Functionally gradient material additive manufacturing method and device for shock absorber

By adjusting the wire feeding speed and stacking direction of Ni wire and Ti wire, TIG welding technology is used to form a nickel-titanium alloy gradient structure, which solves the problems of high manufacturing cost of shock absorber materials and difficult alloy ratio, and achieves low-cost, high-performance Made of nickel-titanium alloy gradient functional materials, the elasticity and compression resistance of the material are improved.

CN118650247BActive Publication Date: 2024-10-29LANZHOU UNIVERSITY OF TECHNOLOGY
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411132314.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-10-29
Estimated Expiration
2044-08-19

AI Technical Summary

Technical Problem

The manufacturing cost of existing gradient functional materials for shock absorbers is high and the alloy ratio is difficult when manufacturing nickel-titanium alloys, which limits their application in low-cost and high-performance fields.

Method used

By adjusting the wire feeding speed and stacking direction of Ni wire and Ti wire, using TIG welding technology to form a gradient structure of NiTi alloy, controlling the Ni/Ti element content, and realizing the manufacturing of gradient functional materials of NiTi alloy.

Benefits of technology

It reduces the manufacturing cost of gradient functional materials for shock absorbers, improves the elastic recovery performance and compression resistance of nickel-titanium alloys, overcomes the problem of difficult alloy proportioning, and achieves low-cost and high-performance material manufacturing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118650247B_ABST
    Figure CN118650247B_ABST
Patent Text Reader

Abstract

The invention relates to the field of additive manufacturing technology, and is a method and device for additive manufacturing of gradient functional materials for shock absorbers, the former of which comprises the following steps: adjusting test equipment; starting the test, setting the wire feeding speeds of Ni wire and Ti wire, setting the stacking speed, and performing the first layer of additive manufacturing, and after the first layer of additive manufacturing is completed, adjusting the tungsten pole tip height and the stacking direction, and performing the second layer of additive manufacturing; the invention uses different Ti / Ni alloy component ratios and adopts a stacking additive method to complete multi-layer stacking additive manufacturing and develop Ti / Ni alloy gradient functional materials; thereby, the additive manufacturing technology is used to overcome the problem of difficult alloy ratio in nickel-titanium alloy, and nickel-titanium alloy has the characteristics of high elasticity, memory effect, and easy availability and low cost of materials, which reduces the manufacturing cost of the gradient functional material additive of the shock absorber and improves the practicality of the nickel-titanium alloy gradient functional material additive of the shock absorber.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of additive manufacturing technology, and in particular to a method and device for additive manufacturing of gradient functional materials for shock absorbers. Background Art

[0002] As a key shock absorbing device, shock absorbers are widely used in automobiles, bridges, buildings, and medical equipment. Shock absorbers are designed to eliminate or suppress impact pulses and dissipate kinetic energy. Their function is to absorb or dissipate energy, reduce the impact of vibration, thereby improving the stability of the structure and increasing durability. When the structure is subjected to external impact, the shock absorber will be compressed immediately. The compressed shock absorber will rebound back to its normal position, causing part of the structure to be lifted. This bouncing process is repeated continuously, and the amplitude gradually decreases each time. If the bouncing is not controlled, it will not only lead to structural instability, but also make its operation difficult. Therefore, shock absorbers have high requirements on the elastic recovery degree of materials. Among them, the cylinder and piston rod, as key components, are mostly made of high-strength steel to provide good structural strength and durability.

[0003] In order to meet the needs of structural parts, researchers use alloy steel and composite materials (such as carbon fiber or glass fiber) as shock-absorbing materials, taking advantage of their high strength, fatigue resistance and quality to replace traditional manganese steel materials. However, due to the limitations of processing costs and uses, they are currently limited to high-end applications. In order to achieve the manufacturing of low-cost and high-performance shock-absorbing materials, this paper proposes a method for additive manufacturing of gradient functional materials for shock absorbers. The flexibility of the additive manufacturing process path and the diversity of manufacturing methods make it highly adaptable in the manufacture of gradient functional parts. Summary of the invention

[0004] The present invention provides a method and device for additive manufacturing of gradient functional materials for shock absorbers, which overcomes the shortcomings of the above-mentioned prior art and can effectively solve the problems of high manufacturing cost of gradient functional materials for existing shock absorbers and difficult alloy ratio when using nickel-titanium alloy for manufacturing.

[0005] To solve the above problems, one of the technical solutions described in the present invention is implemented in the following way: A method for additive manufacturing of a gradient functional material for a shock absorber comprises the following steps:

[0006] S101, adjust the test equipment;

[0007] S102, start the test, set the wire feeding speed of Ni wire and Ti wire, set the stacking speed, perform the first layer of additive manufacturing, after the first layer of additive manufacturing is completed, adjust the tungsten electrode tip height and stacking direction, and perform the second layer of additive manufacturing;

[0008] S103, repeating the above step S102 to complete the additive manufacturing of multi-layer stacking;

[0009] S104, close the test equipment, remove the additive manufacturing sample, and end the test.

[0010] The above adjustment test equipment includes the following steps:

[0011] Turn on the TIG welding power supply, adjust the process parameters, open the argon gas bottle, and set the flow rate of the protective gas during additive manufacturing;

[0012] Turn on two wire feeders, adjust the wire feeding speed, and adjust the position of the double wires so that the double wires are symmetrically distributed in the XZ direction;

[0013] Turn on the AC power supply and set the AC power parameters for the welding wire;

[0014] Adjust the position of the tungsten electrode tip, move the TIG welding gun to the initial position, grind the titanium alloy substrate, and fix the position of the titanium alloy substrate in preparation for experimental needs.

[0015] The wire feeding speed and stacking speed are set as above to perform the first layer of additive manufacturing. After the first layer of additive manufacturing is completed, the tungsten electrode tip height and stacking direction are adjusted to perform the second layer of additive manufacturing; including:

[0016] Adjust the height of the tungsten electrode tip, and keep the distance between the tungsten electrode tip and the stacking layer at 5mm;

[0017] Adjust the wire feeding speed of the Ni / Ti heterogeneous twin wires to control the Ni / Ti content of the additive manufacturing layer to form a NiTi alloy gradient part;

[0018] During stacking, different wire feeding speed ratios are used on the XY plane, that is, the wire feeding speed ratios of the previous and next passes in each layer are different, and two wire feeding speed ratios are used in each layer to control the content of Ni and Ti elements;

[0019] When adding the first layer, the Ni / Ti wire feeding speed ratio used in the first pass is 1:1.5, and the Ni / Ti wire feeding speed ratio used in the second pass is 1:2. By analogy, the wire feeding speed ratio of the odd-numbered passes in the first layer is 1:1.5, and the wire feeding speed ratio of the even-numbered passes is 1:2.

[0020] When adding the second layer, the Ni / Ti wire feeding speed ratio used in the first pass is 1:2, and the Ni / Ti wire feeding speed ratio used in the second pass is 1:1.5. By analogy, the wire feeding speed ratio of the odd-numbered passes in the second layer is 1:2, and the wire feeding speed ratio of the even-numbered passes is 1:1.5.

[0021] Repeat the first layer additive method to complete the additive manufacturing of odd-numbered layers of the multi-layer stacking, repeat the second layer additive method to complete the additive manufacturing of even-numbered layers of the multi-layer stacking, and the stacking direction of the odd-numbered layers is the Y direction, and the stacking direction of the even-numbered layers is the X direction. The stacking direction of the next layer is adjusted by 90° based on the stacking direction of the previous layer, thereby completing the additive manufacturing of the multi-layer stacking.

[0022] The above-mentioned additive manufacturing of multi-layer stacking also includes, after the additive manufacturing is completed, cutting it into columns with a diameter of 25 mm and a height of 40 mm by wire cutting.

[0023] The second technical solution of the present invention is achieved by the following method: a gradient functional material additive manufacturing device for a shock absorber, implementing a gradient functional material additive manufacturing method for a shock absorber, including: a TIG welding gun, a TIG welding power source, an argon gas bottle, a wire feeder 1, a wire feeder 2, a Ni wire, a Ti wire, an AC power source, a titanium alloy substrate, and an additive manufacturing layer;

[0024] The argon gas cylinder is used to provide shielding gas for additive manufacturing; the TIG welding power source is used to power the TIG welding gun;

[0025] The TIG welding gun is used to hold the tungsten electrode to achieve welding; and can deliver and spray the shielding gas provided by the argon cylinder;

[0026] Wire feeder - used to provide Ti wire and adjust wire feeding speed;

[0027] Wire feeder 2 is used to provide Ni wire and adjust the wire feeding speed;

[0028] The AC power supply is used to provide AC power to the Ni wire and the Ti wire;

[0029] The titanium alloy substrate is used to provide support for the additive manufacturing layer, facilitating the stacking of the additive manufacturing layer.

[0030] The present invention achieves different Ti / Ni ratios by adjusting the wire feeding speeds of Ni wire and Ti wire, thereby facilitating the in-situ formation of Ti / Ni in the additive manufacturing metallurgical process, and completing multi-layer stacking additive manufacturing through different Ti / Ni alloy component ratios and adopting a stacking additive method to develop Ti / Ni alloy gradient functional materials. Thus, the additive manufacturing technology is utilized to overcome the problem of difficult alloy ratios in nickel-titanium alloys, and nickel-titanium alloys have the characteristics of high elasticity, memory effect, and easy availability of materials at low cost, thereby reducing the manufacturing cost of the gradient functional material additive of the shock absorber and improving the practicability of the nickel-titanium alloy gradient functional material additive of the shock absorber. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] The specific implementation modes of the present invention are further described in detail below in conjunction with the accompanying drawings.

[0032] Figure 1 This is a flow chart of the method of Example 1 of the present invention.

[0033] Figure 2 Schematic diagram of the nickel-titanium alloy gradient component in Example 1 of the present invention.

[0034] Figure 3 This is a compression performance diagram of the gradient functional material in Example 1 of the present invention.

[0035] Figure 4 It is a schematic diagram of the structure in Example 2 of the present invention and a schematic diagram of double wire crossing.

[0036] In the figure: 1-TIG welding gun, 2-TIG welding power source, 3-argon gas cylinder, 4-wire feeder 1, 5-wire feeder 2, 6-Ni wire, 7-Ti wire, 8-AC power source, 9-titanium alloy substrate, 10-additive manufacturing layer. DETAILED DESCRIPTION

[0037] The present invention is not limited by the following embodiments, and specific implementation methods can be determined based on the technical solution of the present invention and actual conditions.

[0038] Example 1: Figure 1 As shown, the embodiment of the present invention discloses a method for additive manufacturing of a functional gradient material for a shock absorber, comprising the following steps:

[0039] S101, adjust the test equipment;

[0040] S102, start the test, set the wire feeding speed of Ni wire 6 and Ti wire 7, set the stacking speed, and perform the first layer of additive manufacturing. After the first layer of additive manufacturing is completed, adjust the tungsten electrode tip height and stacking direction, and perform the second layer of additive manufacturing;

[0041] S103, repeating the above step S102 to complete the additive manufacturing of multi-layer stacking;

[0042] S104, close the test equipment, remove the additive manufacturing sample, and end the test.

[0043] Wherein, in step S101, adjusting the test equipment includes the following steps:

[0044] Turn on the TIG welding power source 2, adjust the process parameters, open the argon gas bottle 3, and set the flow rate of the protective gas during additive manufacturing;

[0045] Turn on the two wire feeders, adjust the wire feeding speed, and adjust the position of the double wires so that the double wires are symmetrically distributed in the XZ direction, such as Figure 4 As shown in the partial enlarged figure;

[0046] Turn on the AC power supply 8 and set the AC power parameters for the welding wire;

[0047] The position of the tungsten electrode tip is adjusted, the TIG welding gun 1 is moved to the initial position, the titanium alloy substrate 9 is polished, and the position of the titanium alloy substrate 9 is fixed in preparation for the experimental needs.

[0048] Among them, Figure 2 As shown, in step S102, the wire feeding speed and the stacking speed are set to perform the first layer of additive manufacturing. After the first layer of additive manufacturing is completed, the tungsten electrode tip height and the stacking direction are adjusted to perform the second layer of additive manufacturing; including:

[0049] Adjust the height of the tungsten electrode tip, and keep the distance between the tungsten electrode tip and the stacking layer at 5mm;

[0050] Adjusting the wire feeding speed of the Ni / Ti heterogeneous twin wires to control the Ni / Ti content of the additive manufacturing layer 10 to form a nickel-titanium alloy gradient part;

[0051] During stacking, different wire feeding speed ratios are used on the XY plane, that is, the wire feeding speed ratios of the previous and next passes in each layer are different, and two wire feeding speed ratios are used in each layer to control the content of Ni and Ti elements;

[0052] When adding the first layer, the Ni / Ti wire feeding speed ratio used in the first pass is 1:1.5, and the Ni / Ti wire feeding speed ratio used in the second pass is 1:2. By analogy, the wire feeding speed ratio of the odd-numbered passes in the first layer is 1:1.5, and the wire feeding speed ratio of the even-numbered passes is 1:2.

[0053] When adding the second layer, the Ni / Ti wire feeding speed ratio used in the first pass is 1:2, and the Ni / Ti wire feeding speed ratio used in the second pass is 1:1.5. By analogy, the wire feeding speed ratio of the odd-numbered passes in the second layer is 1:2, and the wire feeding speed ratio of the even-numbered passes is 1:1.5.

[0054] Repeat the first layer additive method to complete the additive manufacturing of odd-numbered layers of the multi-layer stacking, repeat the second layer additive method to complete the additive manufacturing of even-numbered layers of the multi-layer stacking, and the stacking direction of the odd-numbered layers is the Y direction, and the stacking direction of the even-numbered layers is the X direction. The stacking direction of the next layer is adjusted by 90° based on the stacking direction of the previous layer, thereby completing the additive manufacturing of the multi-layer stacking.

[0055] The stacking speed can be set as required by the existing well-known welding carriage during the test; and the stacking direction can be adjusted and set by the welding carriage; wherein the height of the tungsten electrode tip can be adjusted manually.

[0056] The additive manufacturing of multi-layer stacking also includes, after the additive manufacturing is completed, cutting it into a cylinder with a diameter of 25 mm and a height of 40 mm by wire cutting. This facilitates subsequent elasticity testing. In general, by repeating the additive method of the first and second layers, and the first layer and other odd-numbered layers use the stacking direction of the Y direction, and the second layer and other even-numbered layers use the stacking direction of the X direction, a total of 30 layers are added.

[0057] In order to test the compression performance of additively manufactured parts, compression tests were carried out on gradient functional parts and parts made of different steel materials. Figure 3 As shown in the figure, it can be seen that the elastic properties of gradient functional materials are better than those of steel parts, the recovery effect after compression is better, and the compression resistance is also better than that of ordinary steel parts.

[0058] Example 2: Figure 4 As shown, the embodiment of the present invention discloses a gradient functional material additive manufacturing device for a shock absorber, and implements a gradient functional material additive manufacturing method for a shock absorber, including: a TIG welding gun 1, a TIG welding power source 2, an argon gas bottle 3, a wire feeder 1 4, a wire feeder 2 5, a Ni wire 6, a Ti wire 7, an AC power source 8, a titanium alloy substrate 9, and an additive manufacturing layer 10;

[0059] The argon gas cylinder 3 is used to provide shielding gas during additive manufacturing; the TIG welding power source 2 is used to supply power to the TIG welding gun 1;

[0060] The TIG welding gun 1 is used to clamp the tungsten electrode to achieve welding; and can deliver and spray the shielding gas provided by the argon gas bottle 3;

[0061] The wire feeder 4 is used to provide the Ti wire 7 and adjust the wire feeding speed;

[0062] The wire feeder 2 5 is used to provide Ni wire 6 and adjust the wire feeding speed;

[0063] The AC power source 8 is used to provide AC power to the Ni wire 6 and the Ti wire 7;

[0064] The titanium alloy substrate 9 is used to provide support for the additive manufacturing layer 10 , so as to facilitate the stacking of the additive manufacturing layer 10 .

[0065] Among them, the argon cylinder 3 is used to provide protective gas during additive manufacturing, and after turning on the TIG welding power supply 2, the flow rate of the protective gas during additive manufacturing is adjusted; while turning on the TIG welding power supply 2, the process parameters of the power supply are adjusted to facilitate providing power to the TIG welding gun 1.

[0066] Among them, wire feeder 1 4 and wire feeder 2 5 adjust the appropriate wire feeding speed in the later experiment, and adjust the positions of the double wires, namely Ni wire 6 and Ti wire 7, so that the double wires are symmetrically distributed in the XZ direction.

[0067] Among them, after turning on the AC power supply 8, the AC power output of the AC power supply 8 is adjusted by the AC power parameters passed through the welding wire; by moving the TIG welding gun 1 to the initial position, adjusting the position of the tungsten tip, the titanium alloy substrate 9 is polished, and then the position of the titanium alloy substrate 9 is fixed for experimental needs; the titanium alloy substrate 9 can be Ti6Al4V, referred to as TC4.

[0068] Among them, Figure 4 As shown in the partial enlarged figure, in order to accurately control the accuracy during additive manufacturing, the distance between the extreme end of the tungsten electrode and the additive layer is set to 5 mm, the ends of the two welding wires, namely the ends of the Ni wire 6 and the Ti wire 7, coincide with the extension line of the tip of the tungsten electrode at point O, and the vertical distance between point O and the titanium alloy substrate 9 is 3 mm. The angle between the welding wire and the tungsten electrode is controlled to be 70° in the ZY plane, and the angle between the welding wire and the tungsten electrode is controlled to be 45° in the ZX plane.

[0069] In summary, the present invention achieves different Ti / Ni ratios by adjusting the wire feeding speeds of the Ni wire 6 and the Ti wire 7, which is convenient for the in-situ formation of Ti / Ni in the additive manufacturing metallurgical process, and uses titanium alloy wire and nickel alloy wire to control the Ni / Ti alloy component ratio. The deposition path planning in the form of a texture is adopted, and the stacking additive method is adopted to complete the additive manufacturing of multi-layer stacking, and the Ti / Ni alloy gradient functional material is developed; thus, the additive manufacturing technology is used to overcome the problem of difficult alloy ratio in the nickel-titanium alloy, and the nickel-titanium alloy has the characteristics of high elasticity, memory effect, and easy availability and low cost of materials, which reduces the manufacturing cost of the shock absorber gradient functional material additive and improves the practicality of the shock absorber nickel-titanium alloy gradient functional material additive.

Claims

1. A method for additive manufacturing of a functional gradient material for a shock absorber, characterized in that it comprises the following steps: S101, adjust the test equipment; S102, start the test, set the wire feeding speed of Ni wire and Ti wire, set the stacking speed, perform the first layer of additive manufacturing, after the first layer of additive manufacturing is completed, adjust the tungsten tip height and stacking direction, and perform the second layer of additive manufacturing; specifically, Adjust the height of the tungsten electrode tip, and keep the distance between the tungsten electrode tip and the stacking layer at 5mm; Adjust the wire feeding speed of the Ni / Ti heterogeneous twin wires to control the Ni / Ti content of the additive manufacturing layer to form a NiTi alloy gradient part; During stacking, different wire feeding speed ratios are used on the XY plane, that is, the wire feeding speed ratios of the previous and next passes in each layer are different, and two wire feeding speed ratios are used in each layer to control the content of Ni and Ti elements; When adding the first layer, the Ni / Ti wire feeding speed ratio used in the first pass is 1:1.5, and the Ni / Ti wire feeding speed ratio used in the second pass is 1:

2. By analogy, the wire feeding speed ratio of the odd-numbered passes in the first layer is 1:1.5, and the wire feeding speed ratio of the even-numbered passes is 1:

2. When adding the second layer, the Ni / Ti wire feeding speed ratio used in the first pass is 1:2, and the Ni / Ti wire feeding speed ratio used in the second pass is 1:1.

5. By analogy, the wire feeding speed ratio of the odd-numbered passes in the second layer is 1:2, and the wire feeding speed ratio of the even-numbered passes is 1:1.

5. S103, repeating the above step S102 to complete the additive manufacturing of multi-layer stacking; S104, closing the test equipment, removing the additive manufacturing specimen, and ending the test; Repeating the above step S102 to complete the additive manufacturing of multi-layer stacking includes: Repeat the first layer additive method to complete the additive manufacturing of odd-numbered layers of multi-layer stacking, repeat the second layer additive method to complete the additive manufacturing of even-numbered layers of multi-layer stacking, and the stacking direction of the odd-numbered layers is the Y direction, and the stacking direction of the even-numbered layers is the X direction, and the stacking direction of the next layer is adjusted by 90° based on the stacking direction of the previous layer, thereby completing the additive manufacturing of the multi-layer stacking; The method of completing the additive manufacturing of the multi-layer stacking also includes, after the additive manufacturing is completed, cutting it into columns with a diameter of 25 mm and a height of 40 mm by wire cutting.

2. The functional gradient material additive manufacturing method for shock absorber according to claim 1, characterized in that: The adjustment test equipment comprises the following steps: Turn on the TIG welding power supply, adjust the process parameters, open the argon gas bottle, and set the flow rate of the protective gas during additive manufacturing; Turn on two wire feeders, adjust the wire feeding speed, and adjust the position of the double wires so that the double wires are symmetrically distributed in the XZ direction; Turn on the AC power supply and set the AC power parameters for the welding wire; Adjust the position of the tungsten electrode tip, move the TIG welding gun to the initial position, grind the titanium alloy substrate, and fix the position of the titanium alloy substrate in preparation for experimental needs.

Citation Information

Patent Citations

  • Heterogeneous grid structure layered composite material and double-wire electric arc additive manufacturing method thereof

    CN112276294A

  • Method for assisting dual wires in additive in-situ synthesis of NiTi shape memory alloy based on electron beam scanning

    CN113770377A

  • High-strength maraging steel wire material for additive manufacturing and additive manufacturing process of high-strength maraging steel wire material

    CN116657056A

  • Device and method for manufacturing gradient material through alternating-current-assisted double-wire argon arc welding additive