On-board calibration board and preparation method thereof, and on-board calibration device

By setting up growth substrate, doping layer and partition layer on the star calibration plate, combined with the structure of the protective layer, the problems of easy blockage of the multi-porous plate and insufficient environmental resistance are solved, and Lambertian and resistance enhancement are achieved Effect.

CN118640956BActive Publication Date: 2024-11-19JIHUA LAB
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411105170.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-19
Estimated Expiration
2044-08-13

AI Technical Summary

Technical Problem

Existing multi-porous plates as star-mounted plates are susceptible to blockage in the cosmic environment, difficult to preserve, and lack the ability to resist cosmic particles and ultraviolet radiation.

Method used

The attenuation layer with a growth substrate, a doped layer and a partition layer is plated on the substrate. Combined with the structure of the protective layer, the attenuation and diffuse transmission of sunlight are achieved by stacking the doped layer and partition layer, instead of the attenuation of the porous plate. It can prevent micropore blockage and protect against cosmic particles and ultraviolet radiation through protective layers.

Benefits of technology

The Lambertian nature of the star-on-sized calibration plate is realized, avoiding the problem of micropore blockage, and at the same time enhancing the resistance to cosmic particles and ultraviolet radiation, ensuring the long-term stability and storage of the scale plate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118640956B_ABST
    Figure CN118640956B_ABST
Patent Text Reader

Abstract

The present application discloses an on-board calibration plate and its preparation method, and an on-board calibration device, belonging to the field of aerospace remote sensing technology. The on-board calibration plate comprises: a substrate, and a growth substrate, an attenuation layer, and a protective layer sequentially located on the light incident side of the substrate; the attenuation layer comprises a stacked doping layer and a blocking layer, and the doping layer is in contact with the growth substrate; the doping layer comprises a first material and a second material, and the transmittance between the first material and the second material differs by at least 10%. The present application solves the technical problem that the micropores of the porous plate used as an on-board calibration plate are easily clogged, resulting in difficulty in preservation, and the protective layer can resist the erosion of cosmic particles and ultraviolet radiation in the on-board calibration working environment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of aerospace remote sensing technology, and in particular to an on-board calibration plate and a preparation method thereof, and an on-board calibration device. Background Art

[0002] With the development of satellite-based quantitative remote sensing technology, onboard calibration technology has become increasingly important. Conventional onboard calibration sources, such as diffuse reflection and transmission plates made of materials like quartz and polytetrafluoroethylene, are difficult to use for long-term calibration tasks due to their poor resistance to erosion by cosmic particles, ultraviolet light, and atomic oxygen.

[0003] In recent years, the method of attenuating sunlight based on porous plates has begun to be valued as a standard source. However, the preparation of porous plates is very difficult, and their micropores are easily clogged, making them difficult to preserve. Summary of the Invention

[0004] The main purpose of this application is to provide an on-board calibration plate and its preparation method, as well as an on-board calibration device, aiming to solve the technical problem that the micropores of the porous plate used as an on-board calibration plate are easily clogged, resulting in difficulty in preservation. It also has a certain Lambertian property and can resist the erosion of cosmic particles and ultraviolet radiation in the on-board calibration working environment.

[0005] To achieve the above objectives, the present application provides an on-board calibration board, comprising:

[0006] A substrate, and a growth substrate, an attenuation layer, and a protective layer sequentially located on the light incident side of the substrate;

[0007] The attenuation layer includes a doping layer and a blocking layer stacked together, and the doping layer is in contact with the growth substrate;

[0008] The doping layer includes a first material and a second material, and the transmittance between the first material and the second material differs by at least 10%.

[0009] In one embodiment, the first material is a metal, and the second material is a metal, a metal oxide, a metal salt, or an organic compound.

[0010] In one embodiment, the transmittance of the first material is higher than the transmittance of the second material, and the mass ratio between the first material and the second material is 1:(3-1000).

[0011] In one embodiment, the growth substrate includes metal, metal oxide, metal salt or organic compound, and the growth substrate excludes first main group metal elements and liquid metal elements.

[0012] In one embodiment, the barrier layer includes metal, metal oxide, metal salt or organic compound, and the barrier layer excludes first main group metal elements and liquid metal elements.

[0013] In one embodiment, the protective layer includes Au, Pt, Ag2O, Al2O3 or BaSO4.

[0014] In one embodiment, the substrate comprises quartz, glass or ceramic.

[0015] In one embodiment, the thickness of the growth substrate is 0.1-50 nm;

[0016] And / or, the thickness of the doping layer is 50-500 nm;

[0017] And / or, the thickness of the barrier layer is 1-20 nm;

[0018] And / or, the thickness of the protective layer is 1-50 nm.

[0019] In addition, to achieve the above-mentioned purpose, the present application also provides a method for preparing an on-board calibration plate, which is used to prepare the on-board calibration plate as described above, and the method comprises:

[0020] Prepare the substrate;

[0021] preparing a growth substrate on the surface of the substrate;

[0022] preparing a doping layer on the surface of the growth substrate;

[0023] preparing a barrier layer on the surface of the doping layer;

[0024] Repeat the steps of preparing the doping layer and the isolation layer 3-10 times to form an attenuation layer;

[0025] A protective layer is prepared on the surface of the attenuation layer.

[0026] In addition, to achieve the above-mentioned purpose, the present application also provides an on-board calibration device, including the on-board calibration board as described above.

[0027] The present application provides an on-board calibration plate, comprising: a substrate, a growth substrate, an attenuation layer, and a protective layer sequentially located on the light-entering side of the substrate; the attenuation layer comprises a stacked doping layer and a barrier layer, the doping layer being in contact with the growth substrate; the doping layer comprises a first material and a second material, the transmittances of the first and second materials differing by at least 10%. The provision of the growth substrate facilitates the attachment of the attenuation layer, which primarily attenuates sunlight. The transmittances of the first and second materials in the doping layer differ by at least 10%, meaning the transmittance difference is sufficiently large that sunlight can propagate through the material with higher transmittance while being blocked by the material with lower transmittance. The barrier layer is stacked with the doping layer, and light transmitted through the doping layer diffusely transmits through the barrier layer, giving the on-board calibration plate a certain Lambertian characteristic. Sunlight enters through the protective layer for on-board calibration, thereby replacing the attenuation function of a porous plate. Because there are no tiny holes, there is no micropore clogging that would make storage difficult. Furthermore, the protective layer protects the inner attenuation layer, thereby resisting erosion by cosmic particles, ultraviolet radiation, and atomic oxygen. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] In order to more clearly illustrate the technical solutions in the embodiments of the present drawings or related technologies, the drawings required for use in the embodiments or related technical descriptions will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present drawings. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying any creative work.

[0029] Figure 1 This is a cross-sectional view of an onboard calibration plate according to an embodiment of the present application;

[0030] Figure 2 This is a schematic diagram of the scene where sunlight passes through the attenuation layer;

[0031] Figure 3 Schematic diagram of the scene where sunlight passes through the protective layer and enters the calibration plate on the satellite;

[0032] Figure 4 Schematic diagram of transmittance test of Example 1;

[0033] Figure 5 Schematic diagram of Lambertian property of Example 1;

[0034] Figure 6 Schematic diagram of transmittance test in Example 2;

[0035] Figure 7 Schematic diagram of Lambertian property of Example 2;

[0036] Figure 8 Schematic diagram of transmittance test of Example 3;

[0037] Figure 9 Schematic diagram of Lambertian properties of Example 3.

[0038] Description of reference numerals:

[0039] A, direction of light propagation; M1, particles of the first material; M2, particles of the second material;

[0040] 100, onboard calibration plate; 110, base plate; 120, growth substrate;

[0041] 130, attenuation layer; 131, doping layer; 132, isolation layer; 140, protective layer.

[0042] The realization of the objectives, functional features and advantages of this application will be further explained in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION

[0043] It should be understood that the specific embodiments described herein are only used to explain the present application and are not intended to limit the present application.

[0044] " range " disclosed in the present application is limited in the form of lower limit and upper limit, and given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of special range. The scope limited in this way can be to include end value or not include end value, and can be arbitrarily combined, that is, any lower limit can form a range with any upper limit combination. For example, if the scope of 60-120 and 80-110 is listed for specific parameters, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range value 1 and 2 are listed, and if the maximum range value 3,4 and 5 are listed, then the following range can all be expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In this application, unless otherwise specified, the numerical range " ab " represents the abbreviation of any real number combination between a and b, wherein a and b are all real numbers. For example, a numerical range of "0-5" indicates that all real numbers between "0-5" are listed herein, and "0-5" is simply an abbreviation for these numerical combinations. Furthermore, when a parameter is expressed as an integer ≥ 2, this is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0045] To make the above-mentioned objects, features and advantages of the present application more clearly understood, the technical solutions of the present application are further described below with reference to the accompanying drawings and embodiments. However, the present application is not limited to the embodiments listed, but also includes any other known modifications within the scope of the rights claimed in the present application.

[0046] There are two major problems that need to be solved with existing calibration plates: one is that the calibration plates have a weak ability to resist corrosion from cosmic particles, ultraviolet rays, and atomic oxygen; the other is that when a porous plate is used as a calibration plate, it is very difficult to prepare, and the micropores of the porous plate itself are easily clogged due to various reasons and lose their original effect. The present application proposes a method for preparing an on-board calibration plate, which prepares an attenuation plate by coating a layer of stable material (the material can be a stable metal or other stable non-metallic material) on a substrate. Since the particle size of this material is very small, it can produce a significant scattering effect and a certain Lambertian property, so the attenuation plate can be suitable for on-board calibration. The diffuse transmission plate prepared by this method not only has strong resistance to cosmic particles, ultraviolet rays, and atomic oxygen, but also has the advantages of simple preparation and easy storage.

[0047] The embodiment of the present application provides a satellite calibration board, Figure 1 This is a cross-sectional view of an onboard calibration plate according to an embodiment of the present application. Figure 1 As shown, the on-board calibration board 100 includes:

[0048] A substrate 110, and a growth substrate 120, an attenuation layer 130, and a protective layer 140 sequentially located on the light incident side of the substrate 110; the attenuation layer 130 includes a stacked doping layer 131 and a blocking layer 132, and the doping layer 131 is in contact with the growth substrate 120; the doping layer 131 includes a first material and a second material, and the transmittance between the first material and the second material differs by at least 10%.

[0049] Substrate 110 supports functional coatings such as the growth substrate 120 and the attenuation layer 130. Optionally, substrate 110 comprises quartz, glass, or ceramic. The thickness of substrate 110 is controlled within an appropriate range to ensure a certain degree of transparency for sunlight. It is understood that using a relatively common inorganic material for the substrate can also help control costs. The light-incident side of the onboard calibration plate 100 refers to the side on which light is incident during use.

[0050] The growth substrate 120 contacts the substrate 110 and facilitates the subsequent growth of the coating. Optionally, the growth substrate 120 comprises a metal, metal oxide, metal salt, or organic compound, and excludes first-group metal elements and liquid metal elements. The material of the growth substrate 120 and the material of the attenuation layer 130 have a certain affinity to ensure stable adhesion of the attenuation layer 130. First-group metal elements are reactive and easily undergo chemical reactions, resulting in compositional changes. Liquid metal elements, however, do not allow for stable adhesion, and therefore these two elements are excluded. Optionally, the thickness of the growth substrate 120 is 0.1-50 nm, for example, 0.1 nm, 1 nm, 5 nm, 10 nm, 20 nm, 30 nm, 40 nm, or 50 nm. A growth substrate that is too thin will not facilitate the subsequent growth of the coating. A growth substrate that is too thick will consume more material and provide less adhesion to the attenuation layer 130.

[0051] The attenuation layer 130 is used to attenuate sunlight and is a film layer that plays the main attenuation role. The number of layers of the attenuation layer 130 can be 3-10 layers, for example, 3 layers, 4 layers, 5 layers, 6 layers, 7 layers, 8 layers, 9 layers, and 10 layers. The attenuation layer 130 includes a doping layer 131 and a barrier layer 132 that are stacked, and the doping layer 131 is in contact with the growth substrate 120. The doping layer 131 includes a first material and a second material, and the transmittance between the first material and the second material differs by at least 10%, for example, 10%, 15%, 20%, 30%, etc. The transmittance difference between the first material and the second material is less than 10%, and cannot play an attenuation role. After the sunlight reaches the doping layer 131, the light transmitted from the position of the material with higher transmittance is less attenuated. For example, if the transmittance of the first material is higher, the position of the first material particles can be regarded as micropores in the porous plate, which attenuates the sunlight. The isolation layer 132 is combined with the doping layer 131 to play an attenuation role. The stacking of the doping layer 131 and the isolation layer 132 provides multi-level attenuation of sunlight. The isolation layer 132 has excellent diffuse transmission performance.

[0052] Optionally, the transmittance of the first material is higher than that of the second material, and the mass ratio between the first material and the second material is 1:(3-1000), for example, 1:3, 1:5, 1:10, 1:20, 1:50, 1:100, 1:500, 1:1000, etc. The first material with high transmittance occupies a smaller proportion of the doped layer 131. The higher the proportion of the first material, the more micropore-like structures are present in the onboard calibration plate 100. It is understood that the greater the difference in transmittance between the first material and the second material, the smaller the required mass ratio can be. In extreme cases, for example, if the second material is completely opaque, the required mass ratio is 1:3. Theoretically, the maximum mass ratio can reach positive infinity. Optionally, the first material is a metal, and the second material is a metal, metal oxide, metal salt, or organic compound. The transmittance of a metal oxide is generally lower than that of a metal, metal salt, or organic compound. The thickness of the doping layer 131 may be 50-500 nm, for example, 50 nm, 80 nm, 100 nm, 200 nm, 300 nm, 400 nm, or 500 nm.

[0053] Optionally, the barrier layer 132 includes a metal, metal oxide, metal salt, or organic compound, and excludes first main group metal elements and liquid metal elements. The thickness of the barrier layer 132 can be 1-20 nm, for example, 1 nm, 3 nm, 5 nm, 10 nm, 15 nm, 18 nm, or 20 nm. The barrier layer 132 is thinner than the doped layer 131, separating two adjacent doped layers 131 and enhancing diffuse transmission performance.

[0054] The protective layer 140 is used to protect the inner attenuation layer 130 and protect the calibration plate from ultraviolet radiation and cosmic particles in the working environment. The protective layer 140 can be made of a stable metal or metal compound. Optionally, the protective layer includes Au, Pt, Ag2O, Al2O3 or BaSO4. The thickness of the protective layer 140 can be 1-50nm, for example, 1nm, 3nm, 5nm, 10nm, 20nm, 30nm, 40nm, 45nm, 50nm. If the thickness of the protective layer 140 is too thin, the inner attenuation layer 130 is easily exposed. It is understandable that the protective layer 140 can not only be located on the side farthest from the substrate 110, but can also wrap the attenuation layer 130 and the growth substrate 120 and directly contact the substrate 110.

[0055] Figure 2 is a schematic diagram of a scene where sunlight passes through the attenuation layer 130, as shown in FIG. Figure 2 As shown, a local area of ​​the on-board calibration plate 100 is selected. Figure 2The arrow direction A in the figure represents the propagation direction of light. The first material particle M1 is a high-transmittance material, and the second material particle M2 is a low-transmittance material. The attenuation of light after passing through the first material particle M1 is weaker. Therefore, the doped layer 131 can be regarded as a porous layer densely covered with micropores to attenuate light.

[0056] Figure 3 is a schematic diagram of a scene where sunlight is incident from the protective layer 140, as shown in FIG. Figure 3 As shown, in the light propagation direction A, sunlight sequentially passes through the protective layer 140, the attenuation layer 130 consisting of a stacked barrier layer 132 and a doping layer 131, and the growth substrate 120, before exiting the substrate 110. A section of the film structure is selected longitudinally along the light propagation direction A. After reaching the doping layer 131, sunlight is scattered between particles of the low-transmittance material, generating a certain degree of Lambertian behavior. It can also transmit through particles of the high-transmittance material, reaching the next barrier layer 132. After being attenuated by multiple attenuation layers 130, the light exiting the substrate 110 meets the requirements for on-board calibration.

[0057] In this embodiment, an on-board calibration plate comprises: a substrate, a growth substrate, an attenuation layer, and a protective layer sequentially located on the light-entering side of the substrate; the attenuation layer comprises a stacked doping layer and a barrier layer, the doping layer being in contact with the growth substrate; the doping layer comprises a first material and a second material, the transmittances of the first and second materials differing by at least 10%. The provision of the growth substrate facilitates the attachment of the attenuation layer, which primarily attenuates sunlight. The transmittances of the first and second materials in the doping layer differ by at least 10%, meaning the transmittance difference is sufficiently large that sunlight can propagate through the material with higher transmittance while being blocked by the material with lower transmittance. The barrier layer is stacked with the doping layer, and light transmitted through the doping layer diffusely transmits through the barrier layer, giving the on-board calibration plate a certain Lambertian characteristic. Sunlight enters the protective layer for on-board calibration, thereby replacing the attenuation function of a porous plate. Because the protective layer lacks micropores, there is no pore clogging that could hinder storage. Furthermore, the protective layer protects the inner attenuation layer, thereby resisting erosion by cosmic particles, ultraviolet radiation, and atomic oxygen.

[0058] The present application provides a method for preparing an onboard calibration plate. In this embodiment, the method for preparing the onboard calibration plate includes:

[0059] Step S10, preparing a substrate;

[0060] Select a plate made of quartz, glass or ceramic as the substrate and clean it before use.

[0061] Step S20, preparing a growth substrate on the surface of the substrate;

[0062] The growth substrate can be prepared by evaporation, deposition, sputtering or coating. The growth substrate includes metals, metal oxides, metal salts or organic compounds, and the growth substrate excludes first main group metal elements and liquid metal elements. Among them, the metal can be metal elements such as Au, Ag, Cr, Al, Pt, Fe, etc.; the metal oxide can be any of the above metals rapidly oxidized by atomic oxygen or high temperature, or the corresponding metal oxide can be directly used to prepare the growth substrate; the metal salt can be an organic salt or an inorganic salt; the organic compound can be a polymer material such as graphene, polytetrafluoroethylene, etc., and the organic compound can only be prepared by evaporation, deposition or coating. The coating method can be spraying, dipping, or spin coating.

[0063] Step S30, preparing a doping layer on the surface of the growth substrate;

[0064] The doping layer can be prepared by evaporation, deposition, or sputtering. For organic doping, only evaporation and deposition are acceptable; sputtering is not acceptable. The doping layer can be a combination of metals, metals and metal oxides, metals and metal salts, or metals and organic compounds, in a specific ratio.

[0065] Step S40, preparing a barrier layer on the surface of the doping layer;

[0066] The isolation layer can be prepared by evaporation, deposition, sputtering or coating. It includes metals, metal oxides, metal salts or organic compounds, and the isolation layer excludes the first main group metal elements and liquid metal elements. Among them, the metal can be Au, Ag, Cr, Al, Pt, Fe and other metal elements; the metal oxide can be any of the above metals rapidly oxidized by atomic oxygen or high temperature, or the corresponding metal oxide can be directly used to prepare the isolation layer; the metal salt can be an organic salt or an inorganic salt; the organic compound can be a polymer material such as graphene, polytetrafluoroethylene, and the organic compound can only be used by evaporation, deposition or coating. The coating method can be spraying, dipping, or spin coating.

[0067] Step S50, repeating the process of preparing the doping layer and the isolation layer 3-10 times to form an attenuation layer;

[0068] The number of repeated operations determines the number of stacked layers. More layers increase the light attenuation, but further increasing the number of layers increases the manufacturing cost. The operation can be repeated 3, 4, 5, 6, 7, 8, 9, or 10 times to ensure that the attenuation layer has sufficient attenuation and diffuse transmission properties while maintaining a reasonable manufacturing cost.

[0069] Step S60: preparing a protective layer on the surface of the attenuation layer.

[0070] The protective layer may include a metal, a metal oxide, or a metal salt, and may be prepared by evaporation, deposition, or sputtering. The protective layer may include Au, Pt, Ag2O, Al2O3, or BaSO4.

[0071] In this embodiment, an on-board calibration plate is prepared using appropriate process conditions and raw materials, which can replace the micropores of a porous plate. Since the material particles in the doping layer are very small, a significant scattering effect and a certain Lambertian property can be produced. Therefore, the plate with attenuation effect can be suitable for on-board calibration. It not only has strong resistance to cosmic particles, ultraviolet rays, and atomic oxygen, but also has the advantages of simple preparation and easy storage.

[0072] The present application also provides an on-board calibration device, including the on-board calibration board described above. The on-board calibration device of this embodiment has the same technical features and benefits as the on-board calibration board described above, which will not be described in detail here.

[0073] Example 1

[0074] Ordinary quartz glass was used as the substrate, gold (Au) and molybdenum oxide (MoO3) were used to prepare the doping layer, metal chromium (Cr) was used as the growth substrate, and C-60 was used to prepare the isolation layer.

[0075] First, a 1 nm thick Cr layer was evaporated on a clean quartz glass sheet as a growth substrate.

[0076] Then gold (Au) and molybdenum trioxide (MoO3) are mixed and evaporated in a ratio of 1:14 to deposit a 20nm thick mixed coating of gold (Au) and molybdenum trioxide (MoO3). At this time, the transmittance of gold is higher than that of molybdenum trioxide, thus producing a porous sheet with a thin layer of gold as the "small holes".

[0077] A layer of C-60 is deposited on the mixed coating as a barrier layer with a thickness of 1 nm.

[0078] The gold trioxide mixed coating and the carbon barrier layer are evaporated again, and repeated twice to form a multilayer structure.

[0079] Finally, a 3nm gold layer is evaporated on the isolation layer as a protective layer.

[0080] Figure 4 This is a schematic diagram of transmittance testing in Example 1. Figure 4 The horizontal axis is the angle, the vertical axis is the transmittance, and the angle of the horizontal axis is the angle between the light detector and the calibration plate on the satellite. Figure 5 is a Lambertian diagram of Example 1, Figure 5The horizontal coordinate is the zenith angle, and the vertical coordinate is the relative BTDF (Bidirectional Transmittance Distribution Function) value. Figure 4 and Figure 5 It can be seen that the on-board calibration plate prepared in Example 1 can meet the requirements of on-board calibration.

[0081] Example 2

[0082] A frosted glass sheet was used as a substrate, and two metals, gold (Au) and silver (Ag), were used to prepare the doping layer. Indium tin oxide (ITO) was used as a growth substrate, and silver (Ag) was used to prepare the isolation layer.

[0083] First, a 30 nm thick layer of indium tin oxide (ITO) was sputtered on a clean frosted glass sheet as a growth substrate.

[0084] Then, gold (Au) and silver (Ag) are mixed and evaporated in a ratio of 1:9 to form a 10nm thick mixed layer of gold (Au) and silver (Ag). The quartz sheet is placed on a high-temperature hot plate for rapid oxidation. At this time, the silver in the mixed layer will be oxidized to produce Ag2O with low transmittance. At this time, the transmittance of gold is higher than that of Ag2O, thus producing a porous sheet with a thin layer of gold as the "small holes".

[0085] A layer of metallic silver with a thickness of 1 nm is evaporated on the mixed coating as a barrier layer.

[0086] The gold-silver mixed plating layer and the silver barrier layer are evaporated again, and this is repeated 5 times to form a multi-layer structure.

[0087] Finally, a 3nm gold layer is evaporated on the isolation layer as a protective layer.

[0088] Figure 6 This is a schematic diagram of transmittance testing in Example 2. Figure 6 The horizontal axis is the angle, the vertical axis is the transmittance, and the angle of the horizontal axis is the angle between the light detector and the calibration plate on the satellite. Figure 7 is a Lambertian diagram of Example 2, Figure 7 The horizontal coordinate is the zenith angle, and the vertical coordinate is the relative BTDF value. Figure 6 and Figure 7 It can be seen that the on-board calibration plate prepared in Example 2 can meet the requirements of on-board calibration.

[0089] Example 3

[0090] A metal oxide ceramic sheet is used as the substrate, and two materials, silver (Ag) and octahydroxyquinoline aluminum (Alq3), are used to prepare the doping layer. Graphene is used as the growth substrate, and aluminum (Al) is used to prepare the isolation layer.

[0091] First, a 1nm thick layer of graphene is deposited on a clean metal oxide ceramic wafer as a growth substrate.

[0092] Then silver (Ag) and octahydroxyquinoline aluminum (Alq3) are mixed and evaporated in a ratio of 1:19 to form a 20nm thick silver (Ag)-octahydroxyquinoline aluminum (Alq3) mixed coating. At this time, the transmittance of silver is higher than that of octahydroxyquinoline aluminum, thereby producing a porous sheet with a thin layer of gold as the "small holes".

[0093] A layer of metallic aluminum is evaporated on the mixed coating, and then rapidly oxidized using the same method to obtain a layer of aluminum oxide with a thickness of 1 nm as a barrier layer.

[0094] A silver (Ag)-octahydroxyquinoline aluminum (Alq3) mixed coating and an aluminum oxide barrier layer were evaporated again, and the process was repeated 10 times to form a multilayer structure.

[0095] Finally, a 30nm thick BaSO4 layer was spin-coated on the isolation layer as a protective layer.

[0096] Figure 8 This is a schematic diagram of transmittance testing in Example 3. Figure 8 The horizontal axis is the angle, the vertical axis is the transmittance, and the angle of the horizontal axis is the angle between the light detector and the calibration plate on the satellite. Figure 9 is a Lambertian diagram of Example 3, Figure 9 The horizontal coordinate is the zenith angle, and the vertical coordinate is the relative BTDF value. Figure 8 and Figure 9 It can be seen that the on-board calibration plate prepared in Example 3 can meet the requirements of on-board calibration.

[0097] The serial numbers of the above embodiments of the present application are for description only and do not represent the advantages or disadvantages of the embodiments.

[0098] The above are only preferred embodiments of the present application and do not limit the patent scope of the present application. Any equivalent structure or equivalent process transformation made using the contents of the present application specification and drawings, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present application.

Claims

1. A satellite calibration board, characterized in that: The on-board calibration board comprises: A substrate, and a growth substrate, an attenuation layer and a protective layer sequentially located on the light incident side of the substrate; The attenuation layer comprises a doping layer and an isolation layer which are stacked, the doping layer is in contact with the growth substrate, and the number of layers of the attenuation layer is 3-10; The doping layer includes a first material and a second material, the transmittance between the first material and the second material differs by at least 10%, the first material is a metal, and the second material is a metal, a metal oxide, a metal salt or an organic compound.

2. The on-board calibration board according to claim 1, characterized in that: The transmittance of the first material is higher than the transmittance of the second material, and the mass ratio between the first material and the second material is 1:(3-1000).

3. The on-board calibration board according to claim 1, characterized in that: The growth substrate includes metal, metal oxide, metal salt or organic compound, and the growth substrate excludes first main group metal elements and liquid metal elements.

4. The on-board calibration board according to claim 1, characterized in that: The barrier layer includes metal, metal oxide, metal salt or organic compound, and the barrier layer excludes first main group metal elements and liquid metal elements.

5. The on-board calibration board according to claim 1, characterized in that: The protective layer includes Au, Pt, Ag2O, Al2O3 or BaSO4.

6. The on-board calibration board according to claim 1, characterized in that: The substrate includes quartz, glass or ceramic.

7. The on-board calibration board according to any one of claims 1 to 6, characterized in that: The thickness of the growth substrate is 0.1-50 nm; And / or, the thickness of the doping layer is 50-500 nm; And / or, the thickness of the barrier layer is 1-20 nm; And / or, the thickness of the protective layer is 1-50 nm.

8. A method for preparing a satellite calibration plate, characterized in that: For preparing a satellite calibration plate according to any one of claims 1 to 7, the method comprising: Prepare substrate; preparing a growth substrate on the surface of the substrate; preparing a doping layer on the surface of the growth substrate; preparing a barrier layer on the surface of the doping layer; Repeat the steps of preparing the doping layer and the isolation layer for 3 to 10 times to form an attenuation layer; A protective layer is prepared on the surface of the attenuation layer.

9. An on-board calibration device, characterized in that: The invention comprises the on-board calibration board as claimed in any one of claims 1 to 7.

Citation Information

Patent Citations

  • Phase shift blank mask and photomask for use in flat panel displays

    CN113009774A

  • On-satellite calibration device, calibration system and calibration method for remote sensor

    CN113219502A

  • High-transmittance and low-resistance composite ITO film

    CN113223753A

  • Systems and methods of sensor calibration using switchable in-path optical diffuser

    US20230034351A1