One-component water-soluble acrylic pressure-sensitive adhesive and preparation method thereof
By developing a single component water-soluble acrylate pressure-sensitive adhesive containing specific proportions and types, the problem of inability to water-soluble after film formation of traditional adhesives is solved, the goal of repulping and environmental protection is achieved, and the production efficiency and mechanics are improved. performance.
Patent Information
- Application Number
- CN202411118878.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-08-15
AI Technical Summary
Traditional acrylate pressure-sensitive adhesives cannot dissolve water after forming film, resulting in no re-pulping, affecting environmental protection and production efficiency.
Develop a single component water-soluble acrylate pressure-sensitive adhesive containing 35%-39% soft monomer, 2.5%-5% hard monomer, 3.5%-25% functional monomer, 0.01-0.5% Initiator, 50%-60% solvent, 0-1.5% curing agent, 0-1.5% curing agent inhibitor and 3%-10% neutralizing agent, ensure good mechanical properties through specific preparation methods. and water soluble.
It realizes water-soluble repulping of traditional adhesives while ensuring mechanical properties, simplifies the process, saves costs, and improves production efficiency.
Smart Images

Figure CN118638495B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of pressure-sensitive adhesives, in particular to a single-component water-soluble acrylate pressure-sensitive adhesive and a preparation method thereof. Background Art
[0002] Acrylic pressure-sensitive adhesives are generally based on soft acrylic monomers such as butyl acrylate and isooctyl acrylate, supplemented by hard monomers such as methyl acrylate, methyl methacrylate, vinyl acetate, and some functional monomers such as acrylic acid, hydroxyethyl acrylate, hydroxypropyl acrylate, etc., and copolymers are obtained by copolymerization. Acrylic pressure-sensitive adhesives have the advantages of excellent bonding properties, aging resistance, low cost, stable performance, and simple synthesis process. Therefore, they are widely used in many fields such as self-adhesive tapes, labels, medicine, automotive parts, electronic appliances, and home care.
[0003] In recent years, acrylic pressure-sensitive adhesives have been more widely used and developed. With the progress of the times, people are paying more and more attention to the environmental protection of various products. Saving, environmental protection and recyclability have become the hallmarks of today's social development. Considering this aspect, the water-based acrylic pressure-sensitive adhesive has become the general trend of the industry. A large number of pressure-sensitive adhesive products are used in the papermaking, printing and packaging industries. Therefore, there are also a large number of adhesives in the waste paper we recycle daily. These adhesives will adhere to the fibers and are difficult to remove, which will affect the normal operation of the production equipment and reduce production efficiency. Therefore, waste paper containing traditional adhesives is generally considered to be non-repulpable. In order to solve this problem, redeveloping repulpable adhesives has become a very important direction. Summary of the invention
[0004] The purpose of this section is to summarize some aspects of the embodiments of the present invention and briefly introduce some preferred embodiments. Some simplifications or omissions may be made in this section and the specification abstract and the invention title of this application to avoid blurring the purpose of this section, the specification abstract and the invention title, and such simplifications or omissions cannot be used to limit the scope of the present invention.
[0005] Therefore, the purpose of the present invention is to provide a one-component water-soluble acrylic pressure-sensitive adhesive and a preparation method thereof, which can well solve the problem that the traditional adhesive cannot be water-soluble after film formation and cannot be pulped again, while ensuring good mechanical properties.
[0006] To solve the above technical problems, according to one aspect of the present invention, the present invention provides the following technical solutions:
[0007] A one-component water-soluble acrylic pressure-sensitive adhesive, comprising, by weight proportion:
[0008] 35%-39% soft monomer, 2.5%-5% hard monomer, 3.5%-25% functional monomer, 0.01-0.5% initiator, 50%-60% solvent, 0-1.5% curing agent, 0-1.5% curing agent inhibitor, 3%-10% neutralizer;
[0009] The soft monomer is composed of butyl acrylate, isooctyl acrylate and methoxy polyethylene glycol acrylate with a molecular weight of 400.
[0010] As a preferred embodiment of the one-component water-soluble acrylic pressure-sensitive adhesive described in the present invention, the hard monomer is one or more of methyl acrylate, methyl methacrylate, vinyl acetate and styrene.
[0011] As a preferred embodiment of the one-component water-soluble acrylic pressure-sensitive adhesive described in the present invention, the functional monomer is one or more of acrylic acid, methacrylic acid, hydroxyethyl acrylate, hydroxypropyl acrylate, N-hydroxymethyl acrylamide and glycidyl methacrylate.
[0012] As a preferred embodiment of the one-component water-soluble acrylic pressure-sensitive adhesive of the present invention, the initiator is one or both of azobisisobutyronitrile and dibenzoyl peroxide.
[0013] As a preferred embodiment of the one-component water-soluble acrylic pressure-sensitive adhesive of the present invention, the solvent is one or more of ethanol, ethyl acetate, isopropanol, acetone, methanol and toluene.
[0014] As a preferred embodiment of the one-component water-soluble acrylic pressure-sensitive adhesive of the present invention, the curing agent is aluminum acetylacetonate, and the curing agent inhibitor is acetylacetone.
[0015] As a preferred embodiment of the one-component water-soluble acrylic pressure-sensitive adhesive of the present invention, the neutralizing agent is one or more of AMP-95, triethanolamine, and sodium hydroxide aqueous solution.
[0016] A method for preparing a one-component water-soluble acrylic pressure-sensitive adhesive, the specific steps are as follows:
[0017] S1. Weigh the required solvents in proportion, mix them evenly and put them into the reaction bottle, start stirring and heat them in a water bath to 74-85°C to produce a stable reflux;
[0018] S2, weigh the required monomers and initiators in proportion, mix them evenly, and after the initiator is completely dissolved and the reflux in the reaction bottle is stable, start dripping the mixture into the reaction bottle through a constant pressure separatory funnel, and it takes 2 hours to drip;
[0019] S3, after the mixed monomers are dripped, the first stage of heat preservation is started at the reflux temperature, the first stage of heat preservation time is 2 hours, after the heat preservation is completed, the first group of initiators dissolved in the solvent are added, and then the second stage of heat preservation is carried out at the reflux temperature, the second stage of heat preservation time is 1 hour, after the heat preservation is completed, the second group of initiators dissolved in the solvent are added, and then the third stage of heat preservation is carried out at the reflux temperature, the third stage of heat preservation time is 2h;
[0020] S4. After the third heat preservation stage is completed, the temperature is lowered to 40°C, and a diluent solvent, a curing agent and a neutralizing agent are added and stirred to obtain the desired single-component water-soluble acrylic pressure-sensitive adhesive.
[0021] Compared with the prior art, the present invention has the beneficial effects that the water-soluble pressure-sensitive adhesive prepared by the present invention has good mechanical properties, does not need to add an external curing agent, is simple and economical, and can be water-soluble and re-pulped. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the present invention will be described in detail below in combination with the accompanying drawings and detailed embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative labor. Among them:
[0023] Figure 1 The present invention is a flow chart of a method for producing a one-component water-soluble acrylic pressure-sensitive adhesive. DETAILED DESCRIPTION
[0024] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below with reference to the accompanying drawings.
[0025] In order to make the objectives, technical solutions and advantages of the present invention more clear, the embodiments of the present invention will be further described in detail below with reference to the accompanying drawings.
[0026] The invention provides a single-component water-soluble acrylic pressure-sensitive adhesive and a preparation method thereof, which can well solve the problem that the conventional adhesive cannot be water-soluble after film formation, resulting in the inability to be re-pulped, while ensuring good mechanical properties.
[0027] In order to illustrate the above scheme, the following Examples 1-4 and Comparative Examples 1-2 are provided for verification. Example 1
[0028] Accurately weigh 33g of acetone, 100g of isopropanol, and 40g of ethanol, mix them evenly, and add them to the reaction bottle. Start to heat up to about 75°C, let the solvent begin to reflux stably, accurately weigh 145g of butyl acrylate, 20g of acrylic acid, 15g of vinyl acetate, 20g of hydroxyethyl acrylate, and 0.125g of azobisisobutyronitrile, mix them evenly, add them to a constant pressure separatory funnel, and drip them in 2 hours. After the dripping is completed, start the first insulation at reflux temperature for 2 hours. After the first insulation is completed, add 0.25g of benzoyl peroxide dissolved in 2.5g of acetone, start the second insulation, and the second insulation time is 1 hour. After the second insulation is completed, add 0.25g of benzoyl peroxide dissolved in 2.5g of acetone, and start the third insulation for 2 hours. After the third insulation time was over and the temperature began to drop to 40°C, 20 g of isopropanol was added for dilution, and then 12.4 g of AMP-95 was added for neutralization to obtain a hydrosol sample.
[0029] The prepared hydrosol sample was coated on the corona surface of a 25 μm transparent PET film, the thickness of the coated dry glue was about 25 μm, and then baked at 120° C. for 2 minutes and attached to a release PET to obtain a hydrosol tape. Example 2
[0030] Accurately weigh 117 g of ethyl acetate and 16 g of isopropanol, mix them evenly and add them into the reaction bottle. Start to raise the temperature to about 78°C and allow the solvent to begin to reflux stably. Accurately weigh 57g of butyl acrylate, 58g of isooctyl acrylate, 20g of acrylic acid, 15g of methyl acrylate, 10g of hydroxyethyl acrylate, 40g of ethoxyethoxyethyl acrylate, and 0.1g of dibenzoyl peroxide, mix well and add to a constant pressure separatory funnel, and drip it in 2 hours. After the dripping is completed, start the first section of insulation at reflux temperature for 2 hours. After the first section of insulation is completed, 0.2g of dibenzoyl peroxide dissolved in 2.5g of ethyl acetate is added, and the second section of insulation is started. The insulation time for the second section is 1 hour. After the insulation of the second section is completed, 0.2g of dibenzoyl peroxide dissolved in 2.5g of ethyl acetate is added, and the third section of insulation is started again. The insulation time is 2 hours. After the third section of insulation time is completed, start to cool to 40°C, add 55g of isopropanol to dilute, and neutralize with 16.6g of triethanolamine to obtain a hydrosol sample.
[0031] The prepared hydrosol sample was coated on the corona surface of a 25 μm transparent PET film, the thickness of the coated dry glue was about 25 μm, and then baked at 120° C. for 2 minutes and attached to a release PET to obtain a hydrosol tape. Example 3
[0032] Accurately weigh 117g of ethyl acetate and 16g of isopropanol, mix them evenly and add them to the reaction bottle, start to heat up to about 78°C, let the solvent begin to reflux stably, accurately weigh 57.5g of butyl acrylate, 57.5g of isooctyl acrylate, 20g of acrylic acid, 15g of methyl acrylate, 10g of hydroxyethyl acrylate, 40g of methoxy polyethylene glycol acrylate (400), and 0.05g of azobisisobutyronitrile, mix them evenly and add them to the constant pressure separatory funnel, and drip them in 2 hours. After the dripping is completed, The first insulation was started at the reflux temperature for 2 hours. After the first insulation was completed, 0.1 g of azobisisobutyronitrile dissolved in 2.5 g of ethyl acetate was added. The second insulation was started for 1 hour. After the second insulation was completed, 0.1 g of azobisisobutyronitrile dissolved in 2.5 g of ethyl acetate was added. The third insulation was started for 2 hours. After the third insulation was completed, the temperature was lowered to 40°C, 55 g of isopropanol was added for dilution, 1.85 g of 30% sodium hydroxide aqueous solution and 10.4 g of triethanolamine were added for neutralization, 1 g of acetylacetone and 1 g of aluminum acetylacetonate were added to obtain a hydrosol sample.
[0033] The prepared hydrosol sample was coated on the corona surface of a 25 μm transparent PET film, the thickness of the coated dry glue was about 25 μm, and then baked at 120° C. for 2 minutes and attached to a release PET to obtain a hydrosol tape. Example 4
[0034] Accurately weigh 101g ethyl acetate, 19.3g isopropanol, and 43.3g toluene, mix well, and add them to the reaction bottle. Start to heat up to about 81°C, let the solvent begin to reflux stably, accurately weigh 68g butyl acrylate, 67g isooctyl acrylate, 20g acrylic acid, 15g methyl acrylate, 10g hydroxyethyl acrylate, 20g ethoxyethoxyethyl acrylate (600), and 0.05g azobisisobutyronitrile, mix well, add to the constant pressure separatory funnel, drip it in 2 hours, and add the resultant solution. After the reaction was completed, the first insulation was started at the reflux temperature for 2 hours. After the first insulation was completed, 0.1 g of azobisisobutyronitrile dissolved in 2.5 g of ethyl acetate was added, and the second insulation was started for 1 hour. After the second insulation was completed, 0.1 g of azobisisobutyronitrile dissolved in 2.5 g of ethyl acetate was added, and the third insulation was started for 2 hours. After the third insulation was completed, the temperature was lowered to 40°C, 25 g of isopropanol was added for dilution, 3.7 g of 30% sodium hydroxide aqueous solution was added for neutralization, 0.2 g of acetylacetone and 0.2 g of aluminum acetylacetonate were added to obtain a hydrosol sample.
[0035] The prepared hydrosol sample was coated on the corona surface of a 25 μm transparent PET film, the thickness of the coated dry glue was about 25 μm, and then baked at 120° C. for 2 minutes and attached to a release PET to obtain a hydrosol tape.
[0036] Comparative Example 1
[0037] Accurately weigh 33g acetone, 100g isopropanol, and 40g ethanol, mix them evenly, add them to the reaction bottle, start to heat up to about 75℃, let the solvent begin to reflux stably, accurately weigh 153g butyl acrylate, 12g acrylic acid, 15g vinyl acetate, 20g hydroxyethyl acrylate, and 0.125g azobisisobutyronitrile, mix them evenly, add them to the constant pressure separatory funnel, and drip them in 2 hours. After the dripping is completed, start the first stage of insulation at reflux temperature , the insulation time is 2 hours, after the first insulation is completed, 0.25g of dibenzoyl peroxide dissolved in 2.5g of acetone is added, and the second insulation is started, the second insulation time is 1 hour, after the second insulation is completed, 0.25g of dibenzoyl peroxide dissolved in 2.5g of acetone is added, and the third insulation is started, the insulation time is 2 hours, after the third insulation time is completed, the temperature begins to drop to 40°C, 20g of isopropanol is added for dilution, and then 12.4g of AMP-95 is added for neutralization to obtain a hydrosol sample.
[0038] The prepared hydrosol sample was coated on the corona surface of a 25 μm transparent PET film, the thickness of the coated dry glue was about 25 μm, and then baked at 120° C. for 2 minutes and attached to a release PET to obtain a hydrosol tape.
[0039] Comparative Example 2:
[0040] Accurately weigh 33 g of acetone, 100 g of isopropanol, and 40 g of ethanol, mix them evenly, and add them into the reaction bottle. Start to raise the temperature to about 75°C and allow the solvent to begin to reflux stably. Accurately weigh 153g of butyl acrylate, 12g of acrylic acid, 15g of vinyl acetate, 20g of hydroxyethyl acrylate, and 0.125g of azobisisobutyronitrile, mix well and add to a constant pressure separatory funnel, and drip it in 2 hours. After the dripping is completed, start the first insulation at reflux temperature for 2 hours. After the first insulation is completed, add 0.25g of dibenzoyl peroxide dissolved in 2.5g of acetone, start the second insulation, and the second insulation time is 1 hour. After the second insulation is completed, add 0.25g of dibenzoyl peroxide dissolved in 2.5g of acetone, and then start the third insulation for 2 hours. After the third insulation time is completed, start to cool to 40°C, add 20g of isopropanol to dilute, then add 12.4g of AMP-95 for neutralization, add 1g of acetylacetone and 1g of aluminum acetylacetonate to obtain a hydrosol sample.
[0041] The prepared hydrosol sample was coated on the corona surface of a 25 μm transparent PET film, the thickness of the coated dry glue was about 25 μm, and then baked at 120° C. for 2 minutes and attached to a release PET to obtain a hydrosol tape.
[0042] The four tape samples prepared by the above four embodiments and two comparative examples were tested. The peeling force test was carried out in accordance with the "180° peeling strength test method for pressure-sensitive adhesive tape" GB / T 2792-1998, and the rolling ball initial adhesion test was carried out in accordance with the "Pressure-sensitive adhesive tape initial adhesion test method-inclined rolling ball method" GB / T 4852-2002. The water solubility test method is: cut the tape with a width of 2.5 cm and a length of 15 cm, tear off the release film, completely immerse in water, and observe the dissolution of the adhesive surface after 24 hours. The test results are shown in Table 1 and Table 2:
[0043] Table 1 is the instant performance test data of the single-component water-soluble pressure-sensitive adhesive prepared in Examples 1-4 and Comparative Examples 1-2
[0044] sample 180° peeling force (N / 25mm) Rolling ball initial adhesion Sticky at room temperature Water Solubility Example 1 14.4 <3# 2h drop 10% dissolved Example 2 14.8 13# 15h drop Completely dissolved Example 3 11.5 16# 70h drop Completely dissolved Example 4 15.2 <3# 20h drop Completely dissolved Comparative Example 1 10.1 3# 5h drop Insoluble Comparative Example 2 8.2 3# 80h drop Insoluble
[0045] Table 2 is the performance test data of the one-component water-soluble pressure-sensitive adhesive prepared in Examples 1-4 and Comparative Examples 1-2 after aging
[0046] sample 180° peeling force (N / 25mm) Rolling ball initial adhesion Sticky at room temperature Water Solubility Example 1 13.8 <3# 2h50min drop 10% dissolved Example 2 14.5 13# 15h drop Completely dissolved Example 3 10 14# 126h drop Completely dissolved Example 4 14.3 <3# 50h drop Completely dissolved Comparative Example 1 9.8 3# 5.5h drop Insoluble Comparative Example 2 6.5 3# 115h drop Insoluble
[0047] It can be seen from the test data of the above 4 embodiments and 2 comparative examples that when the amount of acrylic acid is small, the film cannot be dissolved in water after neutralization. This may be because the amount of acid is too small, and the overall hydrophilicity after neutralization is still not strong enough, resulting in the film being unable to be dissolved in water. It can be seen from Example 1 that after increasing the amount of acrylic acid to 5%, a small amount of the film can be dissolved in water, but it still cannot be completely dissolved, and the initial adhesion after neutralization is generally low. After different soft monomers with stronger hydrophilicity were introduced in Examples 2-4, the water solubility of the film was significantly improved, and even if a built-in curing agent was added, it would not affect the final water solubility. When methoxy polyethylene glycol acrylate with a molecular weight of 400 was selected, the peeling force, rolling ball initial adhesion, room temperature sustained adhesion and water solubility can be better balanced, and the comprehensive performance is optimal.
[0048] Although the present invention has been described above with reference to the embodiments, various modifications may be made thereto and parts thereof may be replaced by equivalents without departing from the scope of the present invention. In particular, as long as there is no structural conflict, the various features in the embodiments disclosed in the present invention may be used in combination with each other in any manner, and the fact that these combinations are not exhaustively described in this specification is only for the sake of omitting space and saving resources. Therefore, the present invention is not limited to the specific embodiments disclosed herein, but includes all technical solutions falling within the scope of the claims.
Claims
1. A one-component water-soluble acrylic pressure-sensitive adhesive, characterized in that: By quality, including: 122 g ethyl acetate, 71 g isopropanol, 57.5 g butyl acrylate, 57.5 g isooctyl acrylate, 20 g acrylic acid, 15 g methyl acrylate, 10 g hydroxyethyl acrylate, 40 g methoxy polyethylene glycol acrylate having a molecular weight of 400, 0.25 g azobisisobutyronitrile, 1.85 g 30% aqueous sodium hydroxide solution, 10.4 g triethanolamine, 1 g acetylacetone and 1 g aluminum acetylacetonate; Among them, the single-component water-soluble acrylic pressure-sensitive adhesive is prepared as follows: Accurately weigh 117g of ethyl acetate and 16g of isopropanol, mix them evenly and add them to the reaction bottle, start to heat up to about 78°C, let the solvent begin to reflux stably, accurately weigh 57.5g of butyl acrylate, 57.5g of isooctyl acrylate, 20g of acrylic acid, 15g of methyl acrylate, 10g of hydroxyethyl acrylate, 40g of methoxy polyethylene glycol acrylate with a molecular weight of 400, and 0.05g of azobisisobutyronitrile, mix them evenly and add them to the constant pressure separatory funnel, drip them in 2 hours, and the addition is completed. Then, the first insulation at reflux temperature was started for 2 hours. After the first insulation was completed, 0.1 g of azobisisobutyronitrile dissolved in 2.5 g of ethyl acetate was added, and the second insulation was started for 1 hour. After the second insulation was completed, 0.1 g of azobisisobutyronitrile dissolved in 2.5 g of ethyl acetate was added, and the third insulation was started for 2 hours. After the third insulation was completed, the temperature began to drop to 40°C, 55 g of isopropanol was added for dilution, 1.85 g of 30% sodium hydroxide aqueous solution and 10.4 g of triethanolamine were added for neutralization, 1 g of acetylacetone and 1 g of aluminum acetylacetonate were added to obtain a hydrosol sample.
2. A method for preparing the one-component water-soluble acrylic pressure-sensitive adhesive according to claim 1, characterized in that: The specific steps are as follows: Accurately weigh 117g of ethyl acetate and 16g of isopropanol, mix them evenly and add them to the reaction bottle, start to heat up to about 78°C, let the solvent begin to reflux stably, accurately weigh 57.5g of butyl acrylate, 57.5g of isooctyl acrylate, 20g of acrylic acid, 15g of methyl acrylate, 10g of hydroxyethyl acrylate, 40g of methoxy polyethylene glycol acrylate with a molecular weight of 400, and 0.05g of azobisisobutyronitrile, mix them evenly and add them to the constant pressure separatory funnel, drip them in 2 hours, and the addition is completed. Then, the first insulation at reflux temperature was started for 2 hours. After the first insulation was completed, 0.1 g of azobisisobutyronitrile dissolved in 2.5 g of ethyl acetate was added, and the second insulation was started for 1 hour. After the second insulation was completed, 0.1 g of azobisisobutyronitrile dissolved in 2.5 g of ethyl acetate was added, and the third insulation was started for 2 hours. After the third insulation was completed, the temperature began to drop to 40°C, 55 g of isopropanol was added for dilution, 1.85 g of 30% sodium hydroxide aqueous solution and 10.4 g of triethanolamine were added for neutralization, 1 g of acetylacetone and 1 g of aluminum acetylacetonate were added to obtain a hydrosol sample.
Citation Information
Patent Citations
Water-soluble polyacrylate pressure-sensitive adhesive for tags and preparation method and application of water-soluble polyacrylate pressure-sensitive adhesive
CN108659752A
Pressure-sensitive adhesive tape, preparation method thereof, and resin composition used for preparing pressure-sensitive adhesive tape
CN110467890A
Benzene-free solvent type peelable pressure-sensitive adhesive and preparation method thereof
CN113549413A
Acrylic acid pressure-sensitive adhesive and preparation method thereof as well as polaroid protective film and preparation method thereof
CN115612428A
Acrylate polymer, pressure-sensitive adhesive composition, protective film, and display device
CN116023603A