A light-transmitting soft stone sheet and its preparation process

By using glass powder and silicon acrylic emulsion to prepare light-transmitting soft stone sheets, the existing stone yield is limited and hard and brittle, achieving high light-transmitting, aesthetics and durability, and is suitable for a variety of decorative applications .

CN118652074BActive Publication Date: 2024-11-15CHUANHAIJU (CHENGDU) INTELLECTUAL PROPERTY OPERATION CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411140493.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-11-15
Estimated Expiration
2044-08-20

AI Technical Summary

Technical Problem

The existing light-transmitting stone has limited output and a hard and brittle texture, which is difficult to meet the paving flatness requirements. At the same time, there is a lack of green and environmentally friendly alternatives, making it difficult to achieve beautiful light-transmitting effects.

Method used

Using glass powder and aqueous resin silicon acrylic emulsion as the main materials, light-transmissive soft stone sheets are prepared through a specific process, combined with mold molding and natural drying, to form a sheet with light-transmissive and flexible characteristics, and achieve five-color color by color adjustment. Colorful effect.

Benefits of technology

It provides a light-transmitting soft stone sheet with high light transmission, impact resistance and excellent aesthetics. It is suitable for indoor and outdoor decoration, and has good water resistance, heat resistance and mechanical properties, and adapts to the paving needs of different flatness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present invention relates to the technical field of light-transmitting soft stone, specifically to a light-transmitting soft stone sheet and a preparation process thereof, comprising the following mass components: 62-68 parts of glass powder, 3-8 parts of aluminum hydroxide, 22-30 parts of silicone-acrylic emulsion, 4-6 parts of water, 0.3-0.6 parts of dispersant, 0.2-0.4 parts of wetting agent, and 0.1-0.5 parts of sodium carboxymethyl cellulose. The present invention uses glass powder as a main inorganic material and water-based resin silicone-acrylic emulsion as a binder to mix and prepare a slurry, which is then formed and dried in a mold to form a sheet with light-transmitting and bendable properties. The slurry can be toned according to demand, so that the light-transmitting soft stone sheet can be light-transmitting in the presence of a back light source, thereby showing a colorful light effect, which is very aesthetic.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of light-transmitting soft stone, in particular to a light-transmitting soft stone sheet and a preparation process thereof. Background Art

[0002] With the development of urban lighting, stones with light-transmitting effects have become the new favorite in the field. A light source is set on the back of the semi-transparent decorative sheet, and the backlight will show a hazy color after passing through the plate. Different optical effects can also be achieved through molds with different textures. However, the output of natural stone is limited, its texture is hard and brittle, and the flatness of the paving surface is required to be high. At the same time, in order to reflect the concept of green environmental protection, we propose a light-transmitting soft stone sheet and its preparation process. Summary of the invention

[0003] The object of the present invention is to provide a light-transmitting soft stone sheet and a preparation process thereof, so as to solve the problems raised in the above-mentioned background technology.

[0004] In order to solve the above technical problems, the present invention provides the following technical solutions: a light-transmitting soft stone sheet, comprising the following components by mass: 62 to 68 parts of glass powder, 3 to 8 parts of aluminum hydroxide, 22 to 30 parts of silicone-acrylic emulsion, 4 to 6 parts of water, 0.3 to 0.6 parts of dispersant, 0.2 to 0.4 parts of wetting agent, and 0.1 to 0.5 parts of sodium carboxymethyl cellulose (CMC).

[0005] Furthermore, the glass powder is a powdered high-transmittance glass powder with a particle size of 120 mesh to 600 mesh.

[0006] Furthermore, the aluminum hydroxide is powdered aluminum hydroxide with a particle size of 325 mesh to 900 mesh.

[0007] Furthermore, the thickness of the light-transmitting soft stone sheet is 3 to 10 mm.

[0008] A preparation process of a light-transmitting soft stone sheet, comprising the following processes:

[0009] Take deionized water, stir and add dispersant, wetting agent, glass powder and aluminum hydroxide, and disperse for 2 to 5 minutes; add sodium carboxymethyl cellulose and continue to disperse for 30 minutes; add silicone acrylic emulsion, stir and disperse for 20 minutes; adjust the color according to the needs to obtain slurry;

[0010] Apply it to the inside of the mold, dry it naturally, and demould it to obtain a sheet.

[0011] In the above technical solution, glass powder is used as the main inorganic material, and water-based resin silicone acrylic emulsion is used as a binder to mix and prepare a slurry, which will be formed and dried in a mold to form the required sheet material, which has light-transmitting and bendable properties, that is, a light-transmitting soft stone sheet material, which can adapt to paving surfaces of different flatness; and compared with natural stone, it has good impact resistance. The slurry can be toned according to demand, so that the light-transmitting soft stone sheet material can be light-transmitting in the presence of a back light source, thereby showing a colorful effect, with excellent aesthetics, suitable for architectural interior and exterior wall decoration of indoor walls and ceilings in hotels, entertainment venues, etc. When the light source is turned on when the ambient light is dark, it can also be used as an atmosphere light.

[0012] Further, the silicone-acrylic emulsion is prepared by the following process:

[0013] Take deionized water, heat it to 57-63°C, add emulsifier, stir and dissolve to obtain emulsifier solution;

[0014] Take 42% to 50% of the mass of the emulsifier solution, heat it to 80 to 90°C, slowly add 75% to 82% of the mass of octamethylcyclotetrasiloxane and 75% to 82% of the mass of γ-methacryloxypropyltrimethoxysilane, add them all within 30 minutes, keep the temperature and react for 100 to 150 minutes to obtain a silicone pre-emulsion;

[0015] Take the remaining emulsifier solution, raise the temperature to 58-65°C, slowly add the allyl monomer and the remaining silicone monomer within 30 minutes, and stir rapidly to react for 25-40 minutes to obtain an acrylic pre-emulsion;

[0016] Slowly add acrylic pre-emulsion and initiator to the silicone pre-emulsion within 60 minutes, while raising the temperature to 72-80°C, then to 88-95°C, stirring and reacting for 100-150 minutes; lowering the temperature to below 40°C, adjusting the pH of the system to 7-8 with aqueous ammonia to obtain silicone-acrylic emulsion.

[0017] Further, the silicone acrylic emulsion includes the following components by mass: 12 to 20 parts of silicone monomer, 80 to 88 parts of allyl monomer, 3.0 to 3.5 parts of emulsifier, 0.8 to 1.5 parts of initiator potassium persulfate and 120 parts of deionized water;

[0018] The emulsifier is a compound of OP-1 and SDBS with a mass ratio of 2:3.

[0019] Furthermore, the organosilicon monomer is a compound of phenylcyclosilane, octamethylcyclotetrasiloxane, and γ-methacryloxypropyltrimethoxysilane;

[0020] The volume ratio of octamethylcyclotetrasiloxane, γ-methacryloxypropyltrimethoxysilane, and phenylcyclosilane is 10:5:(1-3);

[0021] The phenylcyclosilane is a mixture of one or more of 2,4,6-trimethyl-2,4,6-triphenylcyclotrisiloxane, 2,2,4,6-tetramethyl-4,6-diphenyl-2,4,6-triphenylcyclotrisiloxane and 2,4,4,6,6-pentamethyl-2-phenylcyclotrisiloxane.

[0022] Furthermore, the allyl monomer includes the following components: by mass, 50% to 58% methyl methacrylate, 34% to 42% butyl acrylate, 1% to 3% acrylic acid and 3% to 10% alkenyl rosin compound.

[0023] Further, the alkenyl rosin compound is prepared by the following process:

[0024] Take rosin and tetrabutylammonium bromide, mix and dissolve them in anhydrous ethanol, heat to 80-87°C, slowly add epichlorohydrin, add it within 30 minutes, and react for 4 hours; evaporate the ethanol, wash with hot water, distill under reduced pressure, and dry to obtain product A;

[0025] Mix and dissolve product A, 2-(ethylamino)ethyl 2-propenoate and triethylamine in anhydrous ethanol, raise the temperature to 82-90°C, and stir to react for 5 hours; wash, rotary evaporate, and dry to obtain product B;

[0026] The product B and anhydrous ethanol are mixed, n-butyl bromide is added, and the reaction is stirred for 12 to 48 hours; dimethyl carbonate is added, and the stirring is continued for 1 to 2 hours; suction filtration, washing, and drying are performed to obtain an alkenyl rosin compound.

[0027] Further, the mass ratio of rosin, epichlorohydrin, and tetrabutylammonium bromide is 10:(5.2-5.5):(0.15-0.20);

[0028] The ratio of rosin to anhydrous ethanol is 27 g / 100 mL.

[0029] Further, the mass ratio of product A, 2-(ethylamino)ethyl 2-acrylate (CAS No. 51914-45-5), and triethylamine is 10: (3.7-4.1): (3.9-4.3);

[0030] The ratio of product A to anhydrous ethanol is 24 g / 100 mL.

[0031] Further, the mass ratio of product B, n-butyl bromide, and dimethyl carbonate is 10:(2.8-3.1):(1.9-2.1);

[0032] The ratio of product B to anhydrous ethanol is 24 g / 100 mL.

[0033] In the above technical solution, the silicone-acrylic emulsion is obtained by copolymerization of silicone monomers and allyl monomers (such as methyl methacrylate, butyl acrylate, acrylic acid). The acrylic resin prepared by the allyl monomer has good bonding properties, so that the silicone-acrylic emulsion can be used as an adhesive. The polymer prepared by the silicone monomer has extremely low surface energy, and its hydrophobicity, mechanical properties and heat resistance are excellent; the silicone-acrylic emulsion prepared also has heat resistance, water resistance, antifouling, weather resistance and other properties and better mechanical strength.

[0034] Silicone is introduced by free radical copolymerization of allyl monomers, and through the hydrolysis and condensation of the silicon-oxygen bonds in the silicone monomers, a local three-dimensional network structure containing Si-O-Si bonds is formed, which can significantly improve the "hot sticky and cold brittle" problem of acrylic resins made from allyl monomers, while improving its water resistance. However, when the amount of silicone monomer is high, the gel rate of silicone-acrylic emulsion is high; and the molecular chain structure formed after the hydrolysis and condensation of siloxane is a three-dimensional network, not a long-chain polysiloxane macromolecule with a linear structure, resulting in the silicone-acrylic emulsion molecular chain not being flexible enough, and the flexibility of the produced sheet is insufficient. Therefore, in the above-mentioned silicone-acrylic emulsion, the present application obtains a methacryloxypropyl-terminated polysiloxane through a cationic ring-opening reaction of γ-methacryloxypropyltrimethoxysilane with phenylcyclosilane and octamethylcyclotetrasiloxane, which has a linear long-chain macromolecular silicone with better flexibility, and can effectively improve the low-temperature flexibility of the silicone-acrylic emulsion, and improve the water resistance, heat resistance and performance of the prepared sheet at low temperatures. And introduce phenyl groups into the linear long chain, and use its polarization effect to make it have a higher refractive index, thereby improving the optical properties of the silicone-acrylic emulsion and increasing the light transmittance of the sheet. And its unsaturated carbon-carbon double bond is directly connected to the acyloxy group with a larger electronegativity, has a higher reactivity, and helps to promote the copolymerization reaction between the silicone pre-emulsion and the allyl monomer.

[0035] In the above technical scheme, the allyl monomer contains alkenyl rosin compounds, which are successively prepared from rosin and epichlorohydrin under the action of tetrabutylammonium bromide to generate acyloxy groups to obtain rosin compounds containing hydroxypropyl chloride (referred to as product A); the chlorine group in product A reacts with the amine group in 2-(ethylamino)ethyl 2-propenoate to obtain a tertiary amino rosin compound (referred to as product B); product B reacts with n-butyl bromide to obtain a quaternized rosin compound, the bromide ion of which is replaced by dimethyl carbonate, thereby forming a quaternized rosin compound containing allyl groups (referred to as alkenyl rosin compounds), the structure of which has certain surface activity and is conducive to the formation of emulsion. The introduction of rosin-based emulsion can improve the "hot sticky and cold brittle" problem of acrylic resin prepared by allyl monomer, improve its ductility, promote the improvement of the low temperature resistance of the prepared sheet, and avoid its cracking; and can improve the water resistance of the sheet to a certain extent. The introduction of alkenyl rosin compounds makes the silicone acrylic emulsion have cationic properties, which can show certain antibacterial and antistatic properties, and give the sheet antibacterial, mildew-proof and dust-proof capabilities.

[0036] Furthermore, the glass powder is surface modified, and the specific process is as follows:

[0037] Add coupling agent to ethanol aqueous solution, mix for 5-12 minutes; add glass powder, heat to 60-65° C., stir for modification for 4-5 hours; wash and dry to obtain modified glass powder.

[0038] Further, the ratio of glass powder, coupling agent, and ethanol aqueous solution is 10 g: (0.5-1.0) g: 100 mL;

[0039] In the ethanol-water solution, the volume concentration of ethanol is 90%;

[0040] The silane coupling agent is one of 4-trimethoxysilylbutyric acid, 7-trimethoxysilylheptanoic acid and 10-trimethoxysilyldecanoic acid.

[0041] In the above technical solution, the glass powder is surface-coupled and modified with carboxyl siloxane, which can have better dispersibility in the slurry, and contribute to the uniform system of its performance and function. In addition, the carboxyl group is negatively charged in the slurry water dispersion, and can form a strong electrostatic force with the quaternary ammonium salt in the silicone-acrylic emulsion, which helps the adhesion between the glass powder and the silicone-acrylic emulsion, and further improves its comprehensive performance.

[0042] Compared with the prior art, the present invention has the following beneficial effects:

[0043] The present invention describes a light-transmitting soft stone sheet and a preparation process thereof. Glass powder is used as a main inorganic material and a water-based resin silicone acrylic emulsion is used as a binder. A slurry is prepared by mixing, and the slurry is formed and dried in a mold to form a sheet with light-transmitting and bendable properties. The slurry can be colored according to needs so that the light-transmitting soft stone sheet can be light-transmitting in the presence of a back light source, thereby showing a colorful light effect and being extremely aesthetic. DETAILED DESCRIPTION

[0044] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0045] In the following specific implementations,

[0046] Glass powder: P-8, from Saint-Anne Technology (Dongguan) Co., Ltd.

[0047] Aluminum hydroxide: AH-1, from China Aluminum Shandong Co., Ltd.;

[0048] Dispersant: METOLAT 362, from Mingling, Germany;

[0049] Wetting agent: PE-100, from Koning, Germany;

[0050] Sodium carboxymethyl cellulose: from Merck reagent;

[0051] The emulsifier is a compound of OP-1 and SDBS with a mass ratio of 2:3;

[0052] Commercially available silicone acrylic emulsion: HS-1001, from Zhengzhou Guangjie Chemical Co., Ltd.;

[0053] The thickness of the translucent soft stone sheet is 6 mm.

[0054] Embodiment 1: A process for preparing a light-transmitting soft stone sheet, comprising the following processes:

[0055] Step 1, take 27g of rosin and tetrabutylammonium bromide, mix and dissolve in 100mL of anhydrous ethanol, heat to 80°C, slowly add epichlorohydrin, add within 30min, and react for 4h; evaporate the ethanol, wash with hot water, distill under reduced pressure, and dry to obtain product A; the mass ratio of rosin, epichlorohydrin, and tetrabutylammonium bromide is 10:5.2:0.15;

[0056] 24g of product A, 2-(ethylamino)ethyl 2-acrylate and triethylamine were mixed and dissolved in 100mL of anhydrous ethanol, heated to 82°C, and stirred for reaction for 5h; washed, rotary evaporated, and dried to obtain product B; the mass ratio of product A, 2-(ethylamino)ethyl 2-acrylate and triethylamine was 10:3.7:3.9;

[0057] 24 g of product B and 100 mL of anhydrous ethanol were mixed, n-butyl bromide was added, and the mixture was stirred for 12 h; dimethyl carbonate was added, and the mixture was stirred for 1 h; the mixture was filtered, washed, and dried to obtain an alkenyl rosin compound; the mass ratio of product B, n-butyl bromide, and dimethyl carbonate was 10:2.8:1.9;

[0058] Step 2, take deionized water, heat it to 57°C, add an emulsifier, stir and dissolve, and obtain an emulsifier solution;

[0059] Take 42% of the emulsifier solution by weight, heat it to 80°C, slowly add 75% of octamethylcyclotetrasiloxane by weight and 75% of γ-methacryloxypropyltrimethoxysilane by weight, add them all within 30 minutes, keep the temperature and react for 100 minutes to obtain a silicone pre-emulsion;

[0060] Take the remaining emulsifier solution, raise the temperature to 58°C, slowly add the allyl monomer and the remaining silicone monomer, add them all within 30 minutes, and stir rapidly to react for 25 minutes to obtain an acrylic pre-emulsion;

[0061] Slowly add acrylic pre-emulsion and initiator to the silicone pre-emulsion within 60 minutes, and heat to 72°C, then to 88°C, and stir to react for 100 minutes; cool to below 35°C, and adjust the pH of the system to 7 with ammonia water to obtain silicone acrylic emulsion;

[0062] The silicone acrylic emulsion includes the following components by mass: 12 parts of silicone monomer, 88 parts of allyl monomer, 3.0 parts of emulsifier, 0.8 parts of initiator potassium persulfate and 120 parts of deionized water; the silicone monomer is a compound of octamethylcyclotetrasiloxane, γ-methacryloxypropyltrimethoxysilane and phenylcyclosilane in a volume ratio of 10:5:1; the phenylcyclosilane is 2,4,4,6,6-pentamethyl-2-phenylcyclotrisiloxane; the allyl monomer includes the following components: by mass, 54% methyl methacrylate, 42% butyl acrylate, 1% acrylic acid and 3% alkenyl rosin compound;

[0063] Step 3, adding a coupling agent to a 90% ethanol aqueous solution and mixing for 5 minutes; adding glass powder, heating to 60°C, stirring and modifying for 4 hours; washing and drying to obtain modified glass powder; the ratio of glass powder, coupling agent, and ethanol aqueous solution is 10g:0.5g:100mL; the silane coupling agent is 4-trimethoxysilylbutyric acid;

[0064] Step 4, take deionized water, stir and add dispersant, wetting agent, glass powder and aluminum hydroxide, disperse for 2 minutes; add sodium carboxymethyl cellulose, continue to disperse for 30 minutes; add silicone acrylic emulsion, stir and disperse for 20 minutes; adjust the color according to the needs to obtain a slurry; apply it to the inside of the mold, dry naturally, demold, and obtain a sheet, including the following mass components: 62 parts of glass powder, 3 parts of aluminum hydroxide, 30 parts of silicone acrylic emulsion, 4 parts of water, 0.3 parts of dispersant, 0.2 parts of wetting agent, and 0.1 parts of sodium carboxymethyl cellulose.

[0065] Embodiment 2: A process for preparing a light-transmitting soft stone sheet, comprising the following processes:

[0066] Step 1, take 27g of rosin and tetrabutylammonium bromide, mix and dissolve in 100mL of anhydrous ethanol, heat to 85°C, slowly add epichlorohydrin, add within 30min, and react for 4h; evaporate the ethanol, wash with hot water, distill under reduced pressure, and dry to obtain product A; the mass ratio of rosin, epichlorohydrin, and tetrabutylammonium bromide is 10:5.3:0.18;

[0067] 24g of product A, 2-(ethylamino)ethyl 2-acrylate and triethylamine were mixed and dissolved in 100mL of anhydrous ethanol, heated to 85°C, and stirred for reaction for 5h; washed, rotary evaporated, and dried to obtain product B; the mass ratio of product A, 2-(ethylamino)ethyl 2-acrylate and triethylamine was 10:3.9:4.1;

[0068] 24 g of product B and 100 mL of anhydrous ethanol were mixed, n-butyl bromide was added, and the mixture was stirred for 24 h; dimethyl carbonate was added, and the mixture was stirred for 1.5 h; the mixture was filtered, washed, and dried to obtain an alkenyl rosin compound; the mass ratio of product B, n-butyl bromide, and dimethyl carbonate was 10:2.9:2.0;

[0069] Step 2, take deionized water, heat it to 60°C, add emulsifier, stir and dissolve, and obtain emulsifier solution;

[0070] Take 46% of the mass of the emulsifier solution, heat it to 85°C, slowly add 80% of the mass of octamethylcyclotetrasiloxane and 80% of the mass of γ-methacryloxypropyltrimethoxysilane, add them all within 30 minutes, keep the temperature and react for 120 minutes to obtain a silicone pre-emulsion;

[0071] Take the remaining emulsifier solution, raise the temperature to 60°C, slowly add the allyl monomer and the remaining silicone monomer, add them all within 30 minutes, and stir rapidly to react for 30 minutes to obtain an acrylic pre-emulsion;

[0072] Slowly add acrylic pre-emulsion and initiator to the silicone pre-emulsion within 60 minutes, and heat to 75°C, then to 90°C, and stir to react for 120 minutes; cool to below 35°C, and adjust the pH of the system to 7.5 with ammonia water to obtain silicone acrylic emulsion;

[0073] The silicone acrylic emulsion includes the following components by mass: 16 parts of silicone monomer, 84 parts of allyl monomer, 3.2 parts of emulsifier, 1.2 parts of initiator potassium persulfate and 120 parts of deionized water; the silicone monomer is a compound of octamethylcyclotetrasiloxane, γ-methacryloxypropyltrimethoxysilane and phenylcyclosilane in a volume ratio of 10:5:2; the phenylcyclosilane is 2,2,4,6-tetramethyl-4,6-diphenyl-2,4,6-triphenylcyclotrisiloxane; the allyl monomer includes the following components: by mass, 54% methyl methacrylate, 38% butyl acrylate, 2% acrylic acid and 6% alkenyl rosin compound;

[0074] Step 3, adding a coupling agent to a 90% ethanol aqueous solution and mixing for 8 minutes; adding glass powder, heating to 62°C, stirring and modifying for 4.5 hours; washing and drying to obtain modified glass powder; the ratio of glass powder, coupling agent, and ethanol aqueous solution is 10g:0.8g:100mL; the silane coupling agent is 7-trimethoxysilylheptanoic acid;

[0075] Step 4, take deionized water, stir and add dispersant, wetting agent, glass powder and aluminum hydroxide, disperse for 3 minutes; add sodium carboxymethyl cellulose, continue to disperse for 30 minutes; add silicone acrylic emulsion, stir and disperse for 20 minutes; adjust the color according to the needs to obtain a slurry; apply it to the inside of the mold, dry naturally, demold, and obtain a sheet; including the following mass components: 65 parts of glass powder, 5 parts of aluminum hydroxide, 26 parts of silicone acrylic emulsion, 5 parts of water, 0.5 parts of dispersant, 0.3 parts of wetting agent, 0.3 parts of sodium carboxymethyl cellulose.

[0076] Embodiment 3: A process for preparing a light-transmitting soft stone sheet, comprising the following processes:

[0077] Step 1, take 27g of rosin and tetrabutylammonium bromide, mix and dissolve in 100mL of anhydrous ethanol, heat to 87°C, slowly add epichlorohydrin, add within 30min, and react for 4h; evaporate the ethanol, wash with hot water, distill under reduced pressure, and dry to obtain product A; the mass ratio of rosin, epichlorohydrin, and tetrabutylammonium bromide is 10:5.5:0.20;

[0078] 24g of product A, 2-(ethylamino)ethyl 2-acrylate and triethylamine were mixed and dissolved in 100mL of anhydrous ethanol, heated to 90°C, and stirred for reaction for 5h; washed, rotary evaporated, and dried to obtain product B; the mass ratio of product A, 2-(ethylamino)ethyl 2-acrylate and triethylamine was 10:4.1:4.3;

[0079] 24 g of product B and 100 mL of anhydrous ethanol were mixed, n-butyl bromide was added, and the mixture was stirred for 48 h; dimethyl carbonate was added, and the mixture was stirred for 2 h; the mixture was filtered, washed, and dried to obtain an alkenyl rosin compound; the mass ratio of product B, n-butyl bromide, and dimethyl carbonate was 10:3.1:2.1;

[0080] Step 2, take deionized water, heat it to 63°C, add an emulsifier, stir and dissolve, and obtain an emulsifier solution;

[0081] Take 50% of the mass of the emulsifier solution, heat it to 90°C, slowly add 82% of the mass of octamethylcyclotetrasiloxane and 82% of the mass of γ-methacryloxypropyltrimethoxysilane, add them all within 30 minutes, keep the temperature and react for 150 minutes to obtain a silicone pre-emulsion;

[0082] Take the remaining emulsifier solution, raise the temperature to 65°C, slowly add the allyl monomer and the remaining silicone monomer, add them all within 30 minutes, and rapidly stir and react for 40 minutes to obtain an acrylic pre-emulsion;

[0083] Slowly add acrylic pre-emulsion and initiator to the silicone pre-emulsion within 60 minutes, and heat to 80°C, then to 95°C, and stir to react for 150 minutes; cool to below 35°C, and adjust the pH of the system to 8 with ammonia water to obtain silicone acrylic emulsion;

[0084] The silicone acrylic emulsion includes the following components by mass: 20 parts of silicone monomer, 80 parts of allyl monomer, 3.5 parts of emulsifier, 1.5 parts of initiator potassium persulfate and 120 parts of deionized water; the silicone monomer is a compound of octamethylcyclotetrasiloxane, γ-methacryloxypropyltrimethoxysilane and phenylcyclosilane in a volume ratio of 10:5:3; the phenylcyclosilane is 2,4,6-trimethyl-2,4,6-triphenylcyclotrisiloxane; the allyl monomer includes the following components: by mass, 53% methyl methacrylate, 34% butyl acrylate, 3% acrylic acid and 10% alkenyl rosin compound;

[0085] Step 3, adding a coupling agent to a 90% ethanol aqueous solution and mixing for 12 minutes; adding glass powder, heating to 65°C, stirring and modifying for 5 hours; washing and drying to obtain modified glass powder; the ratio of glass powder, coupling agent and ethanol aqueous solution is 10g:1g:100mL; the silane coupling agent is 10-trimethoxysilyldecanoic acid;

[0086] Step 4, take deionized water, stir and add dispersant, wetting agent, glass powder and aluminum hydroxide, disperse for 5 minutes; add sodium carboxymethyl cellulose, continue to disperse for 30 minutes; add silicone acrylic emulsion, stir and disperse for 20 minutes; adjust the color according to the needs to obtain a slurry; apply it to the inside of the mold, dry naturally, demold, and obtain a sheet, including the following mass components: 68 parts of glass powder, 8 parts of aluminum hydroxide, 22 parts of silicone acrylic emulsion, 6 parts of water, 0.6 parts of dispersant, 0.4 parts of wetting agent, and 0.5 parts of sodium carboxymethyl cellulose.

[0087] Comparative Example 1: A process for preparing a light-transmitting soft stone sheet, comprising the following processes:

[0088] Step 1, dimethylaminoethyl methacrylate and n-butyl bromide are mixed, and stirred for 12 hours; dimethyl carbonate is added, and stirring is continued for 60 minutes; suction filtration is performed, and drying is performed to obtain an olefinic compound; the mass ratio of dimethylaminoethyl methacrylate, n-butyl bromide, and dimethyl carbonate is 10:8.8:6.0;

[0089] Steps 2-4 are the same as those in Example 1, except that the alkenyl rosin compound in the process is replaced by the alkenyl compound prepared above to obtain a sheet.

[0090] Comparative Example 2: A process for preparing a light-transmitting soft stone sheet, comprising the following processes:

[0091] Step 1, dissolve 15g of rosin in 100mL of dichloromethane, add 14.2g of oxalyl chloride and 3mL of N,N-dimethylformamide, and stir at 0°C for 3h under nitrogen atmosphere protection; remove excess oxalyl chloride and dichloromethane by rotary evaporation to obtain product A;

[0092] Dissolve 15g of product A in 100mL of dichloromethane, add 8.5g of triethylamine and 2.6g of hydroxyethyl methacrylate in sequence at 0°C, and stir the mixture in a nitrogen atmosphere for 48h; neutralize with sodium bicarbonate solution, dry with anhydrous sodium sulfate, and rotary evaporate to obtain an olefinic rosin compound;

[0093] Step 3, adding a coupling agent to a 90% ethanol aqueous solution and mixing for 5 minutes; adding glass powder, heating to 60°C, stirring and modifying for 4 hours; washing and drying to obtain modified glass powder; the ratio of glass powder, coupling agent, and ethanol aqueous solution is 10g:0.5g:100mL; the silane coupling agent is KH-550;

[0094] Steps 2 and 4 are the same as in Example 1 to obtain a sheet.

[0095] Comparative Example 3: A process for preparing a light-transmitting soft stone sheet.

[0096] In the preparation process of silicone acrylic emulsion, the silicone monomer is γ-methacryloxypropyltrimethoxysilane;

[0097] The other processes were the same as those in Comparative Example 2 to obtain a sheet.

[0098] Comparative Example 4: A preparation process for a translucent soft stone sheet, comprising the following processes: taking deionized water, stirring and adding a dispersant, a wetting agent, glass powder and aluminum hydroxide, and dispersing for 2 minutes; adding sodium carboxymethyl cellulose, and continuing to disperse for 30 minutes; adding a commercially available silicone acrylic emulsion, stirring and dispersing for 20 minutes; adjusting the color according to requirements to obtain a slurry; coating the inside of a mold, naturally drying, and demolding to obtain a sheet, comprising the following mass components: 62 parts of glass powder, 3 parts of aluminum hydroxide, 30 parts of commercially available silicone acrylic emulsion, 4 parts of water, 0.3 parts of a dispersant, 0.2 parts of a wetting agent, and 0.1 parts of sodium carboxymethyl cellulose.

[0099] Experiment: Take the light-transmitting soft stone sheets obtained in Examples 1-3 and Comparative Examples 1-4, prepare samples, test their properties respectively and record the test results:

[0100] Mechanical properties test: a universal testing machine was used to test the tensile properties of the specimens at a tensile rate of 10 mm / min.

[0101] Low temperature performance test: keep the sample at 0℃ for 12h, and test its cantilever beam unnotched impact performance with reference to GB / T 1843;

[0102] Hydrophobic performance test: Use a contact angle meter to test the static contact angle of the sample, and the water droplet is 10μL deionized water;

[0103] Light transmission performance test: Using JC / T 2020-2010 as the reference standard, test the linear light transmittance of the sample;

[0104]

[0105] According to the data in the above table, we can clearly draw the following conclusions:

[0106] The light-transmitting soft stone sheets obtained in Examples 1-3 are compared with the light-transmitting soft stone sheets obtained in Comparative Examples 1-4. The test results show that:

[0107] Compared with the comparative example, the light-transmitting soft stone sheets obtained in Examples 1-3 have higher tensile strength, low-temperature impact strength, transmittance and contact angle data, which fully demonstrates that the present invention achieves improvements in mechanical properties, low-temperature properties, light transmittance and water resistance of light-transmitting soft stone sheets.

[0108] Compared with Example 1, in the silicone-acrylic emulsion of Comparative Example 1, the alkenyl rosin compound is replaced by an alkenyl compound prepared from materials such as dimethylaminoethyl methacrylate, n-butyl bromide, and dimethyl carbonate; in the silicone-acrylic emulsion of Comparative Example 2, the alkenyl rosin compound is prepared from materials such as rosin, oxalyl chloride, and hydroxyethyl methacrylate. Compared with Comparative Example 2, in the silicone-acrylic emulsion of Comparative Example 3, the silicone monomer is γ-methacryloyloxypropyltrimethoxysilane; the silicone-acrylic emulsion in Comparative Example 4 is a commercially available product. The light-transmitting soft stone sheets obtained in Comparative Examples 1-4 have decreased tensile strength, low-temperature impact strength, transmittance, and contact angle data. It can be seen that the arrangement of the light-transmitting soft stone sheet components and their processes of the present invention can promote the comprehensive improvement of its mechanical properties, low-temperature properties, light transmittance, and water resistance.

[0109] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process method article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process method article or device.

[0110] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A process for preparing a light-transmitting soft stone sheet. Features: Including the following processes: Take deionized water, stir and add dispersant, wetting agent, glass powder and aluminum hydroxide, disperse for 2 to 5 minutes; add sodium carboxymethyl cellulose and continue to disperse for 30 minutes; add silicone acrylic emulsion and stir and disperse for 20 minutes; Adjust the color according to the requirements to obtain slurry; Apply on the inside of the mold, dry naturally, demould, and obtain a sheet; The sheet material comprises the following components by weight: 62-68 parts of glass powder, 3-8 parts of aluminum hydroxide, 22-30 parts of silicone-acrylic emulsion, 4-6 parts of deionized water, 0.3-0.6 parts of dispersant, 0.2-0.4 parts of wetting agent, and 0.1-0.5 parts of sodium carboxymethyl cellulose; The silicone-acrylic emulsion is prepared by the following process: Take deionized water, heat it to 57-63°C, add emulsifier, stir and dissolve to obtain emulsifier solution; Take 42% to 50% of the mass of the emulsifier solution, heat it to 80 to 90°C, slowly add 75% to 82% of the mass of octamethylcyclotetrasiloxane and 75% to 82% of the mass of γ-methacryloxypropyltrimethoxysilane, add them all within 30 minutes, keep the temperature and react for 100 to 150 minutes to obtain a silicone pre-emulsion; Take the remaining emulsifier solution, raise the temperature to 58-65°C, slowly add the allyl monomer and the remaining silicone monomer within 30 minutes, and stir rapidly to react for 25-40 minutes to obtain an acrylic pre-emulsion; Slowly add acrylic pre-emulsion and initiator to the silicone pre-emulsion within 60 minutes, and heat to 72-80°C, then to 88-95°C, and stir to react for 100-150 minutes; cool to below 40°C, and adjust the pH of the system to 7-8 with ammonia water to obtain silicone acrylic emulsion; The silicone-acrylic emulsion comprises the following components by weight: 12 to 20 parts of silicone monomer, 80 to 88 parts of allyl monomer, 3.0 to 3.5 parts of emulsifier, 0.8 to 1.5 parts of initiator and 120 parts of deionized water; The allyl monomer comprises the following components: by mass, 50% to 58% methyl methacrylate, 34% to 42% butyl acrylate, 1% to 3% acrylic acid and 3% to 10% alkenyl rosin compound; The organosilicon monomer is a compound of phenylcyclosilane, octamethylcyclotetrasiloxane and γ-methacryloxypropyltrimethoxysilane; The volume ratio of octamethylcyclotetrasiloxane, γ-methacryloxypropyltrimethoxysilane, and phenylcyclosilane is 10:5:(1-3); The phenylcyclosilane is a mixture of one or more of 2,4,6-trimethyl-2,4,6-triphenylcyclotrisiloxane, 2,2,4,6-tetramethyl-4,6-diphenyl-2,4,6-triphenylcyclotrisiloxane, and 2,4,4,6,6-pentamethyl-2-phenylcyclotrisiloxane; The alkenyl rosin compound is prepared by the following process: Take rosin and tetrabutylammonium bromide, mix and dissolve them in anhydrous ethanol, heat to 80-87°C, slowly add epichlorohydrin, add it within 30 minutes, react for 4 hours, and obtain product A; Mix and dissolve product A, 2-(ethylamino)ethyl 2-propenoate and triethylamine in anhydrous ethanol, raise the temperature to 82-90°C, and stir for 5 hours to obtain product B; Mix product B and anhydrous ethanol, add n-butyl bromide, and stir to react for 12 to 48 hours; add dimethyl carbonate, and continue stirring for 1 to 2 hours to obtain an alkenyl rosin compound; The mass ratio of rosin, epichlorohydrin and tetrabutylammonium bromide is 10: (5.2-5.5): (0.15-0.20); The mass ratio of product A, 2-(ethylamino)ethyl acrylate, and triethylamine is 10:(3.7-4.1):(3.9-4.3); The mass ratio of product B, n-butyl bromide and dimethyl carbonate is 10: (2.8-3.1): (1.9-2.1); The glass powder is surface modified by the following specific process: Add a coupling agent to the ethanol aqueous solution and mix for 5 to 12 minutes; add glass powder, heat to 60 to 65° C., and stir for modification for 4 to 5 hours; wash and dry to obtain modified glass powder; The mass ratio of glass powder to coupling agent is 10:(0.5-1.0); the silane coupling agent is 4-trimethoxysilylbutyric acid.

2. A light-transmitting soft stone sheet obtained by the preparation process according to claim 1.