A high carbon cold heading steel wire rod for 15.9 grade bolts and its manufacturing method

Through high-carbon carbon components and online salt bath phase change control technology, tempered pearlite and quasi-spherical carbide tissue are formed, which solves the problems of brittleness and high cost of cold heading steel strips, and achieves the high strength of 15.9-level bolts Match with plasticity and improve productivity.

CN118639121BActive Publication Date: 2024-11-19JIANGSU YONGGANG GROUP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411125829.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-19
Estimated Expiration
2044-08-16

AI Technical Summary

Technical Problem

The existing cold heading steel strips have problems with brittleness risks and high material costs in improving tensile strength, making them difficult to effectively apply to the manufacturing of 15.9-level bolts, and the production process is complex and the efficiency is low.

Method used

Designed with high-carbon carbon components, the chemical components include C: 0.85%~0.89%, Si: 0.84%~0.93%, Mn: 0.62%~0.75%. Through the online salt bath phase change regulation technology, tempered pearlite is formed and The microstructure of quasi-spherical carbides combines annealing, drawing and tempering processes to simplify the production process.

Benefits of technology

It achieves high strength and good plastic matching, reduces material costs and cracking risks, simplifies production processes, and adapts to the high strength and lightweight development needs of fasteners.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118639121B_ABST
    Figure CN118639121B_ABST
Patent Text Reader

Abstract

The invention relates to a high-carbon carbon cold-heading steel wire rod for 15.9-grade bolts and a manufacturing method thereof. The wire rod is produced by rolling with a high C-Si-Mn carbon component. After the wire rod is spun into a wire rod at a spinning temperature of ≥905°C, an online salt bath phase transformation control is performed, so that the wire rod is cooled to a pearlite phase region at a cooling rate of ≥30°C / s for isothermal phase transformation, the pearlite phase transformation is promoted, and the formed pearlite structure and carbide are developed into a spheroidized structure. Finally, the cold-heading steel wire rod is produced through slow cooling on a roller table, and the microstructure includes 80%-90% of tempered pearlite and 10%-20% of quasi-spheroidized carbide in volume percentage. The wire rod can achieve high strength and good plasticity matching of the wire rod, the tensile strength is 1350-1400MPa, the cross-sectional shrinkage is 35%-40%, the production process is simplified to manufacture the wire rod, and the wire rod is used for manufacturing fasteners such as 15.9-grade bolts, and the material cost and cracking risk are effectively reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of hot-rolled cold-heading steel wire rods, and in particular relates to a high-carbon carbon cold-heading steel wire rod for 15.9-grade bolts and a manufacturing method thereof. Background Art

[0002] At present, fasteners are mainly 10.9 and 12.9 grade fasteners, and higher strength grade fasteners are rarely developed and applied. With the increasing requirements for lightweight in the automotive, machinery, construction and other industries, supporting fasteners, as important connecting parts of industrial machinery and equipment, are showing a trend of continuous strengthening. Cold heading steel, as the raw material of fasteners, seriously affects the strength grade of fasteners. Therefore, the development of cold heading steel for 15.9 grade bolts with a tensile strength of more than 1500MPa has become urgent, and higher requirements are put forward for the performance of hot-rolled raw cold heading steel. Existing cold heading steel wire rods are generally low- and medium-carbon carbon structural steels and alloy structural steels. In order to improve the strength of steel, high hardenability or micro-alloying elements will be further added on this basis, but at the same time, the material cost will be significantly increased. The high hardenability of steel is easy to induce abnormal structures such as bainite and martensite on the Stelmor cooling line after wire drawing, which brings the risk of steel brittleness and deteriorates the drawing and cold heading performance, for example:

[0003] Patent CN114058974B discloses a 15.9 grade corrosion-resistant high-strength bolt steel and its production method and heat treatment method, which adopts C-Si-Mn-Cr-Mo-V-Nb-Ti-B-Ni-Cu-Al composition design, combines square billet rolling with high-temperature heating roughing, medium rolling, low-temperature sizing and slow cooling on a cooling bed for excellent rod rolling, to obtain pearlite + ferrite, hot-rolled structure without bainite, martensite and other hard phase structures, and further obtains tempered troostite + dispersed carbide structure by reheating for deformation heat treatment and high-frequency tempering heat treatment. However, on the one hand, the material contains high content of Si, Cr, Mo, and also contains V, Nb, Ti and other micro-alloy components. For the purpose of reducing costs, omitting alloys or reducing alloy content will lead to obvious loss of material strength, and the quenching and tempering heat treatment is the best. The performance grade of the final 15.9 grade bolts is unfavorable. Although the risk of abnormal microstructure precipitation is reduced by low-temperature final rolling and slow cooling, and the risk of brittle fracture caused by small wire specifications and large loss of plasticity and toughness after matrix strengthening is avoided by high-quality rod rolling, it will increase the wear of the rolling mill, lose rolling efficiency, extend the online time of the wire rod, and cannot directly obtain wire rods with smaller diameters, which is not conducive to the production of bolts with smaller specifications; on the other hand, the pearlite lamellae formed in the hot-rolled state will cause the dislocations to be restricted in the ferrite when they move to the interface of the lamellar carbide, resulting in a large stress concentration, insufficient plasticity and toughness, brittle fracture of carbides or formation of microcracks. Although the structure is improved by further heat treatment, the steel needs to be reheated and processed multiple times after cooling, which increases the process, energy consumption and cost, affecting production efficiency.

[0004] Carbon is a relatively cheap strengthening element in steel, and replacing alloy elements is beneficial to reducing the cost of steel. However, the high-carbon steel used in the prior art mainly improves the drawing performance by increasing the troostite content in the structure, and is used in the fields of cords, bridge cables, etc. The technical difficulties and causes of its difficulty in applying to the manufacture of cold heading steel wire rods are: First, with the increase of carbon content, the precipitation of abnormal structure is aggravated, which increases the risk of brittleness and plasticity decreasing too quickly. Limited by the cooling rate of the Stelmor air-cooled line after rolling and spinning, the existing high-carbon steel will use low-speed or insulation cooling to reduce the risk of low-temperature structure precipitation, and extend the time of the wire rod in the troostite phase region to increase the proportion of troostite. However, under low-speed cooling, the wire rod stays in the precipitation zone of secondary cementite for a long time, which will produce serious network carbides, which are difficult to eliminate in subsequent annealing and tempering, and will It affects the uniformity and plasticity of the organization and causes the risk of cracking; second, the increase in carbon content increases the difficulty of improving plasticity. Although low-speed or insulation cooling is adopted directly after spinning, the wire rod is in a low-temperature state after the troostite inoculation during the continuous cooling process. After the strengthening elements such as Mn are added to the material, the activity of C is inhibited, which slows down the diffusion, and the cementite precipitation becomes coarser, and finally cannot be softened. The dislocation density of the obtained organization is high, resulting in insufficient plasticity after further annealing, causing wire breakage during drawing or cracking during cold heading; third, although some cold heading steel wire rods increase the ferrite content in the organization to improve the plasticity of the wire rods to regulate the organization, it will excessively deteriorate the strength of the wire rods. In the process of strengthening the bolts by large-area reduction drawing, the plasticity loss is large, which will aggravate the risk of cold heading cracking and make it difficult to reach the 15.9 grade bolt performance level. Summary of the invention

[0005] The present invention aims to solve at least one of the above-mentioned technical problems to a certain extent. The present invention provides a high-carbon carbon cold heading steel wire rod for 15.9 grade bolts and a manufacturing method thereof. The high-carbon carbon component is utilized to achieve wire rod structure regulation, high strength and good plasticity matching, simplify the production process to manufacture the wire rod, and is used to manufacture 15.9 grade bolts and other fasteners, effectively reducing material costs and cracking risks.

[0006] The technical solution adopted by the present invention to solve its technical problem is:

[0007] A high carbon cold heading steel wire rod for 15.9 grade bolts, the chemical composition and mass percentage of the cold heading steel wire rod include: C: 0.85%-0.89%, Si: 0.84%-0.93%, Mn: 0.62%-0.75%, P≤0.015%, S≤0.015%, the rest is Fe and unavoidable impurities, and the microstructure includes a mixed structure consisting of tempered pearlite accounting for 80%-90% by volume and quasi-spheroidized carbide accounting for 10%-20% by volume.

[0008] The chemical composition and mass percentage design basis of the above-mentioned cold heading steel high carbon wire rod include:

[0009] (1) Carbon: As the main strengthening element added in the present invention, the C element has a lower cost than other alloying elements and can play a role in solid solution strengthening to ensure the matrix strength and high hardenability of steel. As an austenite-forming element, it can expand the austenite phase region and inhibit the formation of ferrite. However, it also increases the decarburization sensitivity and the risk of cementite being distributed in a network along the grain boundary. In addition, if the C element content is too high, the obtained tissue lamellae in the medium temperature range will be thicker, which will lead to slow spheroidization and softening of the tissue, which is not conducive to the control of the matrix tissue. Therefore, based on material cost considerations, facilitating tissue control, ensuring the cold deformation performance of cold heading steel wire rods, and meeting the final performance level requirements of 15.9 grade bolts, the mass percentage of C is controlled to be 0.85% to 0.89%.

[0010] (2) Silicon: Si is the main deoxidizing element in steel. As a solid solution hardening element, it helps to improve the strength of wire rod. At the same time, increasing the Si content can increase the activity of C in the online salt bath phase transformation control, inhibit the precipitation of cementite, make the cementite thinner, and thus reduce the difficulty of carbide transforming to spheroidized structure during the isothermal phase transformation of high-temperature molten salt, which is convenient for softening and improves the plasticity of wire rod. Compared with Mo, which can inhibit the precipitation of cementite, Si is cheaper, which is beneficial to control costs. However, excessive silicon will increase the sensitivity of non-metallic inclusions and surface decarburization. As a ferrite-forming element, Si is too high, which is not conducive to the inhibition of ferrite precipitation during the pearlite phase transformation control process. Therefore, the mass percentage of Si is controlled to be 0.84%~0.93%.

[0011] (3) Manganese: Mn is often added to steel as a deoxidizer during the smelting process. As an austenite-forming element, it can expand the austenite phase region and inhibit the formation of ferrite. The solid-solution Mn element can improve the hardenability of steel. In steel, it can refine pearlite by lowering the critical transition temperature, thereby improving the strength of steel. However, excessive Mn content will aggravate the segregation during the solidification process of the steel billet, reduce the activity of carbon and reduce the diffusion rate of carbon, which is not conducive to the spheroidization of carbides, and increase the overheating sensitivity of steel and the risk of abnormal structure. Excessive Mn content will also increase material costs. Therefore, the mass percentage of Mn is controlled to be 0.62%~0.75%.

[0012] (4) Phosphorus and sulfur: P and S are impurity elements. The lower the better. Therefore, P is controlled to be ≤ 0.015% and S is ≤ 0.015%.

[0013] The above-mentioned cold heading steel wire rod is designed with high C-Si-Mn carbon composition, and C is used as the main added element to replace the addition of strong hardenability elements such as Cr, B, Ni and micro-alloy precious metal elements such as Ti, V, Nb, and Mo, which can effectively reduce material costs and maintain a strengthening component system that can achieve a 15.9-grade bolt performance level after quenching and tempering. Compared with the existing cold heading steel hot-rolled metallographic structure composed of pearlite + ferrite soft phase, or the existing cold heading steel wire rod structure that increases the proportion of ferrite in the structure for the purpose of increasing the plasticity of the wire rod, the structure of the cold heading steel wire rod is mainly tempered pearlite, and the austenite forming elements C and Mn are used to expand the austenite phase region and inhibit the precipitation of ferrite. The pearlite has a coarser interlamellar spacing than the troostite, a higher plasticity than the troostite, and a higher strength than the ferrite. Using this strong plasticity suitable The characteristics of the steel wire rod are combined with the high carbon solid solution strengthening effect to make up for the strength loss caused by not adding high alloy content and micro-alloy components, provide matrix strength and appropriate plasticity, and compared with the existing hot-rolled metallographic structure of high carbon steel with a high sorbitization rate, the cold heading steel wire rod transforms pearlite into tempered pearlite through tempering and spheroidizing structure, and the dislocation density is further reduced, and the deformation resistance effect is greatly weakened. Si is combined to increase the C activity and inhibit the precipitation of cementite, so that the carbide is transformed from spheroidizing structure to quasi-spheroidizing carbide, which can be evenly distributed on the plastic matrix, and the organizational stress is further reduced and improved. There is no abnormal organization such as martensite and bainite that is unfavorable to drawing and cold heading, and then on the basis of not excessively deteriorating the strength of the wire rod, the plasticity and toughness of the wire rod are effectively improved through the regulation of the tempered state organization, so as to achieve high strength and plasticity matching of the wire rod.

[0014] In a preferred embodiment, the interlamellar spacing of the tempered pearlite is 155-190 nm, the interlamellar spacing is relatively fine, and the matrix strength is relatively high.

[0015] In a preferred embodiment, the network carbide level of the cold heading steel wire rod is level 0, which can eliminate the network carbon deterioration phase caused by excessive carbon elements and improve the use value of carbon elements.

[0016] In a preferred embodiment, the diameter of the cold heading steel wire rod is 12.0~26.0mm, the tensile strength is 1350~1400MPa, and the cross-sectional shrinkage rate is 35%~40%. Compared with bars, wire rods with smaller diameters can be directly obtained on the high-wire rolling line, reducing the difficulty of manufacturing small-specification bolts. At the same time, as a hot-rolled raw material, it has significantly improved tensile strength and good plasticity, which can avoid the brittle fracture problem during the wire rod coiling process, improve the yield rate, reduce the fracture loss during transportation and downstream unwinding of the coil, and avoid material waste. 15.9 grade bolts can be manufactured through annealing, drawing, cold heading and tempering processes. Due to the high strength and plasticity of the cold heading steel wire rod, there is no need for excessive deep drawing to reduce the surface and increase the strength, which can effectively reduce the risk of wire breakage during drawing and cracking during cold heading. Due to the high carbon carbon strengthening component system, it is also convenient to achieve the final performance level through tempering after cold heading.

[0017] A method for manufacturing a high-carbon carbon cold heading steel wire rod for 15.9-grade bolts, the manufacturing method comprising:

[0018] The wire rod is produced by rolling the chemical composition of the high carbon cold heading steel wire rod for 15.9 grade bolts according to any one of the above items. After the wire rod is spun into a wire rod at a spinning temperature of ≥905°C, an online salt bath phase transformation control is performed to cool the wire rod to the pearlite phase region at a cooling rate of ≥30°C / s for isothermal phase transformation, promote pearlite phase transformation, and develop the formed pearlite structure and carbide into spheroidized structure. Finally, it is slowly cooled by a roller to produce a cold heading steel wire rod with a mixed structure composed of tempered pearlite accounting for 80% to 90% by volume and quasi-spheroidized carbide accounting for 10% to 20% by volume.

[0019] The above-mentioned manufacturing method uses a higher spinning temperature to avoid the precipitation of network carbides in the spinning stage, and directly performs online salt bath phase transformation control after spinning. On the one hand, compared with the existing low-speed or heat preservation cooling process after spinning, the high heat exchange performance of molten salt can be used to significantly improve the cooling rate of the wire rod, so that the wire rod can be quickly cooled from the austenitizing temperature, skipping the precipitation range of secondary cementite, inhibiting the precipitation of secondary network carbides, and eliminating the adverse effect of network carbon on the wire rod. At the same time, high C and Mn are used to expand the austenite phase region and inhibit ferrite precipitation. Compared with increasing the cooling rate of the Stelmor air-cooled line, the risk of abnormal tissue precipitation will be aggravated due to the increase in the temperature difference of the wire rod. When the wire rod is regulated by molten salt, the molten salt is wrapped on the surface of the wire rod, and there is no temperature difference between the windward side and the leeward side. The temperature drops quickly and evenly, and the wire rod can quickly enter the pearlite phase region, avoiding the risk of abnormal tissue precipitation of martensite and bainite brittle tissue caused by high carbon.

[0020] On the other hand, compared with the insulation cooling but still keeping the wire rod in a state of continuous cooling, the wire rod can be kept consistent with the molten salt temperature when it is regulated by the online salt bath phase transformation, and can be subjected to high-temperature isothermal treatment for a longer time, so that the austenite structure in the wire rod is transformed into pearlite structure in the pearlite phase region, and Si is combined to make the cementite lamellae thinner. The pearlite structure formed by the phase transformation continues to isothermally develop towards the spheroidized structure in the high-temperature molten salt, and the carbide transforms to spheroidization, which promotes the softening of the matrix and reduces the tissue stress and dislocation density. At the same time, the full transformation of the organization also avoids the generation of abnormal organization in the subsequent cooling process. Finally, it is slowly cooled by the roller, and the high temperature state of the wire rod after the molten salt isothermal treatment is used to continue the spheroidization effect, promote the further softening of the wire rod, realize the organization regulation and strength-plasticity matching, and can directly obtain a structure dominated by tempered pearlite and a small amount of quasi-spheroidized carbide. Compared with the existing process, it can also save the further heat treatment process before annealing, so that the efficiency and yield of cold heading steel wire rod can be improved.

[0021] Since the cold heading steel wire rod has a high carbon content and a relatively simple composition, a lower heating furnace temperature and time in the furnace, combined with appropriate soaking time, can promote the homogenization of the steel billet composition before rolling, and reduce the decarburization tendency of the steel billet by controlling the lower oxygen content in the furnace. In a preferred embodiment, the heating furnace temperature is controlled to be ≤1075°C before rolling, the soaking time is 2~3h, the time in the furnace is 3~5h, and the oxygen content in the furnace is ≤1.4%.

[0022] Since the wire rod spinning temperature is relatively high, the limitation of low-temperature spinning on low-temperature rolling can be broken, and a higher rolling temperature is selected to reduce the deformation resistance of the steel billet and the wear on the rolling line, thereby improving the rolling efficiency. At the same time, the risk of decarburization caused by excessively high rolling temperature is avoided. The appropriate initial rolling temperature is combined with a larger initial rolling reduction to appropriately refine the grains. In a preferred embodiment, during the rolling, the initial rolling temperature is controlled to be 1030~1050℃, and the initial rolling reduction is 24%~34%.

[0023] Since the initial rolling temperature is relatively high, a higher final rolling temperature can be further used to promote uniform composition and increase the rolling speed, and a larger final rolling reduction can be used to carry out dynamic recrystallization, refine the grains, strengthen the matrix, and prepare the organization for pearlite nucleation. In a preferred embodiment, during the rolling, the final rolling temperature is controlled to be ≥920°C, and the final rolling reduction is 28%~38%.

[0024] In a preferred embodiment, the molten salt temperature for online salt bath phase transformation control is 575-615°C, and the processing time is 450-650s. The lower the molten salt temperature, the finer the pearlite lamella spacing, the higher the matrix strength after tempering, the increased strength of the wire rod and the decreased plasticity. However, if the molten salt temperature is too low, a large undercooling degree is formed, which promotes the nucleation of troostite with finer lamella spacing, which is not conducive to the plasticity of the wire rod. Even when the molten salt temperature is lower, bainite is formed and precipitated, which significantly deteriorates the plasticity of the wire rod. On the contrary, the higher the molten salt temperature, the larger the pearlite lamella spacing is formed, which can provide more thermal power for the organization to develop towards spheroidization, thereby reducing the strength of the wire rod and increasing the plasticity. However, if the molten salt temperature is too high, the formed Too large spacing between pearlite lamellae or even high temperature will cause ferrite to form and precipitate, which is not good for matrix strength. The longer the treatment time, the better the spheroidization of the organization and the softening of the matrix. However, too long a treatment time will also increase energy consumption and reduce efficiency. The strength will be lost due to excessive softening of pearlite, and the strength and plasticity will decrease due to the growth but agglomeration of quasi-spheroidized carbides. Conversely, the shorter the treatment time, the worse the softening effect, and even the austenite is not fully transformed into pearlite, resulting in abnormal organization or residual austenite, which is not good for the performance of the wire rod. Therefore, the molten salt temperature and treatment time can be further controlled to make the wire rod undergo isothermal phase transformation and spheroidization transformation in the high-temperature molten salt in the pearlite phase region to regulate the matrix organization.

[0025] In a preferred embodiment, the molten salt circulation rate of the online salt bath phase change regulation is 450~650t / h, and the molten salt temperature rise is ≤7°C. A larger molten salt circulation rate can be used to control the molten salt temperature rise, control the wire rod cooling rate and the online salt bath phase change regulation accuracy, and avoid excessive molten salt circulation rate causing increased supercooling and unnecessary energy consumption.

[0026] In a preferred embodiment, the roller slow cooling controls the wire rod to be cooled at a cooling rate of 0.9-1.5°C / s to avoid loss of plasticity due to excessively high cooling rate and loss of manufacturing efficiency due to excessively low cooling rate, thereby further controlling the cooling and softening effect of the wire rod during the roller slow cooling stage.

[0027] In a preferred embodiment, the roller slow cooling adopts closing the heat preservation cover, cooling to below 300° C. and then coiling, which can achieve a better softening effect and facilitate coiling.

[0028] Compared with the prior art, the beneficial effects of the present invention are at least:

[0029] (1) In view of the current situation that the development of cold heading steel wire rods for 15.9 grade fasteners with higher strength is difficult and costly, the cold heading steel wire rods of the present invention are designed with a high C-Si-Mn carbon component, and C is used to replace the addition of expensive alloys, which can effectively reduce material costs and ensure a strengthening component system. At the same time, austenite forming elements C and Mn are used to expand the austenite phase region and inhibit ferrite precipitation. Si is used to increase C activity and inhibit cementite precipitation, so that the microstructure is mainly tempered pearlite with a small amount of quasi-spheroidized carbon. It makes up for the strength loss caused by not adding high alloy content and micro-alloy components. It effectively improves the plasticity and toughness of wire rod through tempering state organization regulation, realizes the matching of high strength and plasticity of wire rod, reaches a tensile strength of 1350~1400MPa, and a cross-sectional shrinkage rate of 35%~40%. It can manufacture 15.9 grade bolts through annealing, drawing, cold heading and tempering process, effectively reducing material cost and cracking risk, adapting to the development needs of high strength and lightweight application of fasteners, and has good market application prospects.

[0030] (2) In view of the current situation that the manufacturing and development of cold heading steel wire rod for 15.9 grade fasteners is difficult, costly and has many processes, the manufacturing method of the present invention combines the high carbon chemical composition design with the online salt bath phase change control technology. It can eliminate the network carbon deterioration phase caused by excessive carbon element through the rapid heat exchange capacity of molten salt, improve the use value of carbon element, and control the rapid entry into the pearlite phase region for isothermal phase change. The pearlite structure formed after the phase change continues to be isothermal in the high-temperature molten salt and develops into a spheroidized structure, promoting the spheroidization of the structure and the softening of the matrix. Finally, the slow cooling by rollers promotes the further softening of the wire rod, which can avoid abnormal hard phase structures such as bainite and martensite, avoid the brittle fracture problem during the wire rod winding process, improve the yield rate, and also save the further heat treatment process before annealing, simplify the production process for manufacturing wire rods, realize structure control and strength-plasticity matching, and have good industrial adaptability. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:

[0032] Figure 1 is a metallographic structure diagram of Example 1 of the present invention;

[0033] Figure 2 is the metallographic structure diagram of Example 2 of the present invention;

[0034] Figure 3 It is the metallographic structure diagram of Example 3 of the present invention. DETAILED DESCRIPTION

[0035] The embodiments described below with reference to the accompanying drawings are exemplary and are only for illustration and do not limit the description of the features and characteristics of the present invention. They are intended to be used to explain the present invention and are sufficient to enable those skilled in the art to implement the present invention. They should not be construed as limiting the scope of the present invention, which is limited only by the appended claims. Embodiment 1:

[0036] A preferred embodiment of the manufacturing method of the cold heading steel high carbon hot rolled wire rod for 15.9 grade bolts of the present invention, the chemical composition and mass percentage of the high carbon hot rolled wire rod include: C: 0.85%, Si: 0.84%, Mn: 0.72%, P: 0.015%, S: 0.012%, and the rest is Fe and unavoidable impurities, and the manufacturing method thereof is manufactured according to the process flow of rolling → spinning → online salt bath phase change control → roller slow cooling → coiling, specifically:

[0037] The rolling process is used to heat a steel billet with a specification of 220mm×220mm through a heating furnace to promote the homogenization of the steel billet composition and reduce the decarburization tendency of the steel billet. After heating to a high-temperature steel billet with rollable plasticity, the steel billet coming out of the heating furnace is rolled into a wire with a diameter of 16mm through a rolling line. A higher rolling temperature is selected to reduce the wear of the steel billet on the rolling line and improve the rolling efficiency. A larger reduction is used to appropriately refine the grains. Specifically: the heating furnace is heated in sequence according to the preheating section, the heating section, and the soaking section. , control the heating furnace temperature to 1065℃, the soaking time to 2.5h, the furnace time to 4h, the oxygen content in the furnace ≤1.4%, the initial rolling temperature to 1040℃, the initial rolling reduction to 30%, the final rolling temperature to 930℃, and the final rolling reduction to 36%; the wire-spinning process is used to convert the wire rods leaving the rolling line into wire rods through a wire-spinning mechanism, and the wire rods are spread on the rollers and transported along the rollers to avoid the risk of cementite precipitation and grain coarsening caused by the high carbon steel being too low in the wire-spinning stage. Specifically: the wire-spinning temperature is controlled to be 910℃.

[0038] The online salt bath phase change control adopts a salt bath tank with molten salt inside. The wire rod after spinning is conveyed through the salt bath tank by rollers and quickly cooled to the molten salt temperature, so that the wire rod is cooled at a cooling rate of 30°C / s, and quickly passes through the precipitation temperature range of secondary cementite, eliminates the network carbon deterioration phase caused by excessive carbon element, and is cooled to the pearlite phase region for isothermal phase change, promotes the phase transformation of austenite to pearlite structure, and makes the formed pearlite structure and carbide develop into spheroidized structure, reduces tissue stress and dislocation density, and promotes matrix softening. Specifically: the molten salt temperature is controlled to be 615°C, the processing time is 650s, the molten salt circulation volume is 450t / h, and the molten salt temperature rise is ≤7°C.

[0039] The roller slow cooling process adopts closing the heat preservation cover, conveying the wire rod from the salt bath tank into the heat preservation cover by rollers, reducing the temperature drop rate of the wire rod, performing slow cooling treatment, and promoting further softening of the wire rod structure. Specifically: the wire rod is controlled to cool to 285°C at a cooling rate of 1.5°C / s; the coiling process is used to coil the wire rod into a coil through a coiling drum, and obtain a high-carbon hot-rolled wire rod product after packaging and storage. Its metallographic structure diagram is as follows Figure 1 shown.

[0040] Comparative Example 1:

[0041] A method for manufacturing wire rod, which differs from Example 1 in that the method is manufactured according to the process flow of low-temperature rolling → low-temperature wire drawing → Stelmor insulation and slow cooling, specifically: the low-temperature rolling controls the heating furnace temperature to 1050°C, the soaking time to 3.5h, the furnace time to 5h, the oxygen content in the furnace ≤1.4%, the initial rolling temperature to 1000°C, the initial rolling reduction to 30%, the final rolling temperature to 800°C, the final rolling reduction to 36%, the wire drawing temperature of the low-temperature wire drawing is 780°C, the Stelmor insulation and slow cooling adopts the method of shutting down all fans and insulation covers, and conveying the wire rod with rollers, the wire rod completes phase change in the cover at a cooling rate of 1.2°C / s, and the finished wire rod is obtained after it comes off the line.

[0042] Comparative Example 2:

[0043] A method for manufacturing a wire rod, which differs from that of Example 1 in that the method is manufactured according to a process flow of low-temperature rolling → low-temperature wire drawing → Stelmor air cooling → insulation and slow cooling. Specifically: the low-temperature rolling controls the heating furnace temperature to 1060°C, the soaking time to 4.5h, the furnace time to 5h, the furnace oxygen content ≤1.4%, the initial rolling temperature to 1015°C, the initial rolling reduction to 30%, the final rolling temperature to 875°C, the final rolling reduction to 36%, the wire drawing temperature of the low-temperature wire drawing to 850°C, the Stelmor air cooling to open 1~6# fans at 25%, so that the wire rod is cooled to 680°C at a cooling rate of 3.6°C / s, the insulation and slow cooling to close all fans and insulation covers to complete the phase change of the wire rod in the cover at a cooling rate of 1.5°C / s, and the finished wire rod is obtained after the coil is rolled off the line. Embodiment 2:

[0044] A preferred embodiment of the manufacturing method of the cold heading steel high carbon hot rolled wire rod for grade 15.9 bolts of the present invention, the chemical composition and mass percentage of the high carbon hot rolled wire rod include: C: 0.89%, Si: 0.86%, Mn: 0.68%, P: 0.012%, S: 0.011%, and the rest is Fe and unavoidable impurities, and the manufacturing method thereof is manufactured according to the process flow of rolling → spinning → online salt bath phase change control → roller slow cooling → coiling, specifically:

[0045] The rolling process is used to heat a steel billet with a specification of 220 mm×220 mm through a heating furnace to promote the homogenization of the steel billet composition and reduce the decarburization tendency of the steel billet. After heating to a high-temperature steel billet with rollable plasticity, the steel billet coming out of the heating furnace is rolled into a wire with a diameter of 26 mm through a rolling line. A higher rolling temperature is selected to reduce the wear of the steel billet on the rolling line and improve the rolling efficiency. A larger reduction is used to appropriately refine the grains. Specifically, the heating furnace is heated in sequence according to the preheating section, the heating section, and the soaking section. The heating furnace temperature is controlled to be 1070°C, the soaking time is 2.5h, the time in the furnace is 4.5h, the oxygen content in the furnace is ≤1.2%, the initial rolling temperature is 1045°C, the initial rolling reduction is 24%, the final rolling temperature is 935°C, and the final rolling reduction is 28%; the wire-spinning process is used to convert the wire rods exiting the rolling line into wire rods through a wire-spinning mechanism, and the wire rods are spread on the rollers and transported along the rollers to avoid the risk of cementite precipitation and grain coarsening caused by excessively low temperature of high carbon steel in the wire-spinning stage. Specifically: the wire-spinning temperature is controlled to be 915°C.

[0046] The online salt bath phase change control adopts a salt bath tank with molten salt inside. The wire rod after spinning is conveyed through the salt bath tank by rollers and quickly cooled to the molten salt temperature, so that the wire rod is cooled at a cooling rate of 31°C / s, and quickly passes through the precipitation temperature range of secondary cementite, eliminates the network carbon deterioration phase caused by excessive carbon element, and is cooled to the pearlite phase region for isothermal phase transformation, promotes the phase transformation of austenite to pearlite structure, and makes the formed pearlite structure and carbide develop into spheroidized structure, reduces tissue stress and dislocation density, and promotes matrix softening. Specifically: the molten salt temperature is controlled to be 603°C, the processing time is 605s, the molten salt circulation volume is 500t / h, and the molten salt temperature rise is ≤7°C.

[0047] The roller slow cooling process adopts closing the heat preservation cover, conveying the wire rod from the salt bath tank into the heat preservation cover by rollers, reducing the temperature drop rate of the wire rod, performing slow cooling treatment, and promoting further softening of the wire rod structure. Specifically: the wire rod is controlled to cool to 290°C at a cooling rate of 1.4°C / s; the coiling process is used to coil the wire rod into a coil through a coiling drum, and obtain a high-carbon hot-rolled wire rod product after packaging and storage. Its metallographic structure diagram is as follows Figure 2 shown.

[0048] Comparative Example 3:

[0049] A method for manufacturing a wire rod, which differs from Example 2 in that the heating furnace temperature is controlled to be 1060°C, the soaking time is 3 hours, the furnace time is 5 hours, the initial rolling temperature is 1020°C, the final rolling temperature is 905°C, and the spinning temperature is 885°C. During the online salt bath phase change regulation, the wire rod is cooled at a cooling rate of 29°C / s, and the finished wire rod is obtained after it comes off the line.

[0050] Comparative Example 4:

[0051] A method for manufacturing wire rod, which differs from Example 2 in that, during the online salt bath phase change regulation, the wire rod is cooled at a cooling rate of 36°C / s, the molten salt temperature is 555°C, the molten salt circulation rate is 700t / h, and the finished wire rod is obtained after going offline.

[0052] Comparative Example 5:

[0053] A method for manufacturing a wire rod, which differs from Example 2 in that, during the online salt bath phase change regulation, the wire rod is cooled at a cooling rate of 30°C / s, the molten salt temperature is 625°C, and the finished wire rod is obtained after going offline. Embodiment 3:

[0054] A preferred embodiment of the manufacturing method of the cold heading steel high carbon hot rolled wire rod for 15.9 grade bolts of the present invention, the chemical composition and mass percentage of the high carbon hot rolled wire rod include: C: 0.88%, Si: 0.9%, Mn: 0.62%, P: 0.013%, S: 0.015%, and the rest are Fe and unavoidable impurities, and the manufacturing method thereof is manufactured according to the process flow of rolling → spinning → online salt bath phase change control → roller slow cooling → coiling, specifically:

[0055] The rolling process is used to heat a steel billet with a specification of 220mm×220mm through a heating furnace to promote the homogenization of the steel billet composition and reduce the decarburization tendency of the steel billet. After heating to a high-temperature steel billet with rollable plasticity, the steel billet coming out of the heating furnace is rolled into a wire with a diameter of 12mm through a rolling line. A higher rolling temperature is selected to reduce the wear of the steel billet on the rolling line and improve the rolling efficiency. A larger reduction is used to appropriately refine the grains. Specifically: the heating furnace is sequentially upgraded in the preheating section, the heating section, and the soaking section. Temperature, control the heating furnace temperature to 1060℃, the soaking time to 2h, the time in the furnace to 3h, the oxygen content in the furnace ≤1.3%, the initial rolling temperature to 1030℃, the initial rolling reduction to 34%, the final rolling temperature to 920℃, and the final rolling reduction to 38%; the wire-spinning process is used to convert the wire rods leaving the rolling line into wire rods through a wire-spinning mechanism, and the wire rods are spread on the roller table and transported along the roller table to avoid the risk of cementite precipitation and grain coarsening caused by excessively low temperature of high carbon steel in the wire-spinning stage. Specifically: the wire-spinning temperature is controlled to 905℃.

[0056] The online salt bath phase change control adopts a salt bath tank with molten salt inside. The wire rod after spinning is conveyed through the salt bath tank by rollers and quickly cooled to the molten salt temperature, so that the wire rod is cooled at a cooling rate of 32°C / s, and quickly passes through the precipitation temperature range of secondary cementite, eliminates the network carbon deterioration phase caused by excessive carbon element, and is cooled to the pearlite phase region for isothermal phase change, promotes the phase transformation of austenite to pearlite structure, and makes the formed pearlite structure and carbide develop into spheroidized structure, reduces tissue stress and dislocation density, and promotes matrix softening. Specifically: the molten salt temperature is controlled to be 584°C, the processing time is 513s, the molten salt circulation volume is 580t / h, and the molten salt temperature rise is ≤7°C.

[0057] The roller slow cooling process adopts closing the heat preservation cover, conveying the wire rod from the salt bath tank into the heat preservation cover by rollers, reducing the temperature drop rate of the wire rod, performing slow cooling treatment, and promoting further softening of the wire rod structure. Specifically: the wire rod is controlled to cool to 280°C at a cooling rate of 1.2°C / s; the coiling process is used to coil the wire rod into a coil through a coiling drum, and obtain a high-carbon hot-rolled wire rod product after packaging and storage. Its metallographic structure diagram is as follows Figure 3 shown.

[0058] Comparative Example 6:

[0059] A method for manufacturing a wire rod, which differs from that of Example 3 in that the processing time of the online salt bath phase change regulation is 420s, and the finished wire rod is obtained after going offline.

[0060] Comparative Example 7:

[0061] A method for manufacturing a wire rod, which differs from Example 3 in that the processing time of the online salt bath phase change regulation is 700s, and the finished wire rod is obtained after going offline. Embodiment 4:

[0062] A preferred embodiment of the manufacturing method of the cold heading steel high carbon hot rolled wire rod for 15.9 grade bolts of the present invention, the chemical composition and mass percentage of the high carbon hot rolled wire rod include: C: 0.88%, Si: 0.93%, Mn: 0.75%, P: 0.013%, S: 0.014%, and the rest is Fe and unavoidable impurities, and the manufacturing method thereof is manufactured according to the process flow of rolling → spinning → online salt bath phase change control → roller slow cooling → coiling, specifically:

[0063] The rolling process is used to heat a steel billet with a specification of 220mm×220mm through a heating furnace to promote the homogenization of the steel billet composition and reduce the decarburization tendency of the steel billet. After heating to a high-temperature steel billet with rollable plasticity, the steel billet coming out of the heating furnace is rolled into a wire with a diameter of 22mm through a rolling line. A higher rolling temperature is selected to reduce the wear of the steel billet on the rolling line and improve the rolling efficiency. A larger reduction is used to appropriately refine the grains. Specifically: the heating furnace is sequentially upgraded in the preheating section, the heating section, and the soaking section. Temperature, control the heating furnace temperature to 1075℃, the soaking time to 3h, the time in the furnace to 5h, the oxygen content in the furnace ≤1.3%, the initial rolling temperature to 1050℃, the initial rolling reduction to 28%, the final rolling temperature to 945℃, and the final rolling reduction to 30%; the wire-spinning process is used to convert the wire rods leaving the rolling line into wire rods through a wire-spinning mechanism, and the wire rods are spread on the rollers and transported along the rollers to avoid the risk of cementite precipitation and grain coarsening caused by excessively low temperature of high carbon steel in the wire-spinning stage. Specifically: the wire-spinning temperature is controlled to be 925℃.

[0064] The online salt bath phase change control adopts a salt bath tank with molten salt inside. The wire rod after spinning is conveyed through the salt bath tank by rollers and quickly cooled to the molten salt temperature, so that the wire rod is cooled at a cooling rate of 33°C / s, and quickly passes through the precipitation temperature range of secondary cementite, eliminates the network carbon deterioration phase caused by excessive carbon element, and is cooled to the pearlite phase region for isothermal phase transformation, promotes the phase transformation of austenite to pearlite structure, and makes the formed pearlite structure and carbide develop into spheroidized structure, reduces tissue stress and dislocation density, and promotes matrix softening. Specifically: the molten salt temperature is controlled to be 575°C, the processing time is 450s, the molten salt circulation volume is 650t / h, and the molten salt temperature rise is ≤7°C.

[0065] The roller slow cooling process adopts closing the insulation cover, and conveying the wire rod coming out of the salt bath tank into the insulation cover by rollers, reducing the temperature drop rate of the wire rod, performing slow cooling treatment, and promoting further softening of the wire rod structure. Specifically: the wire rod is controlled to be cooled to 295°C at a cooling rate of 0.9°C / s; the coiling process is used to coil the wire rod into coils through the coiling drum, and obtain the high carbon hot rolled wire rod finished product after packaging and storage.

[0066] Comparative Example 8:

[0067] A method for manufacturing a wire rod, which differs from Example 4 in that the method is manufactured according to a process flow of rolling → spinning → online salt bath phase change control → air cooling. Specifically: the air cooling process adopts opening a heat preservation cover, using a roller to transport the wire rod out of the salt bath tank for air cooling, and controlling the wire rod to be cooled to 295°C at a cooling rate of 2.3°C / s, and obtaining a finished wire rod after it comes off the line.

[0068] The wire rods obtained in the above-mentioned Examples 1 to 4 and Comparative Examples 1 to 8 were subjected to organizational and performance tests: the tensile test was conducted according to GB-T 228.1-2021 Metallic Material Tensile Test Part 1: Room Temperature Test Method to obtain tensile strength and cross-sectional shrinkage, and the organizational test was conducted according to the metal microstructure detection method of GB / T13298 standard. The comparative results obtained are shown in Table 1 below:

[0069] Table 1. Comparison of wire rod structure properties with different compositions and manufacturing methods

[0070]

[0071] From the comparison results of Example 1 and Comparative Example 1, it can be seen that compared with the troostite + ferrite structure obtained after low-temperature wire drawing and insulation cooling, serious network carbides are produced, and the resulting structure has a high dislocation density, which is easy to cause wire breakage during drawing or cracking during cold heading. The present invention can eliminate the network carbon deterioration phase caused by excessive carbon elements through the design of high-carbon carbon chemical composition combined with online salt bath phase change control technology, thereby improving the use value of carbon elements, and at the same time controlling the rapid entry into the pearlite phase region for isothermal phase transformation, cooperating with austenite forming elements C and Mn to expand the austenite phase region, inhibiting ferrite precipitation, and continuously isothermally promoting structure spheroidization and matrix softening in high-temperature molten salt, and can effectively improve the plasticity and toughness properties of the wire rod through tempered structure control.

[0072] From the comparison results of Example 1 and Comparative Example 2, it can be seen that compared with increasing the spinning temperature and the Stelmor air-cooling intensity, the risk of abnormal tissue precipitation and increased brittleness and excessive decrease in plasticity is aggravated, and the resulting pearlite lamellae have a large spacing and cannot be softened. The present invention avoids the risk of precipitation of brittle abnormal tissues of martensite and bainite caused by high carbon. The pearlite tissue formed by phase transformation continues to isothermally develop into a spheroidized tissue in a high-temperature molten salt, and the carbide transforms into a spheroidized structure, which promotes matrix softening and achieves high strength and plasticity matching of the wire rod.

[0073] It can be seen from Examples 1 to 4 that the present invention adopts a high C-Si-Mn carbon component design to achieve a tensile strength of 1350 to 1400 MPa and a cross-sectional reduction rate of 35% to 40%. 15.9 grade bolts can be manufactured through annealing, drawing, cold heading and tempering processes, which can effectively reduce material costs and cracking risks.

[0074] It can be seen from the comparison results of Example 2 and Comparative Example 3 that the selection of a higher spinning temperature can avoid the precipitation of network carbides in the spinning stage, and can also break the limitation of low-temperature spinning on low-temperature rolling, reduce rolling wear, improve rolling efficiency, and prepare the organization for pearlite nucleation; it can be seen from the comparison results of Example 2 and Comparative Example 4 that the lower the molten salt temperature, the finer the spacing between the pearlite lamellae formed, and the higher the matrix strength after tempering, but the molten salt temperature is too low, which promotes the nucleation of troostite with finer lamellae spacing, which is not conducive to the plasticity of the wire rod; it can be seen from the comparison results of Example 2 and Comparative Example 5 that the higher the molten salt temperature, the larger the spacing between the pearlite lamellae formed, which can provide more thermal power for the development of the organization towards spheroidization, but the molten salt temperature is too high, there is a risk of ferrite precipitation, which is not conducive to the matrix strength.

[0075] From the comparison results of Example 3 and Comparative Example 6, it can be seen that the shorter the treatment time of the online salt bath phase change regulation, the worse the softening effect, which is detrimental to the plasticity of the wire rod; from the comparison results of Example 3 and Comparative Example 7, it can be seen that the longer the treatment time of the online salt bath phase change regulation, the better the tissue spheroidization and matrix softening effect, but too long a time will lead to a decrease in strength and plasticity due to the growth but agglomeration of quasi-spheroidized carbides. From the comparison results of Example 4 and Comparative Example 8, it can be seen that after slow cooling on a roller, the high temperature state of the wire rod after isothermal treatment with molten salt can be used to continue the spheroidization effect, thereby promoting further softening of the wire rod.

[0076] The series of detailed descriptions listed above are only specific descriptions of feasible embodiments of the present invention. They are not intended to limit the scope of protection of the present invention. All equivalent embodiments or changes that do not deviate from the technical spirit of the present invention should be included in the scope of protection of the present invention.

Claims

1. A high carbon cold heading steel wire rod for 15.9 grade bolts, characterized in that: The chemical composition and mass percentage of the cold heading steel wire rod include: C: 0.85% to 0.89%, Si: 0.84% ​​to 0.93%, Mn: 0.62% to 0.75%, P≤0.015%, S≤0.015%, and the rest are Fe and unavoidable impurities. The microstructure includes a mixed structure composed of tempered pearlite accounting for 80% to 90% by volume and quasi-spheroidized carbides accounting for 10% to 20% by volume. The manufacturing method includes: The wire rod is produced by rolling according to the chemical composition of the high carbon cold heading steel wire rod for 15.9 grade bolts. After the wire rod is spun into a wire rod at a spinning temperature of ≥905°C, an online salt bath phase transformation control is performed, so that the wire rod is cooled to the pearlite phase region at a cooling rate of ≥30°C / s for isothermal phase transformation, the pearlite phase transformation is promoted, and the formed pearlite structure and carbide develop into a spheroidized structure. Finally, it is slowly cooled by a roller to produce a cold heading steel wire rod with a mixed structure composed of tempered pearlite and quasi-spheroidized carbide; the molten salt temperature for the online salt bath phase transformation control is 575-615°C, and the processing time is 450-650s.

2. The high carbon cold heading steel wire rod for 15.9 grade bolts according to claim 1, characterized in that: The interlamellar spacing of the tempered pearlite is 155-190 nm, and the network carbide level of the cold heading steel wire rod is level 0.

3. The high carbon cold heading steel wire rod for 15.9 grade bolts according to claim 1 or 2, characterized in that: The diameter of the cold heading steel wire rod is 12.0-26.0 mm, the tensile strength is 1350-1400 MPa, and the cross-sectional shrinkage is 35%-40%.

4. A method for manufacturing high carbon cold heading steel wire rod for 15.9 grade bolts, characterized in that: The manufacturing method thereof comprises: The wire rod is produced by rolling the chemical composition of the high-carbon carbon cold heading steel wire rod for 15.9 grade bolts according to claim 1. After the wire rod is spun into a wire rod at a spinning temperature of ≥905°C, an online salt bath phase transformation control is performed, so that the wire rod is cooled to the pearlite phase region at a cooling rate of ≥30°C / s for isothermal phase transformation, the pearlite phase transformation is promoted, and the formed pearlite structure and carbide develop into a spheroidized structure. Finally, it is slowly cooled by a roller to produce a cold heading steel wire rod with a mixed structure composed of 80% to 90% tempered pearlite and 10% to 20% quasi-spheroidized carbide by volume. The molten salt temperature for the online salt bath phase transformation control is 575 to 615°C, and the processing time is 450 to 650s.

5. The method for manufacturing high carbon cold heading steel wire rod for 15.9 grade bolts according to claim 4, characterized in that: Before rolling, the heating furnace temperature is controlled to be ≤1075°C, the soaking time is 2-3h, the time in the furnace is 3-5h, and the oxygen content in the furnace is ≤1.4%.

6. The method for manufacturing high carbon cold heading steel wire rod for 15.9 grade bolts according to claim 4, characterized in that: During the rolling, the initial rolling temperature is controlled to be 1030-1050° C., the initial rolling reduction is 24%-34%, the final rolling temperature is ≥920° C., and the final rolling reduction is 28%-38%.

7. The method for manufacturing high carbon cold heading steel wire rod for 15.9 grade bolts according to claim 4, characterized in that: The molten salt circulation rate controlled by the online salt bath phase change is 450-650t / h, and the molten salt temperature rise is ≤7°C.

8. The method for manufacturing high carbon cold heading steel wire rod for 15.9 grade bolts according to claim 4, characterized in that: The roller slow cooling controls the wire rod to cool at a cooling rate of 0.9-1.5°C / s.

9. The method for manufacturing the high carbon cold heading steel wire rod for 15.9 grade bolts according to claim 8, characterized in that: The roller slow cooling adopts closing the heat preservation cover, cooling to below 300° C. and coiling.