycerol and sorbitol, and the mass ratio of the two is 1:4.5-5.5.
[0012] By adopting the above technical solution, the compound of glycerol and sorbitol plays a synergistic plasticizing role, and the tensile properties, thermal processing properties and hydrophobicity of the composite material are improved.
[0013] Preferably, the coupling agent is a titanate coupling agent.
[0014] Preferably, the thermal stabilizer is dimethyl phosphate.
[0015] The present application also provides a method for preparing a degradable plastic product, which adopts the following technical solution:
[0016] A method for preparing a degradable plastic product comprises the following steps:
[0017] Pre-treating the corn yellow powder to obtain pre-treated corn yellow powder; weighing each raw material component by weight, and drying PBAT and calcium carbonate for 8-12 hours to remove moisture;
[0018] Spray the plasticizer into the pretreated corn yellow powder, blend at 1300-1500 rpm, mix for 20-30 minutes, take out and seal the material for 18-30 hours to obtain plasticized corn yellow powder;
[0019] After the coupling agent is evenly mixed with anhydrous ethanol, the coupling agent is evenly sprayed into the calcium carbonate and the plasticized corn yellow powder; the calcium carbonate powder and the plasticized corn yellow powder are mixed at 1300-1500 rpm at room temperature, mixed at 100-120° C. for 15-25 minutes, and cooled to obtain the surface-modified calcium carbonate and corn yellow powder;
[0020] Mixing PBAT, a heat stabilizer, surface-modified calcium carbonate and corn yellow powder at high speed for 5-10 minutes at room temperature to obtain a mixed material;
[0021] The mixed material is added into a twin-screw extruder unit for mixing, extrusion and granulation, and the degradable plastic product is obtained after molding.
[0022] Preferably, the method for preparing the pretreated corn yellow powder comprises the following steps:
[0023] The corn yellow powder is filtered through a sieve and impurities are removed, and then placed in a dryer for drying at 60-80°C. Subsequently, 10-20 parts of corn yellow powder are weighed, mixed with 0.15-0.3 parts of complex enzyme and 5-10 parts of water, and then maintained at a constant temperature of 35-45°C for 10-13 minutes to obtain pretreated corn yellow powder.
[0024] In summary, the present application includes at least one of the following beneficial technical effects:
[0025] 1. This application uses PBAT, corn yellow powder, and calcium carbonate to blend and prepare degradable plastic products, which can obtain degradable plastics with high mechanical strength and thermal processing properties. The addition of calcium carbonate can effectively improve the mechanical properties and thermal processing properties of PBAT and corn yellow powder.
[0026] 2. In the preparation process of this application, a coupling agent is used to modify the surface of calcium carbonate and corn yellow powder, which can effectively enhance the compatibility between the PBAT matrix, corn yellow powder and calcium carbonate filler, and effectively enhance the tensile strength and thermal stability of the plastic;
[0027] 3. This application uses plasticizer to modify corn yellow powder, which effectively improves the thermal processability of corn yellow powder and makes it thermoplastic. DETAILED DESCRIPTION
[0028] The present application is further described in detail below with reference to the embodiments.
[0029] Example
[0030] Example 1, S1. After filtering and removing impurities from the corn yellow powder through a sieve, the corn yellow powder was placed in a dryer and dried at 60°C. Subsequently, 10g of the corn yellow powder was weighed, mixed with 0.15g of the complex enzyme and 5g of water, and kept at a constant temperature of 35°C for 13min to obtain pretreated corn yellow powder; 60g of PBAT and 40g of calcium carbonate were dried for 8h to remove moisture; the complex enzyme in this embodiment includes 30,000u / ml of pectinase and 2000u / g of cellulase, and the mass ratio of the two is 1:0.1;
[0031] S2. Spray 1 g of plasticizer onto 3 g of pretreated corn powder, add to a high-speed mixer and blend at 1300 rpm, mix for 20 min, take out and seal the material for 18 h to obtain plasticized corn powder; the plasticizer in this embodiment is a mixture of glycerol and sorbitol, the mass ratio of the two is 1:4.5;
[0032] S3. After 1g of coupling agent titanate coupling agent 201 was mixed with 5g of anhydrous ethanol, it was evenly sprayed onto calcium carbonate and plasticized corn yellow powder; calcium carbonate powder and plasticized corn yellow powder were added to a high-speed stirrer at room temperature, mixed at 100 ° C and 1300 rpm for 15 min, and surface-modified calcium carbonate and corn yellow powder were obtained after cooling;
[0033] S4. PBAT, 0.5 g of a heat stabilizer of dimethyl phosphate, surface-modified calcium carbonate and corn yellow powder were added to a high-speed mixer and mixed at room temperature at a speed of 1500 rpm for 5 min to obtain a mixed material;
[0034] S5. Add the mixed material into a TSJ50 / 100 twin-screw extruder unit for mixing, extrusion and granulation, and obtain a biodegradable plastic product after molding.
[0035] Example 2, S1. After filtering and removing impurities from the corn yellow powder through a sieve, the corn yellow powder was placed in a dryer and dried at 70°C. Subsequently, 15g of corn yellow powder was weighed, mixed with 0.225g of complex enzyme and 7.5g of water, and kept at a constant temperature of 40°C for 11.5min to obtain pretreated corn yellow powder; 80g of PBAT and 50g of calcium carbonate were dried for 10h to remove moisture; the complex enzyme in this embodiment includes 30,000u / ml of pectinase and 2000u / g of cellulase, and the mass ratio of the two is 1:0.1;
[0036] S2. Spray 1 g of plasticizer onto 4 g of pretreated corn powder, add to a high-speed mixer and blend at 1400 rpm, mix for 25 min, take out and seal the material for 24 h to obtain plasticized corn powder; the plasticizer in this embodiment is a mixture of glycerol and sorbitol, the mass ratio of the two is 1:4.5;
[0037] S3. After 1g of coupling agent titanate coupling agent 201 was mixed with 8g of anhydrous ethanol, it was evenly sprayed onto calcium carbonate and plasticized corn yellow powder; calcium carbonate powder and plasticized corn yellow powder were added to a high-speed stirrer at room temperature, mixed at 110 ° C and 1400 rpm for 20 min, and surface-modified calcium carbonate and corn yellow powder were obtained after cooling;
[0038] S4. PBAT, 0.75 g of a heat stabilizer of dimethyl phosphate, surface-modified calcium carbonate and corn yellow powder were added to a high-speed mixer and mixed at room temperature and a speed of 1550 rpm for 7.5 min to obtain a mixed material;
[0039] S5. Add the mixed material into a TSJ50 / 100 twin-screw extruder unit for mixing, extrusion and granulation, and obtain a biodegradable plastic product after molding.
[0040] Example 3, S1. After filtering and removing impurities from the corn yellow powder through a sieve, the corn yellow powder was placed in a dryer and dried at 80°C. Subsequently, 20g of corn yellow powder was weighed and mixed with 0.3g of complex enzyme and 10g of water, and the mixture was kept at a constant temperature of 45°C for 10min to obtain pretreated corn yellow powder; 100g of PBAT and 60g of calcium carbonate were dried for 8h to remove moisture; the complex enzyme in this embodiment includes 30,000u / ml of pectinase and 2000u / g of cellulase, and the mass ratio of the two is 1:0.1;
[0041] S2. Spray 1 g of plasticizer onto 5 g of pretreated corn powder, add to a high-speed mixer and blend at 1500 rpm, mix for 30 min, take out and seal the material for 30 h to obtain plasticized corn powder; the plasticizer in this embodiment is a mixture of glycerol and sorbitol, the mass ratio of the two is 1:4.5;
[0042] S3. After 1 g of coupling agent titanate coupling agent 201 was mixed with 10 g of anhydrous ethanol, it was evenly sprayed onto calcium carbonate and plasticized corn yellow powder; calcium carbonate powder and plasticized corn yellow powder were added to a high-speed stirrer at room temperature, mixed at 120 ° C and 1500 rpm for 25 min, and surface-modified calcium carbonate and corn yellow powder were obtained after cooling;
[0043] S4. PBAT, 1 g of a heat stabilizer of dimethyl phosphate, surface-modified calcium carbonate and corn yellow powder were added to a high-speed mixer and mixed at room temperature at a speed of 1600 rpm for 10 min to obtain a mixed material;
[0044] S5. Add the mixed material into a TSJ50 / 100 twin-screw extruder unit for mixing, extrusion and granulation, and obtain a biodegradable plastic product after molding.
[0045] Example 4: The difference between Example 4 and Example 1 is that the mass of the plasticizer used in S2 of Example 4 is 1.5 g, and the plasticizer is a mixture of glycerol and sorbitol, and the mass ratio of the two is 1:4.5.
[0046] Example 5: The difference between Example 5 and Example 1 is that the mass of the plasticizer used in S2 of Example 5 is 2 g, and the plasticizer is a mixture of glycerol and sorbitol, and the mass ratio of the two is 1:4.5.
[0047] Example 6: The difference between Example 6 and Example 1 is that the mass of the plasticizer used in S2 of Example 6 is 1 g, and the plasticizer is a mixture of glycerol and sorbitol, and the mass ratio of the two is 1:5.
[0048] Example 7: The difference between Example 7 and Example 1 is that the mass of the plasticizer used in S2 of Example 7 is 1 g, and the plasticizer is a mixture of glycerol and sorbitol, and the mass ratio of the two is 1:5.5.
[0049] Example 8: The difference between Example 8 and Example 1 is that the mass of the plasticizer used in S2 of Example 8 is 1 g, and the plasticizer is a mixture of glycerol and sorbitol, and the mass ratio of the two is 1:3.5.
[0050] Example 9: The difference between Example 9 and Example 1 is that the mass of the plasticizer used in S2 of Example 9 is 1 g, and the plasticizer is a mixture of glycerol and sorbitol, and the mass ratio of the two is 1:6.5.
[0051] Example 10: The difference between Example 10 and Example 1 is that the coupling agent used in S3 of Example 10 is titanate coupling agent TTS, with a mass of 1 g.
[0052] Example 11: The difference between Example 11 and Example 1 is that the coupling agent used in S3 of Example 11 is titanate coupling agent 201 with a mass of 1.5 g.
[0053] Example 12: The difference between Example 12 and Example 1 is that the coupling agent used in S3 of Example 12 is titanate coupling agent 201 with a mass of 2 g.
[0054] Example 13: The difference between Example 13 and Example 1 is that the complex enzyme used in S1 of Example 13 includes 30,000 u / ml pectinase and 2,000 u / g cellulase, and the mass ratio of the two is 1:0.12.
[0055] Example 14: The difference between Example 14 and Example 1 is that the complex enzyme used in S1 of Example 14 includes 30,000 u / ml pectinase and 2,000 u / g cellulase, and the mass ratio of the two is 1:0.15.
[0056] Example 15. The difference between Example 15 and Example 1 is that the complex enzyme used in S1 of Example 15 includes 30,000 u / ml pectinase and 2000 u / g cellulase, and the mass ratio of the two is 1:0.05.
[0057] Example 16: The difference between Example 16 and Example 1 is that the complex enzyme used in S1 of Example 16 includes 30,000 u / ml pectinase and 2,000 u / g cellulase, and the mass ratio of the two is 1:0.2.
[0058] Comparative Example
[0059] Comparative Example 1: The difference between Comparative Example 1 and Example 1 is that the mass of the plasticizer used in S2 in Comparative Example 1 is 0 g.
[0060] Comparative Example 2: The difference between Comparative Example 2 and Example 1 is that the mass of the plasticizer used in S2 of Comparative Example 2 is 3 g, and the plasticizer is a mixture of glycerol and sorbitol, and the mass ratio of the two is 1:4.5.
[0061] Comparative Example 3: The difference between Comparative Example 3 and Example 1 is that the mass of the coupling agent used in S3 of Comparative Example 3 is 0 g.
[0062] Comparative Example 4: The difference between Comparative Example 4 and Example 1 is that the coupling agent used in S3 of Comparative Example 4 is titanate coupling agent 201 with a mass of 3 g.
[0063] Performance testing
[0064] The granulated raw materials of Examples 1-16 and Comparative Examples 1-4 were used to prepare plastic film products using a film blowing machine, and the film thickness was 15 μm; the tensile strength and elongation at break of the film were measured using GB / T 1040-2006 "Determination of tensile properties of plastics";
[0065] The Vicat softening point of the film was measured using GB / T 1633-2000 "Determination of Vicat softening temperature (VST) of thermoplastics";
[0066] GB / T 1037-2021 "Plastic film and sheeting - Determination of water vapor transmission properties - Cup weight gain and weight loss method" was used to measure the water vapor transmission rate of the film.
[0067] The results are shown in Table 1.
[0068] The specific test results are as follows:
[0069] Table 1 Performance test results
[0070]
[0071] It can be seen from the test results of Table 1 that the degradable plastic products provided by the present application have high tensile strength and elongation at break, indicating that the degradable plastic products provided by the present application have good mechanical strength; the Vicat softening point is high, indicating that the degradable plastic products provided by the present application have good heat resistance and stability; the water vapor permeability is small, indicating that the degradable plastic products provided by the present application have good hydrophobic properties.
[0072] It can be seen from the test results of Examples 1-3 that the preparation method of the degradable plastic product provided in the present application can obtain a degradable plastic product with high mechanical strength, heat stability and hydrophobicity.
[0073] It can be seen from the test results of Examples 1, 4, 5 and Comparative Examples 1 and 2 that the addition of plasticizers to treat corn yellow powder in the present application can effectively enhance the tensile strength, elongation at break, and Vicat softening point of the degradable plastic products, and reduce the water vapor permeability, indicating that the improved plasticizer in the present application can effectively enhance the mechanical strength, thermal stability and hydrophobicity of the plastic quality; it can be seen from the test results of Examples 1, 6, 7, 8, and 9 that when the mass ratio of the mixture of plasticizers glycerol and sorbitol provided by the present application is 1:4.5-5.5, the mechanical properties, thermal stability and hydrophobicity of the obtained degradable plastic products are optimal. Below or exceeding this range, the mechanical properties, thermal stability and hydrophobicity of the degradable plastic products are all reduced.
[0074] It can be seen from the test results of Examples 1, 10, 11, 12 and Comparative Examples 3 and 4 that the addition of coupling agents to treat corn yellow powder and calcium carbonate in the present application can effectively enhance the tensile strength, elongation at break, and Vicat softening point of the degradable plastic products, and reduce the water vapor permeability, indicating that the improved coupling agent in the present application can effectively enhance the mechanical strength, thermal stability and hydrophobicity of the plastic quality.
[0075] It can be seen from the test results of Examples 1, 13, 14, 15, and 16 that the present application can effectively enhance the tensile strength, elongation at break, and Vicat softening point of the degradable plastic products by treating corn yellow powder with a composite enzyme of pectinase and cellulase, and reduce the water vapor permeability. When the mass ratio of the two is 1:0.1-0.15, the mechanical properties, thermal stability, and hydrophobicity of the obtained degradable plastic products are optimal.
[0076] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed. However, as long as it is within the scope of the claims of the present application, it shall be protected by the patent law.
Claims
1. A degradable plastic product, characterized in that: Made from degradable plastic material; by weight, the degradable plastic material includes 60-100 parts of PBAT, 3-5 parts of pretreated corn yellow powder, 40-60 parts of calcium carbonate, 1-2 parts of plasticizer, 1-2 parts of coupling agent, 5-10 parts of anhydrous ethanol, and 0.5-1 parts of heat stabilizer; The pretreated corn yellow powder is prepared from the following raw materials in parts by weight: 10-20 parts of corn yellow powder, 0.15-0.3 parts of complex enzyme, and 5-10 parts of water; The complex enzyme includes pectinase and cellulase, and the mass ratio of the two is 1:0.1-0.15; The method for preparing the degradable plastic product comprises the following steps: Pre-treating the corn yellow powder to obtain pre-treated corn yellow powder; weighing each raw material component by weight, and drying PBAT and calcium carbonate for 8-12 hours to remove moisture; Spray the plasticizer into the pretreated corn yellow powder, blend at 1300-1500 rpm, mix for 20-30 minutes, take out and seal the material for 18-30 hours to obtain plasticized corn yellow powder; After the coupling agent is evenly mixed with anhydrous ethanol, the coupling agent is evenly sprayed into the calcium carbonate and the plasticized corn yellow powder; the calcium carbonate powder and the plasticized corn yellow powder are mixed at 1300-1500 rpm at room temperature, mixed at 100-120° C. for 15-25 minutes, and cooled to obtain the surface-modified calcium carbonate and corn yellow powder; Add PBAT, heat stabilizer, surface-modified calcium carbonate and corn yellow powder into a high-speed mixer, and mix at high speed for 5-10 minutes at room temperature to obtain a mixed material; The mixed material is added into a twin-screw extruder unit for mixing, extrusion and granulation, and the degradable plastic product is obtained after molding.
2. A degradable plastic product according to claim 1, characterized in that: The plasticizer is a mixture of glycerol and sorbitol, and the mass ratio of the two is 1:4.5-5.
5.
3. The degradable plastic product according to claim 1, characterized in that: The coupling agent is a titanate coupling agent.
4. The degradable plastic product according to claim 1, characterized in that: The thermal stabilizer is dimethyl phosphate.
5. The degradable plastic product according to claim 1, characterized in that: The method for preparing the pretreated corn yellow powder comprises the following steps: The corn yellow powder is filtered through a sieve and impurities are removed, and then placed in a dryer for drying at 60-80°C. Subsequently, 10-20 parts of corn yellow powder are weighed, mixed with 0.15-0.3 parts of complex enzyme and 5-10 parts of water, and then maintained at a constant temperature of 35-45°C for 10-13 minutes to obtain pretreated corn yellow powder.
Citation Information
Patent Citations
High-strength, environment-friendly and biodegradable plastic
CN105949524A
Calcium carbonate high-filled biodegradable plastic film material used as shopping bag and preparation method of material
CN106893273A