A copolymer TPU suitable for electric vehicle fast charging cable and preparation method thereof

By using modified TPU and nanowire deposition technology in cables for electric vehicle charging piles, the mesh structure is formed, which solves the problem of insufficient strength and wear resistance of cable materials, and significantly improves the performance and safety of cables.

CN118652540BActive Publication Date: 2024-12-06SHANDONG LEAD CHEM CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410790004.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-19
Publication Date
2024-12-06
Estimated Expiration
2044-06-19

AI Technical Summary

Technical Problem

The existing cables for electric vehicle charging piles are worn and safe due to their bulky and easy to drag, and are not well-behaved.

Method used

Using a copolymerized TPU composed of TPU, ethylene-acrylate copolymer, compatible agent, composite filler, halogen-free flame retardant, lubricant and antioxidant, the nano-silica modification treatment and alumina nanowire deposition Form a mesh structure to enhance the cross-linking density and wear resistance of the substrate.

Benefits of technology

It significantly improves the strength and wear resistance of cable materials, reduces wear risks, and enhances the performance and safety of cables.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004899732210000101
    Figure BDA0004899732210000101
  • Figure BDA0004899732210000111
    Figure BDA0004899732210000111
Patent Text Reader

Abstract

The invention discloses a copolymer TPU suitable for a cable for fast charging of electric vehicles and a preparation method thereof, which is made of the following raw materials in parts by weight: 60-100 parts of TPU, 5-15 parts of ethylene-acrylate copolymer, 2-7 parts of compatibilizer, 8-15 parts of treatment agent, 10-18 parts of composite filler, 15-26 parts of halogen-free flame retardant, 1-2 parts of lubricant, and 1-2 parts of antioxidant. The copolymer TPU substrate in the present invention can form a mesh structure by introducing the prepared composite filler into the copolymer TPU substrate, effectively increasing the crosslinking density inside the copolymer TPU substrate, and at the same time, spraying the prepared treatment agent on the masterbatch just extruded from the twin-screw extruder, the masterbatch shrinks rapidly after being cooled, thereby increasing the density of the masterbatch, and at the same time, the sprayed treatment agent will penetrate into the masterbatch through the hole defect, and form a reinforcing layer in the masterbatch, thereby improving the hardness and wear resistance of the masterbatch, so that the copolymer TPU substrate has more excellent strength and wear resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of new materials, and in particular to a copolymer TPU suitable for a cable for fast charging of electric vehicles and a preparation method thereof. Background Art

[0002] Thermoplastic polyurethane elastomer, also known as thermoplastic polyurethane rubber, or TPU for short, is a type of elastomer that can be plasticized by heating and dissolved by specific solvents. It has many excellent properties, such as high modulus, high strength, excellent wear resistance, chemical corrosion resistance, hydrolysis resistance, high and low temperature resistance, and mold resistance. These good properties make thermoplastic polyurethane widely used in many fields such as footwear, cables, clothing, automobiles, medicine and health, pipes, films and sheets. With the rapid development of new energy vehicles, charging piles have become an indispensable infrastructure. However, due to the long charging and discharging process of new energy vehicles and high current intensity, the cables are frequently used and exposed outdoors for a long time, so their safety has become a focus of attention.

[0003] For example, the invention patent with announcement number CN106633588A discloses a cable material for electric vehicle charging piles and a preparation method thereof, wherein the components include: SEBS (styrene-based elastomer), nitrile rubber, TPU thermoplastic elastomer, high-density polyethylene, isophthalic polyimide, low-hydrated zinc borate, compatibilizer, DMDPB (2,3-dimethyl-2,3-diphenylbutane); the special cable material for electric vehicle charging piles has the advantages of good flame retardancy, low amount of flame retardant addition, heat resistance, low toxicity and environmental protection of flame retardants, low cost and easy availability, low smoke, good mechanical properties, etc.; however, since the charging cable is very bulky, the user will drag the cable when charging the car, causing the charging cable to rub against the ground, and the outer surface is easily worn and cracked, posing a safety hazard. Summary of the invention

[0004] The object of the present invention is to provide a copolymer TPU suitable for electric vehicle fast charging cables and a preparation method thereof.

[0005] To achieve the above object, the present invention provides the following technical solutions:

[0006] A copolymer TPU suitable for a cable for fast charging of an electric vehicle is prepared from the following raw materials in parts by weight: 60-100 parts of TPU, 5-15 parts of ethylene-acrylate copolymer, 2-7 parts of a compatibilizer, 8-15 parts of a treating agent, 10-18 parts of a composite filler, 15-26 parts of a halogen-free flame retardant, 1-2 parts of a lubricant, and 1-2 parts of an antioxidant.

[0007] As a further preferred embodiment of the present invention, the TPU is one or more of polyether TPU, polyester TPU, and polycaprolactone TPU;

[0008] The ethylene-acrylate copolymer is one or more of ethylene-methyl methacrylate copolymer, ethylene-methyl acrylate copolymer, and ethylene-ethyl acrylate copolymer;

[0009] The compatibilizer is one or more of ethylene-methyl acrylate-maleic anhydride copolymer, POE grafted maleic anhydride copolymer (POE is ethylene-1-octene copolymer), and SEBS grafted maleic anhydride copolymer (SEBS is styrene-ethylene-butylene-styrene block copolymer);

[0010] The lubricant is one or more of calcium stearate, polyethylene wax, and silicone powder;

[0011] The halogen-free flame retardant is one or two of melamine polyphosphate and melamine cyanurate;

[0012] The antioxidant is one or more of antioxidant 1035, antioxidant 168, antioxidant 1098, and antioxidant 330.

[0013] As a further preferred embodiment of the present invention, the preparation method of the treatment agent is as follows:

[0014] 1) Weigh nano-silica and put it into a drying oven, dry it at 100-120° C. for 10-30 min, add silane coupling agent KH550 to deionized water, and adjust the pH value to 4-5 with hydrochloric acid. After hydrolysis for 60-80 min, add the dried nano-silica to the solution, stir it with magnetic force at 80-85° C. until the solution is completely volatilized, wash the remaining solid repeatedly with anhydrous ethanol and dry it to obtain modified silica;

[0015] 2) Weigh silane coupling agent KH550, methyltriethoxysilane and nano-silica sol, adjust the pH to 1-3 with hydrochloric acid, stir magnetically in a water bath at 40-45° C. for 2-5 h, and after sufficient hydrolysis, heat to 80-86° C., continue to react for 2-5 h, and then cool in an ice water bath, and add 1-benzyl-2-methylimidazole dropwise under stirring at 300-500 r / min, continue to react for 1-3 h, then add a mixed solvent, and then add modified silica and aluminum acetylacetonate, react for 30-50 min, and the treating agent can be obtained.

[0016] As a further preferred embodiment of the present invention, in step 1), the usage ratio of the nano-silica, the silane coupling agent KH550, and the deionized water is (5-10) g: (1-2) g: (10-16) mL.

[0017] As a further preferred embodiment of the present invention, in step 2), the usage ratio of the silane coupling agent KH550, methyltriethoxysilane, nano-silica sol, 1-benzyl-2-methylimidazole, mixed solvent, modified silica, and aluminum acetylacetonate is (2-5) g: (4-12) g: (12-20) g: (2-3) mL: (2-4) mL: (2-3) g: (1-2) g;

[0018] The mixed solvent is composed of methanol, ethanol, isopropanol and ethylene glycol monomethyl ether in a volume ratio of (5-7):13:(6-9):1.

[0019] As a further preferred embodiment of the present invention, the preparation method of the composite filler is as follows:

[0020] 1) Weighing aluminum oxide nanopowder, adding it to deionized water, magnetically stirring for 30-50 minutes, then adding glacial acetic acid, stirring thoroughly, transferring it to a reaction kettle, sealing it and placing it in a drying oven, reacting it at 230-240° C. for 5-8 hours, and after the reaction is completed, naturally cooling it to room temperature, repeatedly washing it with deionized water and drying it to obtain aluminum oxide nanowires;

[0021] 2) Measure glycerol and anhydrous ethanol, stir and mix thoroughly, add tetrabutyl titanate, continue stirring for 5-10 minutes, then add alumina nanowires, disperse evenly, transfer to an autoclave, react at 180-190° C. for 24-30 hours, and after the reaction is completed, naturally cool to room temperature, wash the product repeatedly with deionized water and anhydrous ethanol alternately, and then dry to obtain pretreated alumina nanowires;

[0022] 3) Weigh cobalt nitrate and dissolve it in pure water, then add the pretreated alumina nanowires, stir thoroughly and seal, place in an ultrasonic cleaner, treat at 50-56° C. for 60-80 min, wash the obtained product repeatedly with anhydrous ethanol, dry at 60-80° C. for 12-15 h, then heat to 470-500° C. in air, heat and calcine for 90-120 min, and cool naturally to room temperature to obtain a composite filler.

[0023] As a further preferred embodiment of the present invention, in step 1), the usage ratio of the aluminum oxide nanopowder, deionized water and glacial acetic acid is (37-45) g: (400-700) mL: (20-30) g.

[0024] As a further preferred embodiment of the present invention, in step 2), the usage ratio of glycerol, anhydrous ethanol, tetrabutyl titanate and alumina nanowires is (20-30) mL: (60-90) mL: (2-3) g: (8-12) g.

[0025] As a further preferred embodiment of the present invention, in step 3), the ratio of the amount of cobalt nitrate, pure water, and pretreated alumina nanowires is (2-5) g: (100-180) mL: (1-3) g;

[0026] The heating rate is 5-8°C / min.

[0027] A method for preparing a copolymer TPU suitable for a cable for fast charging of electric vehicles comprises the following steps:

[0028] Weigh each component according to weight proportion, mix ethylene-acrylate copolymer, compatibilizer, composite filler, halogen-free flame retardant, lubricant and antioxidant thoroughly to obtain a mixture, dry TPU at 80-90°C for 5-7h, mix it thoroughly with the mixture, extrude it into granules through a twin-screw extruder, the extrusion temperature of the extruder is 180-190°C, and spray the treatment agent evenly on the surface of the masterbatch at the extrusion port of the extruder, keep the temperature in a 40-50°C oven for 30-50min, then raise the temperature to 80-85°C, and cure it at the constant temperature for 3-5h.

[0029] Compared with the prior art, the present invention has the following beneficial effects:

[0030] In the present invention, alumina gel is prepared by a hydrothermal method to obtain alumina nanowires, and alumina nanowires are used as a matrix material. A flaky titanium dioxide nanomaterial doped with metal cobalt is deposited on the alumina nanowires by a hydrothermal method, and then calcined at a high temperature to obtain a composite filler. The doped metal cobalt forms protruding nanoparticles on the surface of the flaky titanium dioxide nanomaterial, which increases the surface roughness of the titanium dioxide nanomaterial, so that the titanium dioxide nanomaterial can be firmly bonded to the alumina nanowires after being deposited on the alumina nanowires. The composite filler is introduced into the copolymer In the TPU substrate, a network structure can be formed by the mutual entanglement of nanowires, which effectively increases the cross-linking density inside the copolymer TPU substrate and enhances its strength, so that it can better resist external forces and is not prone to problems such as wear and cracking, thereby significantly improving the performance of the copolymer TPU substrate. At the same time, the deposited flaky titanium dioxide material can be better combined together to form connecting nodes through the mutual intercalation and stacking between the layers, which helps to enhance the stability of the network structure and enable it to better play an enhancing effect in the copolymer TPU substrate.

[0031] At the same time, in order to further improve the wear resistance of the copolymer TPU substrate and reduce its wear, in the present invention, the nano-silicon dioxide is modified by a silane coupling agent, and an amino group is introduced on its surface, thereby improving its dispersibility in the polymer. Then, the epoxy hydrocarbon silicone resin is prepared by a sol-gel method using nano-silicon dioxide sol, methyltriethoxysilane and KH-550 as raw materials, and 1-benzyl-2-methylimidazole, aluminum acetylacetonate, modified silicon dioxide and a mixed solvent are added to obtain a treating agent. The treating agent is sprayed on the masterbatch just extruded from the twin-screw extruder. Since the temperature of the masterbatch is high at this time and there are certain hole defects on the surface, the sprayed treating agent can play a cooling role on the one hand, so that the masterbatch shrinks rapidly after being cooled, thereby increasing the density of the masterbatch. At the same time, the sprayed treating agent will penetrate into the masterbatch through the hole defects and form a reinforcing layer in the masterbatch, thereby improving the hardness and wear resistance of the masterbatch, thereby further reducing the wear of the copolymer TPU substrate.

[0032] The copolymer TPU substrate of the present invention can form a network structure by introducing the prepared composite filler into the copolymer TPU substrate through the mutual entanglement of nanowires, effectively increasing the crosslinking density inside the copolymer TPU substrate and enhancing its strength. At the same time, the prepared treatment agent is sprayed on the masterbatch just extruded from the twin-screw extruder, so that the masterbatch shrinks rapidly after cooling, thereby increasing the density of the masterbatch. At the same time, the sprayed treatment agent penetrates into the masterbatch through the hole defects and forms a reinforcement layer in the masterbatch, thereby improving the hardness and wear resistance of the masterbatch, thereby further reducing the wear of the copolymer TPU substrate, so that the copolymer TPU substrate has more excellent strength and wear resistance. DETAILED DESCRIPTION

[0033] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0034] In the embodiment of the present invention, TPU is polyether TPU; ethylene-acrylate copolymer is ethylene-methyl methacrylate copolymer; compatibilizer is ethylene-methyl acrylate-maleic anhydride copolymer; halogen-free flame retardant is melamine polyphosphate; lubricant is calcium stearate; antioxidant is antioxidant 1035.

[0035] Example 1

[0036] A copolymer TPU suitable for a cable for fast charging of electric vehicles, made from the following raw materials in parts by weight: 60 parts of TPU, 5 parts of ethylene-acrylate copolymer, 2 parts of a compatibilizer, 8 parts of a treating agent, 10 parts of a composite filler, 15 parts of a halogen-free flame retardant, 1 part of a lubricant, and 1 part of an antioxidant;

[0037] The preparation method of the copolymerized TPU specifically comprises the following steps:

[0038] Weigh each component according to weight proportion, mix ethylene-acrylate copolymer, compatibilizer, composite filler, halogen-free flame retardant, lubricant and antioxidant thoroughly to obtain a mixture, dry TPU at 80°C for 5h, mix it thoroughly with the mixture, extrude it into granules through a twin-screw extruder, the extrusion temperature of the extruder is 180°C, and spray the treating agent evenly on the surface of the masterbatch at the extrusion port of the extruder, keep the temperature in an oven at 40°C for 30min, then raise the temperature to 80°C and cure it at the constant temperature for 3h.

[0039] The preparation method of the treatment agent is as follows:

[0040] 1) Weigh 5 g of nano-silica and put it into a drying oven, dry it at 100° C. for 10 min, add 1 g of silane coupling agent KH550 to 10 mL of deionized water, and adjust the pH value to 4 with hydrochloric acid. After hydrolysis for 60 min, add the dried nano-silica to the solution, stir it with a magnetic force at 80° C. until the solution is completely volatilized, wash the remaining solid repeatedly with anhydrous ethanol and dry it to obtain modified silica;

[0041] 2) Weigh 2g of silane coupling agent KH550, 4g of methyltriethoxysilane and 12g of nano-silica sol, adjust the pH to 1 with hydrochloric acid, stir magnetically in a 40°C water bath for 2h, and after sufficient hydrolysis, heat to 80°C, continue to react for 2h, then cool in an ice water bath, and add 2mL of 1-benzyl-2-methylimidazole dropwise under stirring at 300r / min, continue to react for 1h, then add 2mL of a mixed solvent composed of methanol, ethanol, isopropanol and ethylene glycol monomethyl ether in a volume ratio of 5:13:6:1, then add 2g of modified silica and 1g of aluminum acetylacetonate, react for 30-50min, and the treating agent can be obtained.

[0042] Among them, the preparation method of the composite filler is as follows:

[0043] 1) Weigh 37 g of alumina nanopowder, add it to 400 mL of deionized water, stir it magnetically for 30 min, then add 20 g of glacial acetic acid, stir it thoroughly, transfer it to a reactor, seal it and put it in a drying oven, react it at 230 ° C for 5 h, after the reaction is completed, cool it naturally to room temperature, wash it repeatedly with deionized water and dry it to obtain alumina nanowires;

[0044] 2) 20 mL of glycerol and 60 mL of anhydrous ethanol were measured, and after being fully stirred and mixed, 2 g of tetrabutyl titanate was added, and stirring was continued for 5 min, and then 8 g of alumina nanowires were added. After being evenly dispersed, the mixture was transferred to an autoclave and reacted at 180° C. for 24 h. After the reaction was completed, the mixture was naturally cooled to room temperature, and the product was repeatedly washed with deionized water and anhydrous ethanol alternately and then dried to obtain pretreated alumina nanowires;

[0045] 3) Weigh 2 g of cobalt nitrate and dissolve it in 100 mL of pure water, then add 1 g of pretreated alumina nanowires, stir thoroughly and seal, place in an ultrasonic cleaner, treat at 50° C. for 60 min, wash the obtained product repeatedly with anhydrous ethanol, dry at 60° C. for 12 h, then heat to 470° C. in air at 5° C. / min, heat and calcine for 90 min, and cool naturally to room temperature to obtain a composite filler.

[0046] Example 2

[0047] A copolymer TPU suitable for a cable for fast charging of electric vehicles, made from the following raw materials in parts by weight: 80 parts of TPU, 10 parts of ethylene-acrylate copolymer, 5 parts of a compatibilizer, 12 parts of a treating agent, 15 parts of a composite filler, 23 parts of a halogen-free flame retardant, 1.5 parts of a lubricant, and 1.5 parts of an antioxidant;

[0048] The preparation method of the copolymerized TPU specifically comprises the following steps:

[0049] Weigh each component according to weight proportion, mix ethylene-acrylate copolymer, compatibilizer, composite filler, halogen-free flame retardant, lubricant and antioxidant thoroughly to obtain a mixture, dry TPU at 85°C for 6h, and then mix it thoroughly with the mixture, extrude and granulate it through a twin-screw extruder. The extrusion temperature of the extruder is 186°C, and the treating agent is evenly sprayed on the surface of the masterbatch at the extrusion port of the extruder, and kept at a constant temperature in an oven at 47°C for 40min, then raised to 83°C, and cured at a constant temperature for 4h.

[0050] The preparation method of the treatment agent is as follows:

[0051] 1) Weigh 7 g of nano-silica and put it into a drying oven, dry it at 110° C. for 20 min, add 1.5 g of silane coupling agent KH550 into 13 mL of deionized water, and adjust the pH value to 4.5 with hydrochloric acid. After hydrolysis for 70 min, add the dried nano-silica to the solution, stir it with a magnetic force at 82° C. until the solution is completely volatilized, wash the remaining solid repeatedly with anhydrous ethanol and dry it to obtain modified silica;

[0052] 2) Weigh 3g of silane coupling agent KH550, 7g of methyltriethoxysilane and 16g of nano-silica sol, adjust the pH to 2 with hydrochloric acid, stir magnetically in a 43°C water bath for 3h, and after sufficient hydrolysis, heat to 85°C, continue to react for 3h, then cool in an ice water bath, and add 3mL of 1-benzyl-2-methylimidazole dropwise under stirring at 400r / min, continue to react for 2h, then add 3mL of a mixed solvent composed of methanol, ethanol, isopropanol and ethylene glycol monomethyl ether in a volume ratio of 6:13:7:1, add 2.5g of modified silica and 1.5g of aluminum acetylacetonate, react for 40min, and the treating agent can be obtained.

[0053] Among them, the preparation method of the composite filler is as follows:

[0054] 1) Weigh 42 g of alumina nanopowder, add it to 600 mL of deionized water, stir it magnetically for 40 min, then add 25 g of glacial acetic acid, stir it thoroughly, transfer it to a reactor, seal it and put it in a drying oven, react it at 235 ° C for 7 h, after the reaction is completed, cool it naturally to room temperature, wash it repeatedly with deionized water and dry it to obtain alumina nanowires;

[0055] 2) 25 mL of glycerol and 80 mL of anhydrous ethanol were weighed, and after being fully stirred and mixed, 2.5 g of tetrabutyl titanate was added, and stirring was continued for 7 min, and then 10 g of alumina nanowires were added. After being evenly dispersed, the mixture was transferred to an autoclave and reacted at 185° C. for 27 h. After the reaction was completed, the mixture was naturally cooled to room temperature, and the product was washed alternately with deionized water and anhydrous ethanol and then dried to obtain pretreated alumina nanowires;

[0056] 3) Weigh 3 g of cobalt nitrate and dissolve it in 150 mL of pure water, then add 2 g of pretreated alumina nanowires, stir thoroughly and seal, place in an ultrasonic cleaner, treat at 53 ° C for 70 min, wash the obtained product repeatedly with anhydrous ethanol, dry at 70 ° C for 13 h, then heat to 490 ° C in air at 6 ° C / min, heat and calcine for 110 min, and cool naturally to room temperature to obtain a composite filler.

[0057] Example 3

[0058] A copolymer TPU suitable for a cable for fast charging of electric vehicles, made from the following raw materials in parts by weight: 100 parts of TPU, 15 parts of ethylene-acrylate copolymer, 7 parts of a compatibilizer, 15 parts of a treating agent, 18 parts of a composite filler, 26 parts of a halogen-free flame retardant, 2 parts of a lubricant, and 2 parts of an antioxidant;

[0059] The preparation method of the copolymerized TPU specifically comprises the following steps:

[0060] Weigh each component according to weight proportion, mix ethylene-acrylate copolymer, compatibilizer, composite filler, halogen-free flame retardant, lubricant and antioxidant thoroughly to obtain a mixture, dry TPU at 90°C for 7h, mix it thoroughly with the mixture, extrude it into granules through a twin-screw extruder, the extrusion temperature of the extruder is 190°C, and spray the treating agent evenly on the surface of the masterbatch at the extrusion port of the extruder, keep the temperature in a 50°C oven for 50min, then raise the temperature to 85°C and cure it at the constant temperature for 5h.

[0061] The preparation method of the treatment agent is as follows:

[0062] 1) Weigh 10 g of nano-silica and put it into a drying oven, dry it at 120° C. for 30 min, add 2 g of silane coupling agent KH550 into 16 mL of deionized water, and adjust the pH value to 5 with hydrochloric acid. After hydrolysis for 80 min, add the dried nano-silica to the solution, stir it with a magnetic force at 85° C. until the solution is completely volatilized, wash the remaining solid repeatedly with anhydrous ethanol and dry it to obtain modified silica;

[0063] 2) Weigh 5g of silane coupling agent KH550, 12g of methyltriethoxysilane and 20g of nano-silica sol, adjust the pH to 3 with hydrochloric acid, stir magnetically in a 45°C water bath for 5h, and after sufficient hydrolysis, heat to 86°C, continue to react for 5h, then cool in an ice water bath, and add 3mL of 1-benzyl-2-methylimidazole dropwise under stirring at 500r / min, continue to react for 3h, then add 4mL of a mixed solvent composed of methanol, ethanol, isopropanol and ethylene glycol monomethyl ether in a volume ratio of 7:13:9:1, then add 3g of modified silica and 2g of aluminum acetylacetonate, react for 50min, and the treating agent can be obtained.

[0064] Among them, the preparation method of the composite filler is as follows:

[0065] 1) Weigh 45 g of alumina nanopowder, add it to 700 mL of deionized water, stir it magnetically for 50 min, then add 30 g of glacial acetic acid, stir it thoroughly, transfer it to a reactor, seal it and put it in a drying oven, react it at 240 ° C for 8 h, after the reaction is completed, cool it naturally to room temperature, wash it repeatedly with deionized water and dry it to obtain alumina nanowires;

[0066] 2) 30 mL of glycerol and 90 mL of anhydrous ethanol were measured, and after being fully stirred and mixed, 3 g of tetrabutyl titanate was added, and stirring was continued for 10 min, and then 12 g of alumina nanowires were added. After being evenly dispersed, the mixture was transferred to an autoclave and reacted at 190° C. for 30 h. After the reaction was completed, the mixture was naturally cooled to room temperature, and the product was repeatedly washed with deionized water and anhydrous ethanol alternately and then dried to obtain pretreated alumina nanowires;

[0067] 3) Weigh 5 g of cobalt nitrate and dissolve it in 180 mL of pure water, then add 3 g of pretreated alumina nanowires, stir thoroughly and seal, place in an ultrasonic cleaner, treat at 56 ° C for 80 min, wash the obtained product repeatedly with anhydrous ethanol, dry at 80 ° C for 15 h, then heat to 500 ° C in air at 8 ° C / min, heat and calcine for 120 min, and cool naturally to room temperature to obtain a composite filler.

[0068] Comparative Example 1: This comparative example is basically the same as Example 1, except that it does not contain a composite filler.

[0069] Comparative Example 2: This comparative example is basically the same as Example 1, except that step 1) is omitted in the preparation of the composite filler.

[0070] Comparative Example 3: This comparative example is basically the same as Example 1, except that step 2) is omitted in the preparation of the composite filler.

[0071] Comparative Example 4: This comparative example is substantially the same as Example 1, except that it does not contain a treating agent.

[0072] Comparative Example 5: This comparative example is basically the same as Example 1, except that step 1) is omitted in the preparation of the treatment agent.

[0073] Test experiment:

[0074] The copolymer TPU samples were respectively processed and prepared by the methods provided in Examples 1-3 and Comparative Examples 1-5, and then the wear resistance was tested. The wear resistance of the samples in Examples 1-3 and Comparative Examples 1-5 was tested according to the test method described in GB-9867-2008, and their relative volume wear was tested. The test results are shown in Table 1.

[0075] Table 1

[0076]

[0077]

[0078] It can be seen from Table 1 that the copolymer TPU in the present invention has excellent wear resistance. Applying it to cable materials can significantly reduce the wear of the cable materials and improve the performance of the cable materials.

[0079] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.

Claims

1. A copolymer TPU suitable for electric vehicle fast charging cables, characterized in that: It is made of the following raw materials in parts by weight: 60-100 parts of TPU, 5-15 parts of ethylene-acrylate copolymer, 2-7 parts of compatibilizer, 8-15 parts of treatment agent, 10-18 parts of composite filler, 15-26 parts of halogen-free flame retardant, 1-2 parts of lubricant, and 1-2 parts of antioxidant; The preparation method of the treatment agent is as follows: 1) Weigh nano-silica and put it into a drying oven, dry it at 100-120°C for 10-30 minutes, add silane coupling agent KH550 to deionized water, and adjust the pH value to 4-5 with hydrochloric acid. After hydrolysis for 60-80 minutes, add the dried nano-silica to the solution, stir it with magnetic force at 80-85°C until the solution is completely volatilized, wash the remaining solid repeatedly with anhydrous ethanol and dry it to obtain modified silica; 2) Weigh silane coupling agent KH550, methyltriethoxysilane and nano-silica sol, adjust the pH to 1-3 with hydrochloric acid, stir magnetically in a water bath at 40-45°C for 2-5h, and after sufficient hydrolysis, heat to 80-86°C, continue to react for 2-5h, and then cool in an ice water bath, and add 1-benzyl-2-methylimidazole dropwise under stirring at 300-500r / min, continue to react for 1-3h, then add a mixed solvent, and then add modified silica and aluminum acetylacetonate, react for 30-50min, and then obtain a treating agent; The preparation method of the composite filler is as follows: 1) Weigh alumina nanopowder, add it to deionized water, stir it magnetically for 30-50 minutes, then add glacial acetic acid, stir it thoroughly, transfer it to a reactor, seal it and put it in a drying oven, react it at 230-240°C for 5-8 hours, and after the reaction is completed, cool it naturally to room temperature, wash it repeatedly with deionized water and dry it to obtain alumina nanowires; 2) Measure glycerol and anhydrous ethanol, stir and mix thoroughly, then add tetrabutyl titanate, continue stirring for 5-10 minutes, then add alumina nanowires, disperse evenly, transfer to an autoclave, react at 180-190°C for 24-30 hours, and after the reaction is completed, naturally cool to room temperature, wash the product repeatedly with deionized water and anhydrous ethanol alternately, and then dry it to obtain pretreated alumina nanowires; 3) Weigh cobalt nitrate and dissolve it in pure water, then add the pretreated alumina nanowires, stir thoroughly and seal, place in an ultrasonic cleaner, treat at 50-56°C for 60-80min, wash the obtained product repeatedly with anhydrous ethanol, dry at 60-80°C for 12-15h, then heat to 470-500°C in air, heat and calcine for 90-120min, and cool naturally to room temperature to obtain a composite filler.

2. A copolymer TPU suitable for electric vehicle fast charging cable according to claim 1, characterized in that: The TPU is one or more of polyether TPU, polyester TPU, and polycaprolactone TPU; The ethylene-acrylate copolymer is one or more of ethylene-methyl methacrylate copolymer, ethylene-methyl acrylate copolymer, and ethylene-ethyl acrylate copolymer; The compatibilizer is one or more of ethylene-methyl acrylate-maleic anhydride copolymer, POE grafted maleic anhydride copolymer, and SEBS grafted maleic anhydride copolymer; The lubricant is one or more of calcium stearate, polyethylene wax, and silicone powder; The halogen-free flame retardant is one or two of melamine polyphosphate and melamine cyanurate; The antioxidant is one or more of antioxidant 1035, antioxidant 168, antioxidant 1098, and antioxidant 330.

3. A copolymer TPU suitable for electric vehicle fast charging cable according to claim 1, characterized in that: In step 1), the usage ratio of the nano-silica, the silane coupling agent KH550, and the deionized water is (5-10) g: (1-2) g: (10-16) mL.

4. The copolymer TPU suitable for electric vehicle fast charging cable according to claim 1, characterized in that: In step 2), the usage ratio of the silane coupling agent KH550, methyltriethoxysilane, nano-silica sol, 1-benzyl-2-methylimidazole, mixed solvent, modified silica, and aluminum acetylacetonate is (2-5) g: (4-12) g: (12-20) g: (2-3) mL: (2-4) mL: (2-3) g: (1-2) g; The mixed solvent is composed of methanol, ethanol, isopropanol and ethylene glycol monomethyl ether in a volume ratio of (5-7):13:(6-9):

1.

5. The copolymer TPU suitable for electric vehicle fast charging cable according to claim 1, characterized in that: In step 1), the ratio of the aluminum oxide nanopowder, deionized water and glacial acetic acid is (37-45) g: (400-700) mL: (20-30) g.

6. The copolymer TPU suitable for electric vehicle fast charging cable according to claim 1, characterized in that: In step 2), the usage ratio of glycerol, anhydrous ethanol, tetrabutyl titanate, and aluminum oxide nanowires is (20-30) mL: (60-90) mL: (2-3) g: (8-12) g.

7. The copolymer TPU suitable for electric vehicle fast charging cable according to claim 1, characterized in that: In step 3), the ratio of the cobalt nitrate, pure water, and pretreated alumina nanowires is (2-5) g: (100-180) mL: (1-3) g; The heating rate is 5-8°C / min.

8. A method for preparing a copolymer TPU suitable for electric vehicle fast charging cables according to any one of claims 1 to 7, characterized in that: The specific steps include: Weigh each component according to weight proportion, mix ethylene-acrylate copolymer, compatibilizer, composite filler, halogen-free flame retardant, lubricant and antioxidant thoroughly to obtain a mixture, dry TPU at 80-90°C for 5-7h, mix it thoroughly with the mixture, extrude it into granules through a twin-screw extruder, the extrusion temperature of the extruder is 180-190°C, and spray the treatment agent evenly on the surface of the masterbatch at the extrusion port of the extruder, keep the temperature in a 40-50°C oven for 30-50min, then raise the temperature to 80-85°C, and cure it at the constant temperature for 3-5h.