A method for determining chloride ion content in silver-coated copper powder
By using a mixed solution of ethanol, glycerol, and lipid solvents to promote the precipitation of copper ammonia complexes, and combining it with spectrophotometry, the problem of complex and expensive equipment for chloride ion determination of silver-coated copper powder in the prior art has been solved, achieving highly accurate and convenient chloride ion determination.
Patent Information
- Application Number
- CN202411122392.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-08-15
AI Technical Summary
Existing technologies for determining chloride ion content in silver-coated copper powder suffer from problems such as the large number of reagents, cumbersome operation, poor result repeatability, and expensive equipment, making them difficult to widely apply in general enterprises.
Using a mixed solution of ethanol, glycerol, and lipid solvents reduces solution polarity, increases viscosity, and promotes the precipitation of copper ammonia complexes. Combined with spectrophotometric determination of chloride ion content, this simplifies the operation and improves accuracy.
It improves the accuracy and repeatability of chloride ion determination, simplifies the operation process, reduces equipment costs, and is suitable for widespread application in general enterprises.
Smart Images

Figure CN118641495B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of chemical analysis, and particularly relates to a method for determining the chloride ion content in silver-coated copper powder. Background Art
[0002] As a highly conductive filler with excellent performance, silver-coated copper powder is widely used in electronics, electromechanics, communications, printing, aerospace, weapons and other fields. However, if there are excessive chloride ions in the silver-coated copper powder, it will penetrate and destroy the passivation film covering the metal surface. This destructive effect will make the metal surface more vulnerable to the attack of the corrosive environment, thereby significantly accelerating the corrosion rate of the metal, leading to a decrease in material performance and potential structural problems. In order to ensure the stability and durability of the silver-coated copper powder, it is particularly important to test the chloride ion content of the silver-coated copper powder.
[0003] Common chloride ion content determination techniques include silver titration, mercury titration, ion chromatography, ion selective electrode method, spectrophotometry, and potentiometric titration. However, the mercury titration method requires many types of reagents in large quantities, the process is cumbersome, and the results have poor repeatability. The equipment for ion chromatography and potentiometric titration is expensive and difficult to be widely used in general enterprises, which limits their role in guiding production and meeting testing requirements to a certain extent.
[0004] Spectrophotometry has shown significant advantages in determining chloride ion content. Its instruments and equipment are cheap, easy to operate, and have high sensitivity. Summary of the invention
[0005] The invention provides a method for determining the chloride ion content in silver-coated copper powder. In the precipitation process of copper ammonia complex, a mixed solution of ethanol, glycerol and lipid solvent is used to reduce the polarity of the solution and increase the viscosity of the solution, thereby promoting the precipitation of copper ammonia complex precipitation and further improving the accuracy of chloride ion determination.
[0006] The spectrophotometric method is used to determine the chloride ion content in silver-coated copper powder. The operation steps are simple, and the results are accurate, reliable and highly reproducible.
[0007] The technical solution of the present invention is as follows:
[0008] A method for determining the chloride ion content in silver-coated copper powder comprises the following steps:
[0009] Step 1: Take 0.5 g of silver-coated copper powder and put it in a beaker. Add concentrated nitric acid and digest it on a hot plate until the solution is 10 mL to obtain a light blue solution A, which contains silver nitrate solution and copper nitrate solution.
[0010] As a preferred embodiment, the temperature of the heating plate is 200°C.
[0011] As a preferred embodiment, the silver content of the silver-coated copper powder is one or a combination of 8%, 14%, 17%, 20% and 24%.
[0012] As a preferred embodiment, 30 to 45 mL of concentrated nitric acid is added to every 0.5 g of silver-coated copper powder.
[0013] Step 2: Add ammonia water dropwise to solution A until it turns dark blue. Stop adding when the color no longer deepens. Add 250 mL of mixed solvent. Copper ammonia complex crystals gradually precipitate. Let stand for 1 h and remove the precipitate by suction to obtain solution B.
[0014] As a preferred embodiment, the mixed solvent is a mixed solution of ethanol, glycerol and a lipid solvent, the volume ratio of ethanol, glycerol and the lipid solvent is 7:2:1, and the lipid solvent is one of methyl formate, ethyl formate, methyl acetate or ethyl acetate.
[0015] Ethanol occupies a dominant position in the mixed solvent. The use of mixed solvents reduces the polarity of the solution and increases the viscosity of the solution, thereby promoting the precipitation of copper ammonia complex precipitation. At the same time, the presence of propylene glycol can play a role in the determination of chloride ion content, enhance the stability of the reaction system, reduce interference, etc.
[0016] Step 3: Heat solution B on a hot plate until crystals are precipitated to remove most of the ethanol and avoid the influence of a large amount of ethanol on the experimental determination. Pipette 5 mL of concentrated nitric acid solution and slowly add it to solution B along the inner wall of the beaker. Then add 5 mL of water to rinse the inner wall. While stirring continuously, add 400 g / L ascorbic acid solution drop by drop until the silver is completely precipitated. Continue stirring for 10 min, remove the precipitate by suction filtration to obtain solution C, and fix the volume of solution C to 50 mL.
[0017] As a preferred embodiment, the silver precipitate is continuously washed with 10 g / L ascorbic acid to reduce errors.
[0018] Step 4: Determine the chloride ion content in solution C using spectrophotometry.
[0019] As a preferred embodiment, the spectrophotometry is ultraviolet spectrophotometry.
[0020] Compared with the prior art, the present invention has the following beneficial effects:
[0021] 1. Before determining the chloride ion content by spectrophotometry, remove the metal ions in the solution to be tested to improve the accuracy of the chloride ion determination results.
[0022] 2. In the process of removing metal ions in the solution to be tested, a mixed solvent of ethanol, glycerol and lipid solvent is used, and the polarity of the copper ammine complex in the mixed solvent is lower than that in water, so as to promote the precipitation of copper ammine complex crystals.
[0023] 3. When propylene glycol is added to the ethanol solution, the presence of non-polar bonds in propylene glycol reduces the polarity of the mixed solvent. In addition, the larger molecules in propylene glycol and the relatively smaller molecules in ethanol form a mixed system, which increases the viscosity and stability of the mixed solvent. When a large amount of copper ammonia complex is precipitated, the concentration of the mixed solution can be maintained during a long precipitation process.
[0024] 4. Ethanol and glycerol are both flammable and volatile substances. Adding low-volatile lipid solvents to ethanol and glycerol solvents can reduce the movement speed of molecules in the mixed solvent, thereby maintaining the concentration of the solution; in a weakly alkaline environment, some lipids can react with water to form alcohols, further enhancing the stability of the mixed solvent.
[0025] 5. The present invention adds glycerol solvent and lipid solvent to the ethanol solution, which reduces the polarity of the ethanol solution and increases the viscosity of the solution. The mixed solvent is added to the solution containing the copper ammonia complex, which can further promote the precipitation of the copper ammonia complex and further improve the accuracy of chloride ion determination.
[0026] 6. The present invention provides a method for determining the chloride ion content in silver-coated copper powder. The method combines the advantages of spectrophotometry, which not only ensures the accuracy of the determination results, but also greatly improves the detection speed, providing strong support for the accurate determination of the chloride ion content in silver-coated copper powder. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 This is the working curve for chloride ion concentrations in the range of 0 ~ 700 μg / L.
[0028] Figure 2 This is the working curve for chloride ion concentrations in the range of 600 ~ 2200 μg / L.
[0029] Figure 3 This is the result of determination of chloride ion content in silver-coated copper powder. DETAILED DESCRIPTION
[0030] The preferred embodiments of the present invention are described in detail below in conjunction with the accompanying drawings so that the advantages and features of the present invention can be more easily understood by those skilled in the art, thereby making a clearer and more definite definition of the protection scope of the present invention.
[0031] Main reagents:
[0032] Nitric acid solution (1+1); ammonium ferric sulfate indicator; ammonia water; ethanol; glycerol; ester solvents; hydrochloric acid; ascorbic acid solution (400 g / L): weigh 400 g ascorbic acid, dissolve in water, and dilute to 1000 mL; ascorbic acid solution (10 g / L): weigh 10 g ascorbic acid, dissolve in water, and dilute to 1000 mL; chlorine standard solution 5 μg / mL: accurately weigh 0.8240 g of dry sodium chloride solid (superior purity, calcined at 500-600℃ and cooled), fully dissolve it in pure water and dilute to 1 L volumetric flask, shake well, accurately transfer 5 mL to a 500 mL volumetric flask and dilute to prepare a 5 μg / mL chlorine standard solution. Chlorine standard solution 2.5 μg / mL: accurately transfer 2.5 mL, dilute the above solution to volume in a 500 mL volumetric flask to prepare a 2.5 μg / mL chlorine standard solution; AgNO3 standard solution 0.1 mol / L: accurately weigh 4.2467 g of dry AgNO3 solid, fully dissolve it in pure water and dilute it to volume in a 250 mL volumetric flask to prepare a 0.1 mol / L AgNO3 standard solution, and store it in a brown bottle for later use.
[0033] Experimental process:
[0034] Take 0.5 g of silver-coated copper powder and put it in a 500 mL beaker. Then add 35 mL of concentrated nitric acid. Heat the beaker on a 200 °C hot plate. Stop heating when the solution is 10 mL. A light blue mixed solution A is obtained.
[0035] 200 mL of ethanol, 35 mL of propylene glycol and 15 mL of methyl formate were added into a beaker in sequence and mixed evenly to obtain a mixed solvent B;
[0036] Add 25-28% ammonia water dropwise to the mixed solution A until the solution turns dark blue. Stop adding the solution when the color stops deepening. Then add 250 mL of mixed solvent B. Using the difference in solubility, precipitate the copper-ammine complex in the mixed solvent. After standing for 1 h, remove the precipitate by suction, retain the filtrate, and continue to heat the filtrate on a 200 °C hot plate until crystals precipitate.
[0037] Pipette 5 mL of nitric acid solution and add it to the above solution containing trace crystals, slowly rinse along the inner wall of the beaker, then add 5 mL of water to rinse the inner wall, and add 400 g / L ascorbic acid solution drop by drop while stirring continuously until the silver element is completely precipitated. Continue stirring for 10 min, wash the filter residue continuously with 10 g / L ascorbic acid solution, filter to remove the precipitate, and make the filtrate dilute to 50 mL.
[0038] Drawing of working curve:
[0039] In order to make the calculation result more accurate, the segmented curve method can be used, that is, the chloride ion concentration range of 0 ~ 700 μg / L is one curve, and the range of 600 ~ 2200 μg / L is another curve. The specific operation is as follows:
[0040] (1) Drawing of working curve for chloride ion concentration in the range of 0 ~ 700 μg / L:
[0041] Accurately pipette 0, 0.5, 1, 2, 3, 4, 5, 6, 7 mL of 2.5 μg / mL chlorine standard solution into a 25 mL colorimetric tube, dilute to the scale, add 1 mL (1+1) HNO3 solution, 2 mL, 0.1 mol / L AgNO3 solution, shake well, let stand for 20 min, shake well again before measurement, use blank water as a reference, measure the absorbance at a wavelength of 410 nm with a 3 cm colorimetric dish, and draw a standard curve.
[0042] (2) Drawing of working curve for chloride ion concentration in the range of 600 ~ 2200 μg / L:
[0043] Accurately transfer 0, 3, 4, 5, 6, 7, 8, 9, 10, 11 mL of 5 μg / mL chlorine standard solution into a 25 mL colorimetric tube, dilute to the scale, add 1 mL (1+1) HNO3 solution, 2 mL of 0.1 mol / L AgNO3 solution, shake well, let stand for 20 min, shake well again before measurement, use blank water as a reference, measure the absorbance at a wavelength of 410 nm with a 3 cm colorimetric dish, and draw a standard curve.
[0044] Sample test solution determination:
[0045] Accurately transfer 25 mL of the test solution into a 25 mL (or 50 mL) colorimetric tube, add 1 mL (1+1) HNO3 solution and 2 mL 0.1 mol / L AgNO3 standard solution, shake well, and after 20 min, use a blank solution (pure water, nitric acid, silver nitrate) as a reference, and use a 3 cm cuvette to measure the absorbance at a wavelength of 410 nm. Shake well before measurement.
[0046] By measuring the maximum absorbance of the test solution and comparing it with the standard curve, the concentration of chloride ions in the test solution can be obtained, and then the chloride ion content in the powder can be obtained. The chloride ion content in the silver-coated copper sample can be calculated using the chloride ion standard curve. Example 1
[0047] Two silver-coated copper powders with different chloride ion contents were selected, and the silver content of the silver-coated copper powder was 8%. The chloride ions of the two samples were measured multiple times and the average values were taken. They were numbered ASC-1 and ASC-2 respectively. Example 2
[0048] Two silver-coated copper powders with different chloride ion contents were selected, and the silver content of the silver-coated copper powder was 14%. The chloride ions of the two samples were measured multiple times and the average values were taken. They were numbered ASC-3 and ASC-4 respectively. Example 3
[0049] Two silver-coated copper powders with different chloride ion contents were selected, and the silver content of the silver-coated copper powder was 17%. The chloride ions of the two samples were measured multiple times and the average values were taken. They were numbered ASC-5 and ASC-6 respectively. Example 4
[0050] Two silver-coated copper powders with different chloride ion contents were selected, and the silver content of the silver-coated copper powder was 20%. The chloride ions of the two samples were measured multiple times and the average values were taken. They were numbered ASC-7 and ASC-8 respectively. Example 5
[0051] Two silver-coated copper powders with different chloride ion contents were selected, and the silver content of the silver-coated copper powder was 24%. The chloride ions of the two samples were measured multiple times and the average values were taken. They were numbered ASC-9 and AC-10 respectively.
[0052] Comparative Example
[0053] Take 0.5 g of silver-coated copper powder and put it in a 500 mL beaker. Then add 35 mL of concentrated nitric acid. Heat the beaker on a 200 °C hot plate. Stop heating when the solution is 10 mL. A light blue mixed solution A is obtained.
[0054] Add 25-28% ammonia water dropwise to the mixed solution A until the solution turns dark blue. Stop adding the solution when the color stops deepening. Then add 250 mL of ethanol solution. Using the difference in solubility, precipitate the copper-ammine complex in the mixed solvent. After standing for 1 h, remove the precipitate by suction, retain the filtrate, and continue to heat the filtrate on a 200 °C hot plate until crystals precipitate.
[0055] Pipette 5 mL of nitric acid solution and add it to the above solution containing trace crystals, slowly rinse along the inner wall of the beaker, then add 5 mL of water to rinse the inner wall, and add 400 g / L ascorbic acid solution drop by drop while stirring continuously until the silver element is completely precipitated. Continue stirring for 10 min, wash the filter residue continuously with 10 g / L ascorbic acid solution, filter to remove the precipitate, and make the filtrate dilute to 50 mL.
[0056] Figure 3The present invention is a result of determining the chloride ion content in the silver-coated copper powder in Examples 1 to 5 and a comparative example. The result indicates that in determining the chloride ion content in the silver-coated copper powder, the removal of copper ions by a mixed solvent can effectively improve the accuracy of determining the chloride ion content by spectrophotometry. Moreover, the chloride ion content in the silver-coated copper powder with different silver contents is determined, and the silver-coated copper powder with different chloride ion contents under the same silver content is also determined, providing a method for effectively determining the chloride ion content in the silver-coated copper powder, which not only helps to ensure the safety and effectiveness of the silver-coated copper powder, but also provides strong technical support for research in the field of nanomaterials.
Claims
1. A method for determining the chloride ion content in silver-coated copper powder, characterized in that: include: Step 1: Take 0.5 g of silver-coated copper powder and put it in a beaker. Add nitric acid and digest it on a hot plate until the solution is 10 mL to obtain a light blue solution A. Step 2: Add ammonia water to solution A until it turns dark blue. When the color no longer deepens, stop adding and add 250 mL of mixed solvent. Let stand for 1 h and remove the copper ammonia complex precipitate by suction to obtain solution B. Step 3: Heat solution B on a hot plate until crystals are precipitated. After crystals are precipitated, stop heating. After cooling, take 5 mL of nitric acid solution and slowly add it to solution B along the inner wall of the beaker. Then add 5 mL of water to rinse the inner wall. While stirring continuously, add 400 g / L ascorbic acid solution drop by drop until the silver is completely precipitated. Continue stirring for 10 min, remove the precipitate by suction, obtain solution C, and fix the volume of solution C to 50 mL. Step 4: Determine the chloride ion content in solution C by spectrophotometry; The mixed solvent is a mixed solution of ethanol, glycerol and lipids.
2. The method for determining the chloride ion content in the silver-coated copper powder according to claim 1, wherein: The silver content of the silver-coated copper powder in the step 1 is one of 8%, 14%, 17%, 20% and 24%.
3. The method for determining the chloride ion content in the silver-coated copper powder according to claim 1, wherein: In the step 1, 30 to 45 mL of concentrated nitric acid is added for every 0.5 g of silver-coated copper powder.
4. The method for determining the chloride ion content in the silver-coated copper powder according to claim 1, wherein: The lipid is a combination of one or more of methyl formate, ethyl formate, methyl acetate and ethyl acetate.
5. The method for determining the chloride ion content in the silver-coated copper powder according to claim 1, characterized in that: The volume ratio of the ethanol, glycerol and lipid is 7-8:1-2:0.5-1.
6. The method for determining the chloride ion content in the silver-coated copper powder according to claim 1, characterized in that: During the filtration process of step 3, the filter residue is continuously washed with 10 g / L ascorbic acid.