A high resilience polytetrafluoroethylene material and its preparation process

Through the refining, cyclic directional stretching and low-temperature molding processes of polytetrafluoroethylene powder, the problem of insufficient compression and resilience of polytetrafluoroethylene materials under high pressure and high temperature is solved, and its resilience and creep resistance are significantly improved. Meets the use requirements under complex working conditions.

CN118650904BActive Publication Date: 2024-11-15JIHUA LAB
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411088099.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-15
Estimated Expiration
2044-08-09

AI Technical Summary

Technical Problem

The existing polytetrafluoroethylene materials have poor compression rebound, fatigue resistance and creep resistance under special operating conditions with high pressure and high temperature, making it difficult to meet the long-term reliability requirements of industrial flanges and oil seal materials.

Method used

Using the refining, circular directional stretching, low-temperature molding and sintering processes of polytetrafluoroethylene powder and wetting solvents and fillers, a fibrous structure is formed through directional stretching, combining low-temperature molding and sintering to ensure the stretching state of the molecular chain to improve the material resilience and creep resistance.

Benefits of technology

It significantly improves the resilience and fibrotic structure of polytetrafluoroethylene materials, enhances its performance under complex operating conditions, and meets the higher requirements for material performance by high-end technical equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118650904B_ABST
    Figure CN118650904B_ABST
Patent Text Reader

Abstract

The present application relates to the technical field of composite materials, and discloses a high-resilience polytetrafluoroethylene material and its preparation process. The preparation process comprises the following steps: after mixing polytetrafluoroethylene powder and a wetting solvent, a filler is added, and a polytetrafluoroethylene material is obtained after banburying; the polytetrafluoroethylene material is cyclically oriented and stretched; the polytetrafluoroethylene material is low-temperature molded; and the polytetrafluoroethylene material is sintered to obtain a high-resilience polytetrafluoroethylene material; the temperature of low-temperature molded is ‑10~0°C. The present application utilizes the characteristics of high melt index and easy orientation of fiber crystal form of polytetrafluoroethylene, combines banburying with cyclic oriented stretching and low-temperature molding process, not only fully ensuring the internal fiberization of polytetrafluoroethylene material, but also ensuring that the material is still in a molecular chain stretching state under high molding pressure, and will not curl up due to heat concentration. The polytetrafluoroethylene prepared by this process has a strong fibrosis structure and high resilience.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of composite materials, and mainly to a high-resilience polytetrafluoroethylene material and a preparation process thereof. Background Art

[0002] At present, polymer materials are widely used in the industrial field due to their excellent mechanical properties. With the rapid development of high-end technical equipment, higher requirements are put forward for the mechanical properties such as compression and rebound of polymer materials under high pressure and high temperature special working conditions, especially for industrial flange gaskets. In order to ensure the reliability of long-term use, polymer materials are also required to have sufficient fatigue resistance and creep resistance. At present, polytetrafluoroethylene resin materials in polymer materials have attracted much attention due to their excellent corrosion resistance. However, their compression rebound, fatigue resistance and creep resistance are poor, and they are prone to failure due to deformation during use as flange and oil seal materials. Therefore, it is necessary to propose a new polytetrafluoroethylene material processing technology to improve the problem of poor rebound and compression performance of polytetrafluoroethylene materials. Therefore, the existing technology still needs to be improved and developed. Summary of the invention

[0003] In view of the above-mentioned deficiencies in the prior art, the purpose of the present application is to provide a high-rebound polytetrafluoroethylene material and a preparation process thereof, aiming to solve the problem of poor rebound and compression performance of the existing polytetrafluoroethylene material.

[0004] The technical solution of this application is as follows:

[0005] In a first aspect, the present application provides a preparation process of a high resilience polytetrafluoroethylene material, which comprises the following steps:

[0006] The polytetrafluoroethylene powder and the wetting solvent are mixed, and then the filler is added, and the polytetrafluoroethylene material is obtained after banburying;

[0007] cyclically directional stretching the polytetrafluoroethylene material;

[0008] Low-temperature compression molding of the polytetrafluoroethylene material;

[0009] Then, the polytetrafluoroethylene material is sintered to obtain the high-resilience polytetrafluoroethylene material;

[0010] The temperature of the low temperature compression molding is -10~0℃.

[0011] The present application sequentially processes polytetrafluoroethylene through a process of banburying-cyclic directional stretching-low temperature molding-sintering. The cyclic directional stretching allows the polytetrafluoroethylene molecular segments to be oriented to form a certain fibrous structure. The molded polytetrafluoroethylene material has obvious fibrous shape, low compressibility and high resilience.

[0012] Furthermore, the step of low temperature compression molding the polytetrafluoroethylene material comprises:

[0013] The polytetrafluoroethylene material is placed in a mold while hot, a molding pressure of 10 MPa is applied, the temperature is cooled to -10-0°C, the molding pressure is increased to 40-60 MPa, and the molding is performed for 15 minutes.

[0014] In the present application, a certain pre-pressure is applied and then cooled to facilitate molding and release the stress caused by stretching. The molding pressure is increased at low temperature for cold pressing to alleviate the problem of curling of polytetrafluoroethylene molecular chain segments. The density of the molecular chain is increased in a stretched state, which is beneficial to improving the resilience and creep resistance of the polytetrafluoroethylene material.

[0015] Furthermore, the cyclic directional stretching is performed by a double-roll mill, with the front roller rotating at a speed of 30-40 RPM, the roller temperature at 320-340° C., and the time being 2 hours.

[0016] Furthermore, the banburying temperature is 320-340° C., the banburying rate is 100 RPM, and the banburying is performed for 2 hours and then kept warm for 1 hour.

[0017] Furthermore, the particle size of the polytetrafluoroethylene powder is 20-40 μm.

[0018] Further, the sintering temperature is 365°C;

[0019] The sintering temperature was first increased from room temperature to 220°C at 150°C / h and then kept at that temperature for 10 minutes, then increased to 365°C at 60°C / h and kept at that temperature for 1 hour, and after the sintering was completed, the temperature was decreased to 220°C at 40°C / h and kept at that temperature for 2 hours, and then naturally cooled.

[0020] Furthermore, the wetting solvent is one or more of polyethylene glycol, polyether-modified silicone oil, fatty alcohol polyoxyethylene ether, polyoxyethylene alkylphenol ether and fluorocarbon surfactant.

[0021] Furthermore, the mass ratio of the polytetrafluoroethylene powder to the wetting solvent is 10:1.

[0022] Furthermore, the mass ratio of the polytetrafluoroethylene powder to the filler is 5:1;

[0023] The filler is carbon black.

[0024] In a second aspect, the present application further provides a high resilience polytetrafluoroethylene material, wherein the material is prepared by the preparation process of the high resilience polytetrafluoroethylene material as described in the first aspect.

[0025] Beneficial effects: This application utilizes the high melt index and easy orientation of fiber crystals of polytetrafluoroethylene, combines banburying with cyclic directional stretching and low-temperature molding processes, not only fully ensuring the internal fiberization of polytetrafluoroethylene materials, but also ensuring that the molecular chains inside the material are still in a stretched state under high molding pressure, and will not curl up due to heat concentration. The polytetrafluoroethylene prepared by this process has a strong fiberized organizational structure and high resilience.

[0026] Compared with the traditional cold pressing and sintering process, this application adopts the material stretching and fiberization process to introduce the fiber network structure into the material, and sintering is performed after low-temperature cooling and molding to ensure the fiber network structure while fully cross-linking the molecular chain segments. The polytetrafluoroethylene material prepared by this application has the characteristics of high resilience and high fiberization, which can better meet the performance requirements of gaskets under complex working conditions. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 This is a scanning electron microscope image of the cross section of the high resilience polytetrafluoroethylene material of Example 1 of the present application.

[0028] Figure 2 This is a scanning electron microscope image of the cross section of the polytetrafluoroethylene material of Comparative Example 1 of the present application.

[0029] Figure 3 This is a scanning electron microscope image of the cross section of the polytetrafluoroethylene material of Comparative Example 2 of the present application. DETAILED DESCRIPTION

[0030] The present application provides a high resilience polytetrafluoroethylene material and a preparation process thereof. To make the purpose, technical solution and effect of the present application clearer and more specific, the present application is further described in detail below. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.

[0031] The present application provides a preparation process of a high resilience polytetrafluoroethylene material, which comprises the following steps:

[0032] S1, mixing polytetrafluoroethylene powder and a wetting solvent, adding filler, and kneading to obtain a polytetrafluoroethylene material;

[0033] S2, cyclically directional stretching the polytetrafluoroethylene material;

[0034] S3, molding the polytetrafluoroethylene material at low temperature;

[0035] S4. Sintering the polytetrafluoroethylene material to obtain a high-resilience polytetrafluoroethylene material.

[0036] Taking into account the special molecular structure of polytetrafluoroethylene, this application proposes a processing technology that combines banburying and low-temperature molding. After adding a wetting solvent and a filler to polytetrafluoroethylene powder, banburying and mixing are performed. The polytetrafluoroethylene material is internally fiberized by cyclic directional stretching. The stretched material is added to a mold with a specific shape for low-temperature molding. After molding, the material is demolded and placed in a high-temperature furnace for sintering to obtain a high-resilience polytetrafluoroethylene material. This method has low cost and high efficiency. The polytetrafluoroethylene prepared by this method has higher resilience.

[0037] Furthermore, the particle size of the polytetrafluoroethylene powder is 20-40 μm. In the present application, a higher particle size of the polytetrafluoroethylene powder is not conducive to the reinforcing phase mixing, while if the particle size is lower, the crosslinking degree of the material is insufficient and the mechanical properties are poor. Therefore, the present application controls the particle size of the polytetrafluoroethylene powder to 20-40 μm, so as to ensure the performance improvement effect of the mixing process.

[0038] The polytetrafluoroethylene powder can be commercially available polytetrafluoroethylene powder, or polytetrafluoroethylene suspension powder prepared by suspension polymerization. In the present application, the polytetrafluoroethylene powder can be FR104-4 from Shanghai San Ai Fu New Material Technology Co., Ltd.

[0039] Further, in step S1, the mass ratio of polytetrafluoroethylene powder to wetting solvent is 10:1, and the wetting solvent is one or more of polyethylene glycol, polyether-modified silicone oil, fatty alcohol polyoxyethylene ether, polyoxyethylene alkylphenol ether and fluorocarbon surfactant. Among them, polyethylene glycol can be one or more of polyethylene glycol 200 and polyethylene glycol 400. In the present application, the wetting solvent is selected from a liquid substance with a certain viscosity. By mixing the polytetrafluoroethylene powder and the wetting solvent in a mass ratio of 10:1, the polytetrafluoroethylene powder can have better processability, so that the performance of the polytetrafluoroethylene material is improved, and the selected wetting solvent can gradually volatilize during the subsequent high-temperature processing to avoid affecting the segment performance of the polytetrafluoroethylene material.

[0040] Furthermore, the mass ratio of polytetrafluoroethylene powder to filler is 5:1; the filler is carbon black. In the present application, the carbon black used can play a reinforcing role and play a role in refining grains in the subsequent cooling process.

[0041] Furthermore, in step S1, the banburying temperature is 320-340°C, the banburying rate is 100RPM, and the banburying is carried out for 1 hour after 2 hours of banburying. In the present application, the banburying temperature is based on the glass transition temperature of polytetrafluoroethylene. If the banburying temperature is too low, the processing will be difficult. If the temperature is too high, the polytetrafluoroethylene will be fully cross-linked during the banburying process, which is not conducive to subsequent molding. Among them, by keeping warm for 1 hour after the banburying is completed, it can play two roles: (1) releasing the stress generated by the cross-linking of the chain segments during the banburying process; (2) providing sufficient time for the cross-linking of the chain segments of the polytetrafluoroethylene material. If stretching is performed directly after banburying, the polytetrafluoroethylene material is prone to severe deformation after molding due to excessive internal stress.

[0042] Further, in step S2, the cyclic directional stretching can be performed by high-temperature double rollers, the front roller speed is 30-40RPM, the roller temperature is 320-340°C, and the time is 2h. In the present application, the cyclic directional stretching can be performed by a double-roll mill in the prior art, the front roller is actively rotated by a motor, and the rear roller is driven to rotate, and the polytetrafluoroethylene material produces a certain stretching effect under the traction force of the front roller and the pulling force of the rear roller. After running for a certain period of time, the polytetrafluoroethylene material has a certain degree of directional stretching, and can present a fibrous crystalline structure in the subsequent cooling process. Specifically, if the rotation speed of the front roller in the cyclic directional stretching is too low, it will be difficult to play the stretching and finishing role. If the rotation speed of the front roller is too high, the internal structure of the material will be damaged and the performance will fail. The present application performs cyclic directional stretching on the polytetrafluoroethylene material within the range of 30-40RPM of the front roller rotation speed. At the same time, it can increase the uniformity of the polytetrafluoroethylene material and improve the consistency of the crystal orientation of the polytetrafluoroethylene material. This is beneficial to improving the arrangement effect of the polytetrafluoroethylene material during subsequent low-temperature molding, and is beneficial to improving the resilience of the polytetrafluoroethylene material.

[0043] In the present application, the crosslinking degree of the polytetrafluoroethylene material after banburying and cyclic directional stretching is low. In order to improve the crosslinking degree, the polytetrafluoroethylene material needs to be molded and then sintered. However, heat will be generated during the molding process due to compression. If heat is generated during the molding stage, it will lead to uneven dispersion molding, affecting the material's resilience. Specifically, before molding, the temperature can be lowered to a certain temperature before compression, and at the same time, the problem of premature crosslinking or self-curling of the polytetrafluoroethylene before high-temperature sintering can be avoided due to the high temperature after compression.

[0044] Furthermore, after the cyclic directional stretching, the polytetrafluoroethylene material can be placed in a mold while hot, cooled and formed under a certain pre-pressure, and after the mold is subjected to low temperature treatment, the polytetrafluoroethylene material is cold pressed under a certain molding pressure for a certain time. Among them, the low temperature cooling molding can use a cold pressing mold with a low temperature cooling function, and a coolant pipeline can be set on the outside of the mold for cooling.

[0045] Specifically, in step S3, the step of low-temperature compression molding of the polytetrafluoroethylene material includes:

[0046] The polytetrafluoroethylene material after cyclic directional stretching is placed in a mold while hot, a molding pressure of 10 MPa is applied, the temperature is then cooled to -10~0°C, the molding pressure is then increased to 40-60 MPa, and the molding is performed for 15 minutes.

[0047] In the present application, the polytetrafluoroethylene material is placed in a mold while hot and a pre-pressure of 10 MPa is applied to facilitate molding. At the same time, the stress caused by stretching is released under a certain pre-pressure to avoid stress accumulation that may be caused by direct low-temperature molding.

[0048] When the stretched polytetrafluoroethylene material is molded at room temperature, the material will gather and curl up in advance due to the temperature rise of the molding. In this application, by cooling the molding temperature to -10~0℃, the problem of the curling of the polytetrafluoroethylene molecular chain segments caused by the heat generated by compression inside the polytetrafluoroethylene material during the molding process can be alleviated under low temperature cooling, and the performance of the polytetrafluoroethylene molecular chain segments can be maintained and the fatigue resistance can be improved. At the same time, as the cooling process proceeds, the stretching arrangement effect of the polytetrafluoroethylene chain segments is fixed in time, and the chain segments will not curl up due to heat concentration. After cooling, the molding is maintained at a low temperature to increase the molding pressure so that the polytetrafluoroethylene material can be cold-pressed. The material can increase the density while keeping the molecular chain stretched, which is beneficial to improving the resilience and creep resistance of the polytetrafluoroethylene material after molding.

[0049] Among them, after cooling, the molding pressure is increased to 40-60MPa for molding for 15 minutes. After cooling to a low temperature, if the molding pressure used in the present application is lower than 40 MPa, the molding will be insufficient, and if the molding pressure is higher than 60MPa, the molding pressure is too high, and the crystalline area in the polytetrafluoroethylene material and the amorphous area between the crystalline areas will slip under high pressure, which may easily cause the sintered tube material to be fractured. By molding at 40-60MPa, it is beneficial to maintain the internal structure of the polytetrafluoroethylene material, which is beneficial to the compression rebound performance after molding.

[0050] Furthermore, in step S4, the sintering temperature is 365° C. In the present application, polytetrafluoroethylene material is greatly affected by temperature. If the sintering temperature is too high, polytetrafluoroethylene will decompose. The present application sets the sintering temperature to 365° C. to ensure the integrity of the molecular structure of polytetrafluoroethylene and ensure the performance of the resilience.

[0051] Specifically, if the temperature gradient of the sintering of the polytetrafluoroethylene material is set unreasonably, direct heating or cooling will cause a large deformation of the material, which will affect the control of the size specifications during the production process. Furthermore, in step S4, the sintering temperature is first increased from room temperature to 220°C at 150°C / h and then kept warm for 10 minutes, then increased to 365°C at 60°C / h and kept warm for 1 hour, and after the sintering is completed, the temperature is cooled to 220°C at 40°C / h and kept warm for 2 hours before cooling naturally. In the present application, the molecular chain entanglement and linear expansion effects of the polytetrafluoroethylene material during the sintering stage are fully taken into account. By controlling the heating and cooling speed, the degree of crystallization of the polytetrafluoroethylene material can be guaranteed, so that the polytetrafluoroethylene material has a lower deformation amount, avoiding affecting the processing and mechanical properties of the polytetrafluoroethylene material.

[0052] In the present application, polytetrafluoroethylene is sequentially subjected to the process of internal mixing-cyclic directional stretching-low temperature molding-sintering. The internal mixing allows the polytetrafluoroethylene to be fully mixed with the wetting solvent and carbon black and initially plays a reinforcing role. The cyclic directional stretching allows the polytetrafluoroethylene molecular chain segments to be oriented to form a certain fibrous structure. In this way, after low temperature molding, the shaped polytetrafluoroethylene material can have a higher density. After high temperature sintering, the molecular chains of the polytetrafluoroethylene material are more fully cross-linked, and the fibrous structure has a higher resilience.

[0053] The present application also provides a high-resilience polytetrafluoroethylene material, wherein the material is prepared by the above-mentioned high-resilience polytetrafluoroethylene material preparation process. The high-resilience polytetrafluoroethylene material provided by the present application is prepared by low-temperature molding and sintering after undergoing a banburying and cyclic stretching process. The formed polytetrafluoroethylene material has obvious fiber shape, low compressibility and high resilience, and can better meet the performance requirements of gaskets under complex working conditions.

[0054] The invention is further described below by means of specific examples.

[0055] The preparation method of the high resilience polytetrafluoroethylene material of Example 1 comprises the following steps:

[0056] 1. Evenly mix 5 kg of polytetrafluoroethylene powder and 0.5 kg of fatty alcohol polyoxyethylene ether in a blender to obtain a mixture for later use.

[0057] 2. Pour the mixture prepared in step 1 and 1 kg of carbon black into an internal mixer, set the mixer temperature to 320°C and the mixer speed to 100 RPM, mix for 2 hours and then keep warm for 1 hour. After the mixing is completed, set aside.

[0058] 3. Place the polytetrafluoroethylene material after the internal mixing in step 2 in a double-roll mill for cyclic directional stretching at 330°C for 2 hours, set the front roller speed to 35RPM, and keep it warm for use after the stretching is completed.

[0059] 4. Place the polytetrafluoroethylene material prepared in step 3 in a mold with a diameter of 200 mm while it is still hot, set the molding machine to apply a molding pressure of 10 MPa, connect the cooling liquid to the outside of the mold, and set the temperature to -5°C. After the temperature drops to -5°C, set the molding pressure to 50 MPa, the molding time to 15 minutes, and take it out after the molding is completed.

[0060] 5. Place the cold pressed material prepared in step 4 in a high temperature furnace with a blowing system and sinter it according to the following procedure:

[0061] The temperature was raised from room temperature to 220°C at a rate of 150°C / h and kept at that temperature for 10 minutes. The temperature was then raised to 365°C at a rate of 60°C / h and kept at that temperature for 1 hour. After the sintering was completed, the temperature was lowered to 220°C at a rate of 40°C / h and kept at that temperature for 2 hours before being cooled naturally.

[0062] 6. After step 5 is completed, the high resilience polytetrafluoroethylene material of Example 1 is obtained.

[0063] Comparative Example 1

[0064] The preparation method of the polytetrafluoroethylene material of Comparative Example 1 comprises the following steps:

[0065] 1. Mix 5 kg of polytetrafluoroethylene powder, 0.5 kg of fatty alcohol polyoxyethylene ether and 1 kg of carbon black in a high-speed mixer to obtain a mixture for use.

[0066] 2. Pour the mixture prepared in step 1 into a 200 mm mold at normal pressure, set the molding pressure of the molding machine to 50 MPa, and the molding time to 15 min. After the molding process is completed, demold the mold for use.

[0067] 3. Place the material prepared in step 2 in a high-temperature sintering furnace and sinter according to the following procedure:

[0068] The temperature was raised from room temperature to 220°C at a rate of 150°C / h and kept at that temperature for 10 minutes. The temperature was then raised to 365°C at a rate of 60°C / h and kept at that temperature for 1 hour. After the sintering was completed, the temperature was lowered to 220°C at a rate of 40°C / h and kept at that temperature for 2 hours before being cooled naturally.

[0069] 4. After step 3 is completed, take it out to obtain the polytetrafluoroethylene material of comparative example 1.

[0070] Comparative Example 2

[0071] The preparation method of the polytetrafluoroethylene material of Comparative Example 2 comprises the following steps:

[0072] 1. Evenly mix 5 kg of polytetrafluoroethylene powder and 0.5 kg of fatty alcohol polyoxyethylene ether in a blender to obtain a mixture for later use.

[0073] 2. Pour the mixture prepared in step 1 and 1 kg of carbon black into an internal mixer, set the mixer temperature to 320°C and the mixer speed to 100 RPM, mix for 2 hours and then keep warm for 1 hour. After the mixing is completed, set aside.

[0074] 3. Place the polytetrafluoroethylene material after the internal mixing in step 2 in a double-roll mill for cyclic directional stretching at 330°C for 2 hours, set the front roller speed to 35RPM, and keep it warm for use after the stretching is completed.

[0075] 4. Place the polytetrafluoroethylene material prepared in step 3 in a mold with a diameter of 200 mm, set the molding pressure of the molding machine to 50 MPa, and the molding time to 15 min. After the molding process is completed, demold the material for standby use.

[0076] 5. Place the cold pressed material prepared in step 4 in a high temperature furnace with a blowing system and sinter it according to the following procedure:

[0077] The temperature was raised from room temperature to 220°C at a rate of 150°C / h and kept at that temperature for 10 minutes. The temperature was then raised to 365°C at a rate of 60°C / h and kept at that temperature for 1 hour. After the sintering was completed, the temperature was lowered to 220°C at a rate of 40°C / h and kept at that temperature for 2 hours before being cooled naturally.

[0078] 6. After step 5 is completed, the polytetrafluoroethylene material of comparative example 2 is obtained.

[0079] Performance Testing

[0080] The internal structures of the high resilience polytetrafluoroethylene material of Example 1 and the polytetrafluoroethylene materials prepared in Comparative Examples 1-2 were observed by scanning electron microscopy. The scanning electron microscopy image of the cross section of the high resilience polytetrafluoroethylene material of Example 1 is as follows: Figure 1 As shown, the scanning electron microscope image of the cross section of the polytetrafluoroethylene material of Comparative Example 1 is as shown Figure 2 As shown, the scanning electron microscope image of the cross section of the polytetrafluoroethylene material of Comparative Example 2 is as follows Figure 3 shown.

[0081] The high resilience polytetrafluoroethylene material of Example 1 and the polytetrafluoroethylene material prepared in Comparative Examples 1-2 were tested for compression rate, resilience rate and compressive strength. The compression rate and resilience rate were tested in accordance with GB / T12622-2008, and the compressive strength was tested in accordance with GB / T1041-92. The test results of compression rate, resilience rate and compressive strength are shown in Table 1:

[0082] Table 1

[0083] Example 1 Comparative Example 1 Comparative Example 2 Compression rate / % 12.7 17.6 13.9 Rebound rate / % 59.1 45.2 53.4 Compressive strength / MPa (25% deformation) 15.6 11.4 14.3

[0084] By comparison Figure 1 and Figure 2 It can be seen from the scanning electron microscope image that after the high resilience polytetrafluoroethylene material of Example 1 of the present application has been subjected to the banburying and double-roller stretching treatment, the material has an obvious fibrous structure inside, while the fiber structure of the material of Comparative Example 1, which has not been subjected to the stretching treatment, is not obvious. Figure 1 and Figure 3 It can be seen from the scanning electron microscope image that compared with the comparative example 2 which was not molded at low temperature, the fiber structure of the high resilience polytetrafluoroethylene material of Example 1 of the present application is more delicate and has a higher density. Molding at low temperature can improve the chain segments of the polytetrafluoroethylene material. Comparative performance tests show that the materials treated by banburying and stretching have higher resilience and lower compression than traditional treatments, and the compressive strength after 25% deformation is also significantly improved. After low-temperature mold treatment, the compression rate and rebound rate are also improved, and the compressive strength is improved, indicating that the heat generated by the molding process has certain side effects on material molding, and low-temperature treatment can effectively reduce the impact of side effects, thereby improving the mechanical properties of polytetrafluoroethylene materials. The polytetrafluoroethylene material formed by the preparation process provided by the present application has higher resilience and compressive strength, as well as lower compression, which provides a basis for the research and use of high elastic materials.

[0085] It should be understood that the application of the present application is not limited to the above examples. For ordinary technicians in this field, improvements or changes can be made according to the above description, and all these improvements and changes should fall within the scope of protection of the present application.

Claims

1. A preparation process of high resilience polytetrafluoroethylene material, characterized in that: The following steps are involved: The polytetrafluoroethylene powder and the wetting solvent are mixed, and then the filler is added, and the polytetrafluoroethylene material is obtained after banburying; cyclically directional stretching the polytetrafluoroethylene material; Low-temperature compression molding of the polytetrafluoroethylene material; Then, the polytetrafluoroethylene material is sintered to obtain the high-resilience polytetrafluoroethylene material; The temperature of the low temperature compression molding is -10~0℃; The cyclic directional stretching is carried out by a double-roll mill, with the front roller speed being 30-40RPM, the roller temperature being 320-340°C, and the time being 2h; The front roller is driven by a motor to rotate actively, and the rear roller is driven to rotate.

2. The preparation process of high resilience polytetrafluoroethylene material according to claim 1, characterized in that: The step of low temperature compression molding the polytetrafluoroethylene material comprises: The polytetrafluoroethylene material is placed in a mold while hot, a molding pressure of 10 MPa is applied, the temperature is cooled to -10-0°C, the molding pressure is increased to 40-60 MPa, and the molding is performed for 15 minutes.

3. The preparation process of high resilience polytetrafluoroethylene material according to claim 1, characterized in that: The mixing temperature is 320-340° C., the mixing speed is 100 RPM, and the mixing is performed for 2 hours and then kept warm for 1 hour.

4. The preparation process of high resilience polytetrafluoroethylene material according to claim 3, characterized in that: The particle size of the polytetrafluoroethylene powder is 20-40 μm.

5. The preparation process of high resilience polytetrafluoroethylene material according to claim 1, characterized in that: The sintering temperature is 365°C; The sintering temperature was first increased from room temperature to 220°C at 150°C / h and then kept at that temperature for 10 minutes, then increased to 365°C at 60°C / h and kept at that temperature for 1 hour, and after the sintering was completed, the temperature was decreased to 220°C at 40°C / h and kept at that temperature for 2 hours, and then naturally cooled.

6. The preparation process of high resilience polytetrafluoroethylene material according to claim 1, characterized in that: The wetting solvent is one or more of polyethylene glycol, polyether-modified silicone oil, fatty alcohol polyoxyethylene ether, polyoxyethylene alkylphenol ether and fluorocarbon surfactant.

7. The preparation process of high resilience polytetrafluoroethylene material according to claim 6, characterized in that: The mass ratio of the polytetrafluoroethylene powder to the wetting solvent is 10:

1.

8. The preparation process of high resilience polytetrafluoroethylene material according to claim 1, characterized in that: The mass ratio of the polytetrafluoroethylene powder to the filler is 5:1; The filler is carbon black.

9. A high resilience polytetrafluoroethylene material, characterized in that: The high resilience polytetrafluoroethylene material is prepared by the preparation process of the high resilience polytetrafluoroethylene material as described in any one of claims 1 to 8.