A regenerated composite polymer material and its preparation method and application

By hydrolyzing the used polyamide and reacting with vinyl phosphonic acid, and then mixing it with modified glass fiber and azobisisobutyronitrile, a regenerated composite polymer material with excellent flame retardant, tensile resistance and waterproofing properties are prepared, and the solution is to The waste of waste polyamide resources and environmental pollution have been solved, and efficient material recycling and reuse has been achieved.

CN118652543BActive Publication Date: 2024-12-06NANTONG BEIJIA PLASTIC IND CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410896297.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-04
Publication Date
2024-12-06
Estimated Expiration
2044-07-04

Smart Images

  • Figure BDA0004929064910000031
    Figure BDA0004929064910000031
  • Figure BDA0004929064910000032
    Figure BDA0004929064910000032
  • Figure BDA0004929064910000033
    Figure BDA0004929064910000033
Patent Text Reader

Abstract

The invention discloses a regenerated composite polymer material and a preparation method and application thereof, and relates to the technical field of polymer materials. When preparing the regenerated composite polymer material, the present invention reacts 3-aminopropyl pentamethyldisiloxane and tetramethyltetravinylcyclotetrasiloxane to obtain single-end amino polyvinylsiloxane; then reacts glass fiber with 5,6-epoxyhexyltriethoxysilane and single-end amino polyvinylsiloxane to obtain modified glass fiber; hydrolyzes waste polyamide 66 to obtain regenerated hexamethylenediamine and regenerated adipic acid; reacts regenerated hexamethylenediamine, regenerated adipic acid and vinylphosphonic acid to obtain regenerated polyamide; regenerated polyamide, modified glass fiber and azobisisobutyronitrile are mixed and extruded to prepare a regenerated composite polymer material. The regenerated composite polymer material prepared by the present invention has excellent flame retardant properties, tensile resistance and waterproof properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer materials, in particular to a regenerated composite polymer material and a preparation method and application thereof. Background Art

[0002] Materials science is constantly changing and developing as science and technology advances. The four major materials, metals, inorganic non-metals, polymers and composite materials, play a pivotal role in the development of science and technology and even society. Polymer materials are mainly divided into rubber, fiber and plastic. Among them, plastics have become one of the indispensable materials in the new technology industry because of their light weight, good insulation, good corrosion resistance, good specific strength and toughness, good fatigue resistance, and various molding methods. Engineering plastics mainly include polycarbonate, polyamide, polyoxymethylene, polyphenylene ether, polyester, etc. Among them, polyamide ranks first in production among the five major engineering plastics.

[0003] The increase in production is accompanied by the generation of a large amount of waste. With the increase in environmental awareness, social themes such as sustainable development and green circular economy have become more popular, and people are paying more and more attention to the recycling of waste. Waste polyamide is mainly post-industrial waste and post-consumer waste. At present, most waste is disposed of by landfill and incineration, which not only wastes resources but also easily pollutes the environment. Therefore, the present invention prepares a recycled composite polymer material with excellent flame retardant properties, tensile strength and waterproof properties. Summary of the invention

[0004] The purpose of the present invention is to provide a regenerated composite polymer material and a preparation method and application thereof, so as to solve the problems existing in the prior art.

[0005] In order to solve the above technical problems, the present invention provides the following technical solutions:

[0006] A regenerated composite polymer material is prepared by mixing regenerated polyamide, modified glass fiber and azobisisobutyronitrile and then extruding the mixture.

[0007] As an optimization, the regenerated polyamide is obtained by reacting regenerated hexamethylenediamine and regenerated adipic acid obtained by hydrolyzing waste polyamide 66 with vinylphosphonic acid.

[0008] As an optimization, the waste polyamide 66 is one or more of wastes such as waste polyamide 66 fibers, waste polyamide 66 films, and waste polyamide 66 fragments.

[0009] As an optimization, the modified glass fiber is obtained by reacting glass fiber with 5,6-epoxyhexyltriethoxysilane and single-end amino polyvinyl siloxane in sequence.

[0010] As an optimization, the single-end amino polyvinyl siloxane is obtained by reacting 3-aminopropyl pentamethyl disiloxane and tetramethyltetravinylcyclotetrasiloxane.

[0011] A method for preparing a regenerated composite polymer material comprises the following preparation steps:

[0012] (1) 3-aminopropyl pentamethyldisiloxane and tetramethyltetravinylcyclotetrasiloxane are mixed in a mass ratio of 1:(4-6), stirred at 65N75°C and 100-200 rpm for 20-30 min, trifluoromethylsulfonic acid in an amount of 0.01-0.02 times the mass of 3-aminopropyl pentamethyldisiloxane is added, stirring is continued for 5-7 h, anhydrous sodium carbonate is added to adjust the pH to 6-7, and then filtered, and distilled at 105-115°C and 0.1-0.3 MPa for 1-2 h to obtain single-end amino polyvinylsiloxane;

[0013] (2) 5,6-epoxyhexyltriethoxysilane and anhydrous ethanol are mixed in a mass ratio of 1:(14-16), and ultrasonically dispersed for 20-30 minutes to obtain a 5,6-epoxyhexyltriethoxysilane alcoholysis solution; the glass fiber is soaked in the 5,6-epoxyhexyltriethoxysilane alcoholysis solution for 3-5 hours, then taken out, washed with deionized water and anhydrous ethanol for 3-5 times respectively, and dried at 60N70°C for 11-13 hours to obtain Pre-modified glass fiber; mixing pre-modified glass fiber, single-end amino polyvinyl siloxane, glacial acetic acid and isopropyl alcohol in a mass ratio of 1: (2-3): (0.01-0.03): (2.8-3.2), stirring at 82-84° C. and 100-200 rpm for 11-13 hours, naturally cooling to room temperature and filtering, washing with deionized water for 3N5 times, and drying at 65N75° C. for 8-10 hours to obtain modified glass fiber;

[0014] (3) Soaking the waste polyamide 66 in a sodium hydroxide solution with a mass fraction of 2-4% at 75-85° C. for 1-3 h, washing it with deionized water for 3-5 times, drying it at 75-85° C. for 23-25 ​​h, and then crushing it to a particle size of less than 1 mm to obtain a polyamide powder; mixing the polyamide powder, deionized water and a sulfuric acid solution with a mass fraction of 36-38% in a molar ratio of 1:(29-31):(2-3), stirring it at 105-115° C. and 100-200 rpm for 4-6 h, naturally cool to room temperature and then filter, take the filtrate and add calcium hydroxide 10 to 12 times the mass of the polyamide powder, stir at 95 to 105°C and 200 to 300 rpm for 1 to 3 hours, and distill under reduced pressure to obtain regenerated hexamethylenediamine; dry the filter residue at 75 to 85°C for 9 to 11 hours, add deionized water 16 to 18 times the mass of the polyamide powder, stir at 85 to 95°C and 100 to 200 rpm for 2 to 3 hours, filter while hot, let the filtrate stand and cool to room temperature, precipitate recrystallization, and obtain regenerated adipic acid;

[0015] (4) Regenerated hexamethylenediamine, vinylphosphonic acid, regenerated adipic acid and deionized water were mixed in a molar ratio of 1: (0.2-0.4): (0.4-0.6): (5-7), and the regenerated adipic acid was added to adjust the pH of the solution to 7.3-7.5. The mixture was stirred for 2-3 hours at 225-235° C., 2.4-2.6 MPa and 115-125 r / min under a nitrogen environment, and the mixture was exhausted at 0.008-0.012 MPa / s for 40-50 minutes. The mixture was heated to 255-265° C., 0.02-0.03 MPa and the stirring was continued for 55-65 minutes. n, cooled to room temperature with water, taken out, dried at 105-115° C. for 10-12 h, to obtain regenerated polyamide; the regenerated polyamide and modified glass fiber are mixed in a mass ratio of 1:(0.5-0.6), dried at 105-115° C. for 11-13 h, 0.01-0.03 times the mass of azobisisobutyronitrile of the regenerated polyamide is added, and the mixture is extruded by a twin-screw extruder at 265-275° C. and 700-800 r / min for 2-4 min, and then allowed to stand at 120-130° C. for 18-22 h, and naturally cooled to room temperature to obtain a regenerated polymer material.

[0016] As an optimization, the reaction equation of the single-terminal amino polyvinyl siloxane in step (1) is:

[0017]

[0018] As an optimization, the reaction equation of the pre-modified glass fiber in step (2) is:

[0019]

[0020] As an optimization, the reaction equation of the modified glass fiber in step (2) is:

[0021]

[0022] As an optimization, the reaction equation of the regenerated polyamide in step (4) is:

[0023]

[0024] Compared with the prior art, the beneficial effects achieved by the present invention are:

[0025] When preparing the recycled composite polymer material, the present invention comprises the following steps: reacting 3-aminopropyl pentamethyldisiloxane with tetramethyltetravinylcyclotetrasiloxane to obtain single-end amino polyvinylsiloxane; reacting glass fiber with 5,6-epoxyhexyltriethoxysilane and single-end amino polyvinylsiloxane in sequence to obtain modified glass fiber; hydrolyzing waste polyamide 66 to obtain regenerated hexamethylenediamine and regenerated adipic acid; reacting regenerated hexamethylenediamine, regenerated adipic acid and vinylphosphonic acid to obtain regenerated polyamide; and mixing the regenerated polyamide, the modified glass fiber and azobisisobutyronitrile and then extruding the mixture to prepare the recycled composite polymer material.

[0026] Firstly, 3-aminopropyl pentamethyldisiloxane and tetramethyltetravinylcyclotetrasiloxane are reacted to obtain single-end amino polyvinylsiloxane; glass fiber is reacted with 5,6-epoxyhexyltriethoxysilane and single-end amino polyvinylsiloxane in sequence to obtain modified glass fiber; a silane coupling agent is grafted onto the glass fiber to improve the dispersibility of the glass fiber and enhance the tensile strength of the recycled composite polymer material; meanwhile, epoxy groups are retained on the surface of the glass fiber to react with the amino groups on the single-end amino polyvinylsiloxane and grafted with long silicon oxygen chains, and the flame retardant and waterproof properties of the recycled composite polymer material are improved by virtue of the characteristics of the long silicon oxygen chains being insulating, hydrophobic and having low surface energy.

[0027] Secondly, waste polyamide 66 is hydrolyzed to obtain regenerated hexamethylenediamine and regenerated adipic acid; regenerated hexamethylenediamine, regenerated adipic acid and vinylphosphonic acid are reacted to obtain regenerated polyamide; regenerated polyamide, modified glass fiber and azobisisobutyronitrile are mixed and extruded to prepare a regenerated composite polymer material; sulfuric acid is used to catalyze the hydrolysis of polyamide 66 to recover regenerated hexamethylenediamine and adipic acid to the greatest extent; vinylphosphonic acid is used to replace part of the adipic acid during the polymerization process, and phosphorus is introduced into the main chain of the regenerated polyamide, so that the polymer is dehydrated and carbonized during combustion to form a protective layer to isolate oxygen and improve the flame retardant properties of the regenerated composite polymer material; at the same time, the double bonds on the vinylphosphonic acid can be cross-linked with the double bonds on the single-end amino polyvinylsiloxane to form a complex cross-linking network between the glass fiber and the main chain of the regenerated polyamide, thereby improving the tensile strength of the regenerated composite polymer material. DETAILED DESCRIPTION

[0028] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0029] In order to more clearly illustrate the method provided by the present invention, the following examples are used to describe in detail the various index testing methods of the regenerated composite polymer materials prepared in the following examples are as follows:

[0030] Flame retardant properties: The limiting oxygen index of the recycled composite polymer material obtained in each example and the comparative example was measured according to GB / T2406.

[0031] Tensile strength: The regenerated composite polymer materials obtained in each example and the comparative example were tested for tensile strength at 23°C according to GB / T1040.

[0032] Waterproof performance: The regenerated composite polymer material obtained in each embodiment and the comparative example material were taken with the same size, and the water contact angle was tested using a dynamic and static contact angle meter at 25° C. and a rotating water drop volume of 3 μL.

[0033] Example 1

[0034] A method for preparing a regenerated composite polymer material, the method comprising the following steps:

[0035] (1) 3-aminopropyl pentamethyldisiloxane and tetramethyltetravinylcyclotetrasiloxane were mixed in a mass ratio of 1:4, stirred at 65° C. and 100 rpm for 30 min, trifluoromethylsulfonic acid (0.01 times the mass of 3-aminopropyl pentamethyldisiloxane) was added, and stirring was continued for 7 h. Anhydrous sodium carbonate was added to adjust the pH to 6, and then filtered, and distilled at 105° C. and 0.1 MPa for 2 h to obtain single-end amino polyvinylsiloxane;

[0036] (2) 5,6-epoxyhexyltriethoxysilane and anhydrous ethanol were mixed in a mass ratio of 1:14, and ultrasonically dispersed for 20 minutes to obtain a 5,6-epoxyhexyltriethoxysilane alcoholysis solution; the glass fiber was soaked in the 5,6-epoxyhexyltriethoxysilane alcoholysis solution for 3 hours, then taken out, washed with deionized water and anhydrous ethanol for 3 times, respectively, and dried at 60°C for 13 hours to obtain a pre-modified glass fiber; the pre-modified glass fiber, single-terminal amino polyvinyl siloxane, glacial acetic acid and isopropanol were mixed in a mass ratio of 1:2:0.01:2.8, stirred at 82°C and 100 rpm for 13 hours, naturally cooled to room temperature, filtered, washed with deionized water for 3 times, and dried at 65°C for 10 hours to obtain a modified glass fiber;

[0037] (3) Soaking the waste polyamide 66 in a sodium hydroxide solution with a mass fraction of 2% at 75° C. for 3 h, washing it with deionized water for 3 times after taking it out, drying it at 75° C. for 25 h, and then crushing it to a particle size of less than 1 mm to obtain polyamide powder; mixing the polyamide powder, deionized water and a sulfuric acid solution with a mass fraction of 36% at a molar ratio of 1:29:2, stirring it at 105° C. and 100 rpm for 6 h, filtering it after naturally cooling it to room temperature, adding calcium hydroxide 10 times the mass of the polyamide powder to the filtrate, stirring it at 95° C. and 200 rpm for 3 h, and distilling it under reduced pressure to obtain regenerated hexamethylenediamine; drying the filter residue at 75° C. for 11 h, adding deionized water 16 times the mass of the polyamide powder, stirring it at 85° C. and 100 rpm for 3 h, filtering it while hot, and letting the filtrate stand and cool to room temperature to precipitate recrystallization to obtain regenerated adipic acid;

[0038] (4) Regenerated hexamethylenediamine, vinylphosphonic acid, regenerated adipic acid and deionized water were mixed in a molar ratio of 1:0.2:0.4:5, and the pH of the solution was adjusted to 7.3 by adding regenerated adipic acid. The mixture was stirred for 3 h at 225°C, 2.4 MPa and 115 r / min under a nitrogen environment, and vented at 0.008 MPa / s for 50 min. The mixture was heated to 255°C and 0.02 MPa and stirred for 65 min. The mixture was cooled to room temperature and then taken out and dried at 105°C for 12 h to obtain a regenerated polyamide. The regenerated polyamide and modified glass fiber were mixed in a mass ratio of 1:0.5, dried at 105°C for 13 h, and then 0.01 times the mass of the regenerated polyamide was added to azobisisobutyronitrile. The mixture was extruded by a twin-screw extruder at 265°C and 700 r / min for 4 min, and then allowed to stand at 120°C for 22 h. The mixture was naturally cooled to room temperature to obtain a regenerated polymer material.

[0039] Example 2

[0040] A method for preparing a regenerated composite polymer material, the method comprising the following steps:

[0041] (1) 3-aminopropyl pentamethyldisiloxane and tetramethyltetravinylcyclotetrasiloxane were mixed in a mass ratio of 1:5, stirred at 70° C. and 150 rpm for 25 min, trifluoromethylsulfonic acid (0.015 times the mass of 3-aminopropyl pentamethyldisiloxane) was added, and stirring was continued for 6 h. Anhydrous sodium carbonate was added to adjust the pH to 6.5, and then filtered, and distilled at 110° C. and 0.2 MPa for 1.5 h to obtain single-end amino polyvinylsiloxane;

[0042] (2) 5,6-epoxyhexyltriethoxysilane and anhydrous ethanol were mixed in a mass ratio of 1:15, and ultrasonically dispersed for 25 minutes to obtain a 5,6-epoxyhexyltriethoxysilane alcoholysis solution; the glass fiber was soaked in the 5,6-epoxyhexyltriethoxysilane alcoholysis solution for 4 hours, then taken out, washed with deionized water and anhydrous ethanol for 4 times, respectively, and dried at 65°C for 12 hours to obtain a pre-modified glass fiber; the pre-modified glass fiber, single-terminated amino polyvinyl siloxane, glacial acetic acid and isopropanol were mixed in a mass ratio of 1:2.5:0.02:3, stirred at 83°C and 150 rpm for 12 hours, naturally cooled to room temperature, filtered, washed with deionized water for 4 times, and dried at 70°C for 9 hours to obtain a modified glass fiber;

[0043] (3) Soaking the waste polyamide 66 in a sodium hydroxide solution with a mass fraction of 3% at 80° C. for 2 h, washing it with deionized water for 4 times after taking it out, drying it at 80° C. for 24 h, and then crushing it to a particle size of less than 1 mm to obtain polyamide powder; mixing the polyamide powder, deionized water and a sulfuric acid solution with a mass fraction of 37% at a molar ratio of 1:30:2.5, stirring it at 110° C. and 150 rpm for 5 h, filtering it after naturally cooling it to room temperature, adding calcium hydroxide 11 times the mass of the polyamide powder to the filtrate, stirring it at 100° C. and 250 rpm for 2 h, and distilling it under reduced pressure to obtain regenerated hexamethylenediamine; drying the filter residue at 80° C. for 10 h, adding deionized water 17 times the mass of the polyamide powder, stirring it at 90° C. and 150 rpm for 2.5 h, filtering it while hot, and letting the filtrate stand and cool to room temperature to precipitate recrystallization to obtain regenerated adipic acid;

[0044] (4) Regenerated hexamethylenediamine, vinylphosphonic acid, regenerated adipic acid and deionized water were mixed in a molar ratio of 1:0.3:0.5:6, and the pH value of the solution was adjusted to 7.4 by adding regenerated adipic acid. The mixture was stirred for 2.5 h at 230°C, 2.5 MPa and 120 r / min under a nitrogen environment, and vented at 0.01 MPa / s for 45 min. The mixture was heated to 260°C and 0.025 MPa and stirred for 60 min. The mixture was cooled to room temperature and then taken out and dried at 110°C for 11 h to obtain a regenerated polyamide. The regenerated polyamide and modified glass fiber were mixed in a mass ratio of 1:0.55, dried at 110°C for 12 h, and then 0.02 times the mass of azobisisobutyronitrile of the regenerated polyamide was added. The mixture was extruded by a twin-screw extruder at 270°C and 750 r / min for 3 min, and then allowed to stand at 125°C for 20 h. The mixture was naturally cooled to room temperature to obtain a regenerated polymer material.

[0045] Example 3

[0046] A method for preparing a regenerated composite polymer material, the method comprising the following steps:

[0047] (1) 3-aminopropyl pentamethyldisiloxane and tetramethyltetravinylcyclotetrasiloxane were mixed in a mass ratio of 1:6, stirred at 75° C. and 200 rpm for 20 min, trifluoromethylsulfonic acid (0.02 times the mass of 3-aminopropyl pentamethyldisiloxane) was added, and stirring was continued for 5 h. Anhydrous sodium carbonate was added to adjust the pH to 7, and then filtered, and distilled at 115° C. and 0.3 MPa for 1 h to obtain single-end amino polyvinylsiloxane;

[0048] (2) 5,6-epoxyhexyltriethoxysilane and anhydrous ethanol were mixed in a mass ratio of 1:16, and ultrasonically dispersed for 30 minutes to obtain a 5,6-epoxyhexyltriethoxysilane alcoholysis solution; the glass fiber was soaked in the 5,6-epoxyhexyltriethoxysilane alcoholysis solution for 5 hours, then taken out, washed with deionized water and anhydrous ethanol for 5 times, respectively, and dried at 70°C for 11 hours to obtain a pre-modified glass fiber; the pre-modified glass fiber, single-terminal amino polyvinyl siloxane, glacial acetic acid and isopropanol were mixed in a mass ratio of 1:3:0.03:3.2, stirred at 84°C and 200 rpm for 11 hours, naturally cooled to room temperature, filtered, washed with deionized water for 5 times, and dried at 75°C for 8 hours to obtain a modified glass fiber;

[0049] (3) Soaking the waste polyamide 66 in a sodium hydroxide solution with a mass fraction of 4% at 85° C. for 1 hour, washing it with deionized water for 5 times after taking it out, drying it at 85° C. for 23 hours, and then crushing it to a particle size of less than 1 mm to obtain polyamide powder; mixing the polyamide powder, deionized water and a sulfuric acid solution with a mass fraction of 38% at a molar ratio of 1:31:3, stirring it at 115° C. and 200 rpm for 4 hours, filtering it after naturally cooling it to room temperature, adding calcium hydroxide 12 times the mass of the polyamide powder to the filtrate, stirring it at 105° C. and 300 rpm for 1 hour, and distilling it under reduced pressure to obtain regenerated hexamethylenediamine; drying the filter residue at 85° C. for 9 hours, adding deionized water 18 times the mass of the polyamide powder, stirring it at 95° C. and 200 rpm for 2 hours, filtering it while hot, and letting the filtrate stand and cool to room temperature to precipitate recrystallization to obtain regenerated adipic acid;

[0050] (4) Regenerated hexamethylenediamine, vinylphosphonic acid, regenerated adipic acid and deionized water were mixed in a molar ratio of 1:0.4:0.6:7, and the pH value of the solution was adjusted to 7.5 by adding regenerated adipic acid. The mixture was stirred for 2 h at 235°C, 2.6 MPa and 125 r / min under a nitrogen environment, and vented at 0.012 MPa / s for 40 min. The mixture was heated to 265°C and 0.03 MPa and stirred for 55 min. The mixture was cooled to room temperature and then taken out and dried at 115°C for 10 h to obtain a regenerated polyamide. The regenerated polyamide and modified glass fiber were mixed in a mass ratio of 1:0.6, dried at 115°C for 11 h, and then 0.03 times the mass of azobisisobutyronitrile of the regenerated polyamide was added. The mixture was extruded by a twin-screw extruder at 275°C and 800 r / min for 2 min, and then allowed to stand at 130°C for 18 h. The mixture was naturally cooled to room temperature to obtain a regenerated polymer material.

[0051] Comparative Example 1

[0052] A method for preparing a regenerated composite polymer material, the method comprising the following steps:

[0053] (1) Soaking waste polyamide 66 in a sodium hydroxide solution with a mass fraction of 3% at 80° C. for 2 h, washing it with deionized water for 4 times after taking it out, drying it at 80° C. for 24 h, and then crushing it to a particle size of less than 1 mm to obtain polyamide powder; mixing the polyamide powder, deionized water and a sulfuric acid solution with a mass fraction of 37% at a molar ratio of 1:30:2.5, stirring it at 110° C. and 150 rpm for 5 h, filtering it after naturally cooling it to room temperature, adding calcium hydroxide 11 times the mass of the polyamide powder to the filtrate, stirring it at 100° C. and 250 rpm for 2 h, and distilling it under reduced pressure to obtain regenerated hexamethylenediamine; drying the filter residue at 80° C. for 10 h, adding deionized water 17 times the mass of the polyamide powder, stirring it at 90° C. and 150 rpm for 2.5 h, filtering it while hot, and cooling the filtrate to room temperature to precipitate recrystallization to obtain regenerated adipic acid;

[0054] (2) Regenerated hexamethylenediamine, vinylphosphonic acid, regenerated adipic acid and deionized water were mixed in a molar ratio of 1:0.3:0.5:6, and the pH value of the solution was adjusted to 7.4 by adding regenerated adipic acid. The mixture was stirred for 2.5 h at 230°C, 2.5 MPa and 120 r / min under a nitrogen environment, and vented at 0.01 MPa / s for 45 min. The mixture was heated to 260°C and 0.025 MPa and stirred for 60 min. The mixture was cooled to room temperature and then taken out and dried at 110°C for 11 h to obtain regenerated polyamide. The regenerated polyamide and glass fiber were mixed in a mass ratio of 1:0.55, dried at 110°C for 12 h, and then 0.02 times the mass of azobisisobutyronitrile of the regenerated polyamide was added. The mixture was extruded by a twin-screw extruder at 270°C and 750 r / min for 3 min, and then allowed to stand at 125°C for 20 h. The mixture was naturally cooled to room temperature to obtain a regenerated polymer material.

[0055] Comparative Example 2

[0056] A method for preparing a regenerated composite polymer material, the method comprising the following steps:

[0057] (1) 3-aminopropyl pentamethyldisiloxane and tetramethyltetravinylcyclotetrasiloxane were mixed in a mass ratio of 1:5, stirred at 70° C. and 150 rpm for 25 min, trifluoromethylsulfonic acid (0.015 times the mass of 3-aminopropyl pentamethyldisiloxane) was added, and stirring was continued for 6 h. Anhydrous sodium carbonate was added to adjust the pH to 6.5, and then filtered, and distilled at 110° C. and 0.2 MPa for 1.5 h to obtain single-end amino polyvinylsiloxane;

[0058] (2) 5,6-epoxyhexyltriethoxysilane and anhydrous ethanol were mixed in a mass ratio of 1:15, and ultrasonically dispersed for 25 minutes to obtain a 5,6-epoxyhexyltriethoxysilane alcoholysis solution; the glass fiber was soaked in the 5,6-epoxyhexyltriethoxysilane alcoholysis solution for 4 hours, then taken out, washed with deionized water and anhydrous ethanol for 4 times, respectively, and dried at 65°C for 12 hours to obtain a pre-modified glass fiber; the pre-modified glass fiber, single-terminated amino polyvinyl siloxane, glacial acetic acid and isopropanol were mixed in a mass ratio of 1:2.5:0.02:3, stirred at 83°C and 150 rpm for 12 hours, naturally cooled to room temperature, filtered, washed with deionized water for 4 times, and dried at 70°C for 9 hours to obtain a modified glass fiber;

[0059] (3) Soaking the waste polyamide 66 in a sodium hydroxide solution with a mass fraction of 3% at 80° C. for 2 h, washing it with deionized water for 4 times after taking it out, drying it at 80° C. for 24 h, and then crushing it to a particle size of less than 1 mm to obtain polyamide powder; mixing the polyamide powder, deionized water and a sulfuric acid solution with a mass fraction of 37% at a molar ratio of 1:30:2.5, stirring it at 110° C. and 150 rpm for 5 h, filtering it after naturally cooling it to room temperature, adding calcium hydroxide 11 times the mass of the polyamide powder to the filtrate, stirring it at 100° C. and 250 rpm for 2 h, and distilling it under reduced pressure to obtain regenerated hexamethylenediamine; drying the filter residue at 80° C. for 10 h, adding deionized water 17 times the mass of the polyamide powder, stirring it at 90° C. and 150 rpm for 2.5 h, filtering it while hot, and letting the filtrate stand and cool to room temperature to precipitate recrystallization to obtain regenerated adipic acid;

[0060] (4) The regenerated hexamethylenediamine, regenerated adipic acid and deionized water were mixed in a molar ratio of 1:0.8:6, and the pH value of the solution was adjusted to 7.4 by adding regenerated adipic acid. The mixture was stirred for 2.5 h at 230° C., 2.5 MPa and 120 r / min under a nitrogen environment, and vented at 0.01 MPa / s for 45 min. The mixture was heated to 260° C., 0.025 MPa and stirred for 60 min. The mixture was cooled to room temperature and then taken out and dried at 110° C. for 11 h to obtain a regenerated polyamide. The regenerated polyamide and modified glass fiber were mixed in a mass ratio of 1:0.55, dried at 110° C. for 12 h, and then 0.02 times the mass of azobisisobutyronitrile of the regenerated polyamide was added. The mixture was extruded by a twin-screw extruder at 270° C., 750 r / min for 3 min, and then allowed to stand at 125° C. for 20 h. The mixture was naturally cooled to room temperature to obtain a regenerated polymer material.

[0061] Comparative Example 3

[0062] A method for preparing a regenerated composite polymer material, the method comprising the following steps:

[0063] (1) Soaking waste polyamide 66 in a sodium hydroxide solution with a mass fraction of 3% at 80° C. for 2 h, washing it with deionized water for 4 times after taking it out, drying it at 80° C. for 24 h, and then crushing it to a particle size of less than 1 mm to obtain polyamide powder; mixing the polyamide powder, deionized water and a sulfuric acid solution with a mass fraction of 37% at a molar ratio of 1:30:2.5, stirring it at 110° C. and 150 rpm for 5 h, filtering it after naturally cooling it to room temperature, adding calcium hydroxide 11 times the mass of the polyamide powder to the filtrate, stirring it at 100° C. and 250 rpm for 2 h, and distilling it under reduced pressure to obtain regenerated hexamethylenediamine; drying the filter residue at 80° C. for 10 h, adding deionized water 17 times the mass of the polyamide powder, stirring it at 90° C. and 150 rpm for 2.5 h, filtering it while hot, and cooling the filtrate to room temperature to precipitate recrystallization to obtain regenerated adipic acid;

[0064] (2) Regenerated hexamethylenediamine, regenerated adipic acid and deionized water were mixed in a molar ratio of 1:0.8:6, and the pH value of the solution was adjusted to 7.4 by adding regenerated adipic acid. The mixture was stirred for 2.5 h at 230°C, 2.5 MPa and 120 r / min under a nitrogen environment, and vented at 0.01 MPa / s for 45 min. The mixture was heated to 260°C and 0.025 MPa and stirred for 60 min. The mixture was cooled to room temperature and then taken out and dried at 110°C for 11 h to obtain a regenerated polyamide. The regenerated polyamide and glass fiber were mixed in a mass ratio of 1:0.55, dried at 110°C for 12 h, and then 0.02 times the mass of azobisisobutyronitrile of the regenerated polyamide was added. The mixture was extruded by a twin-screw extruder at 270°C and 750 r / min for 3 min, and then allowed to stand at 125°C for 20 h. The mixture was naturally cooled to room temperature to obtain a regenerated polymer material.

[0065] Effect example

[0066] Table 1 below shows the analysis results of the flame retardant properties, tensile strength and waterproof properties of the recycled composite polymer materials of Examples 1 to 3 of the present invention and Comparative Examples 1 to 3.

[0067] Table 1

[0068] Limiting oxygen index % Water contact angle° Tensile strength MPa Example 1 34.4 134 252 Example 2 35.2 139 254 Example 3 34.9 137 249 Comparative Example 1 26.6 65 122 Comparative Example 2 25.1 137 113 Comparative Example 3 20.3 61 105

[0069] From the comparison of the experimental data of Examples 1 to 3 and Comparative Example 1N3 in Table 1, it can be found that the recycled composite polymer material prepared by the present invention has good flame retardant properties, tensile strength and waterproof properties.

[0070] By comparison, Examples 1, 2, and 3 have higher limiting oxygen index, water contact angle, and tensile strength than Comparative Example 1, which indicates that the silane coupling agent is grafted onto the glass fiber to improve the dispersibility of the glass fiber and enhance the tensile strength of the recycled composite polymer material. At the same time, the epoxy groups are retained on the surface of the glass fiber to react with the amino groups on the single-end amino polyvinylsiloxane to graft long silicon oxygen chains, and the flame retardant and waterproof properties of the recycled composite polymer material are improved by the insulating, hydrophobic, and low surface energy characteristics of the long silicon oxygen chains.

[0071] By comparison, the limiting oxygen index and tensile strength of Examples 1, 2, and 3 are higher than those of Comparative Example 2, which shows that vinyl phosphonic acid is used to replace part of adipic acid in the polymerization process, and phosphorus is introduced into the main chain of the regenerated polyamide, so that the polymer is dehydrated and carbonized during combustion to form a protective layer, isolating oxygen and improving the flame retardant properties of the regenerated composite polymer material; at the same time, the double bonds on the vinyl phosphonic acid can be cross-linked with the double bonds on the single-end amino polyvinyl siloxane to form a complex cross-linking network between the glass fiber and the regenerated polyamide main chain, thereby improving the tensile strength of the regenerated composite polymer material.

[0072] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations within the meaning and scope of the equivalent elements of the claims be included in the invention. Any marking in a claim should not be considered as limiting the claim to which it relates.

Claims

1. A regenerated composite polymer material, characterized in that: The recycled composite polymer material is prepared by mixing recycled polyamide, modified glass fiber and azobisisobutyronitrile and then extruding; The regenerated polyamide is obtained by reacting regenerated hexamethylenediamine and regenerated adipic acid obtained by hydrolyzing waste polyamide 66 with vinylphosphonic acid; The modified glass fiber is obtained by reacting glass fiber with 5,6-epoxyhexyltriethoxysilane and single-terminal amino polyvinyl siloxane in sequence; The single-end amino polyvinyl siloxane is obtained by reacting 3-aminopropyl pentamethyl disiloxane and tetramethyl tetravinyl cyclotetrasiloxane.

2. A method for preparing a regenerated composite polymer material, characterized in that: The method comprises the following preparation steps: (1) 3-aminopropyl pentamethyldisiloxane and tetramethyltetravinylcyclotetrasiloxane were mixed in a mass ratio of 1:(4-6), stirred at 65-75°C and 100-200 rpm for 20-30 min, trifluoromethylsulfonic acid (0.01-0.02 times the mass of 3-aminopropyl pentamethyldisiloxane) was added, and stirring was continued for 5-7 h. Anhydrous sodium carbonate was added to adjust the pH to 6-7, and then filtered. The mixture was distilled at 105-115°C and 0.1-0.3 MPa for 1-2 h to obtain single-end amino polyvinylsiloxane; (2) 5,6-epoxyhexyltriethoxysilane and anhydrous ethanol were mixed in a mass ratio of 1:(14-16), and ultrasonically dispersed for 20-30 minutes to obtain a 5,6-epoxyhexyltriethoxysilane alcoholysis solution; the glass fiber was soaked in the 5,6-epoxyhexyltriethoxysilane alcoholysis solution for 3-5 hours, then taken out, washed with deionized water and anhydrous ethanol for 3-5 times respectively, and dried at 60-70°C for 11-13 hours to obtain Pre-modified glass fiber; mixing pre-modified glass fiber, single-end amino polyvinyl siloxane, glacial acetic acid and isopropyl alcohol in a mass ratio of 1:(2-3):(0.01-0.03):(2.8-3.2), stirring at 82-84°C and 100-200 rpm for 11-13 hours, naturally cooling to room temperature and filtering, washing with deionized water for 3-5 times, and drying at 65-75°C for 8-10 hours to obtain modified glass fiber; (3) Soak the waste polyamide 66 in a sodium hydroxide solution with a mass fraction of 2-4% at 75-85°C for 1-3 h, wash it with deionized water for 3-5 times, dry it at 75-85°C for 23-25 ​​h, and then grind it into a particle size of less than 1 mm to obtain polyamide powder; mix the polyamide powder, deionized water and sulfuric acid solution with a mass fraction of 36-38% in a molar ratio of 1:(29-31):(2-3), stir it at 105-115°C and 100-200 rpm for 4-6 h, naturally cool to room temperature and filter, take the filtrate and add calcium hydroxide 10-12 times the mass of the polyamide powder, stir at 95-105°C and 200-300rpm for 1-3h, and distill under reduced pressure to obtain regenerated hexamethylenediamine; dry the filter residue at 75-85°C for 9-11h, add deionized water 16-18 times the mass of the polyamide powder, stir at 85-95°C and 100-200rpm for 2-3h, filter while hot, let the filtrate stand and cool to room temperature, precipitate recrystallization, and obtain regenerated adipic acid; (4) Mix regenerated hexamethylenediamine, vinylphosphonic acid, regenerated adipic acid and deionized water in a molar ratio of 1:(0.2~0.4):(0.4~0.6):(5~7), add regenerated adipic acid to adjust the pH of the solution to 7.3~7.5, stir under nitrogen environment at 225~235℃, 2.4~2.6MPa, 115~125r / min for 2~3h, exhaust at 0.008~0.012MPa / s for 40~50min, heat to 255~265℃, 0.02~0.03MPa and continue stirring for 55~65min n, cooled to room temperature with water and then taken out, dried at 105-115°C for 10-12h to obtain regenerated polyamide; the regenerated polyamide and modified glass fiber were mixed in a mass ratio of 1:(0.5-0.6), dried at 105-115°C for 11-13h, 0.01-0.03 times the mass of azobisisobutyronitrile of the regenerated polyamide was added, and the mixture was extruded by a twin-screw extruder at 265-275°C and 700-800r / min for 2-4min, and then allowed to stand at 120-130°C for 18-22h, and naturally cooled to room temperature to obtain a regenerated polymer material.