A high temperature resistant and waterproof PET label and its preparation process
The PET label's preparation process, utilizing a thiolated silica-halloysite nanotube composite and epoxidized polyurethane, addresses the issues of deformation and warping in high temperature and humidity by creating a robust cross-linked network, resulting in improved heat resistance and waterproofness.
Patent Information
- Application Number
- CN202410885950.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-03
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-07-03
AI Technical Summary
Traditional PET labels are prone to softening, deformation, and warping in high temperature and high humidity environments, leading to reduced performance and shortened service life.
A preparation process involving a thiolated silica-halloysite nanotube composite and epoxidized polyurethane is used to create a high temperature resistant and waterproof PET label, enhancing the adhesive's heat resistance and waterproofness by forming a cross-linked network through the reaction of thiol groups with epoxy groups.
The PET label exhibits improved peel strength, adhesion, high temperature stability, and excellent waterproof properties due to the enhanced bonding force and compatibility between the modified polyurethane and silica-halloysite nanotube composite.
Smart Images

Figure BDA0004926060170000091 
Figure BDA0004926060170000101
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of PET labels, in particular to a high-temperature resistant and waterproof PET label and a preparation process thereof. Background Art
[0002] PET label is a common material for identifying products and packaging. It has excellent wear resistance, high transparency, high tensile strength, etc., and is widely used in various industries, such as food packaging, drug identification, electronic products, etc. However, traditional PET labels are easily softened and damp in high temperature and high humidity environments, resulting in deformation, bubbles and warping, which affects the performance of PET labels and shortens their service life.
[0003] In order to solve the above problems, the present invention provides a high temperature resistant and waterproof PET label and a preparation process thereof. Summary of the invention
[0004] The object of the present invention is to provide a high temperature resistant and waterproof PET label and a preparation process thereof, so as to solve the problems raised in the above background technology.
[0005] In order to solve the above technical problems, the present invention provides the following technical solutions:
[0006] A preparation process of a high temperature resistant and waterproof PET label comprises the following steps:
[0007] Step 1: taking a thiolated silica-halloysite nanotube composite, epoxidized polyurethane, and triethylamine, and stirring them evenly to obtain a modified polyurethane;
[0008] Step 2: Take modified polyurethane and epoxy resin, heat until melted, add curing agent, dioctyl phthalate and acetone, stir evenly to obtain adhesive;
[0009] Step 3: Take a PET film and apply ink on the PET film; apply adhesive on the release surface of the PET release paper and solidify it to obtain a release paper coated with adhesive; laminate the side of the release paper coated with adhesive and the side of the PET film not coated with ink to obtain a high temperature resistant and waterproof PET label.
[0010] More optimally, the adhesive comprises the following ingredients, by weight: 2-3 parts of modified polyurethane, 10-12 parts of epoxy resin, 5-7 parts of curing agent, 0.3-0.4 parts of dioctyl phthalate, and 1-2 parts of acetone.
[0011] More optimally, the preparation method of the thiolated silica-halloysite nanotube complex is: take ethanol and deionized water, stir evenly, add the silica-halloysite nanotube complex, ultrasonically disperse, add 3-mercaptopropyltriethoxysilane, stir evenly, add acetic acid dropwise to adjust the pH value to 5-6, stir for 30-40 minutes, centrifuge and wash to obtain the thiolated silica-halloysite nanotube complex.
[0012] More optimally, the preparation method of the silica-halloysite nanotube composite is: take halloysite nanotubes and anhydrous ethanol, ultrasonically disperse them, add ammonia water, ultrasonically disperse them at 30-35°C for 20-30 minutes, drop dibutyltin dilaurate, stir at 40-45°C for 30-40 minutes, then drop ethyl orthosilicate, stir at 40-45°C for 3-4 hours, add 1H, 1H, 2H, 2H-perfluorooctyltriethoxysilane, stir for 3-4 hours, centrifuge, wash, and dry to obtain the silica-halloysite nanotube composite.
[0013] More optimally, the preparation method of the epoxidized polyurethane is: take a polyurethane prepolymer, add 2,3-epoxy-1-propanol, react at 60-65°C for 5-6h, add N,N-dimethylethanolamine dropwise, add deionized water dropwise, react for 1-2h, heat to 80-85°C, and distill under reduced pressure to obtain the epoxidized polyurethane.
[0014] More optimally, the preparation method of the polyurethane prepolymer is: take castor oil polyol, dimethylol propionic acid, trimethylol propane, acetone, and toluene diisocyanate, heat to 60-65° C., add dibutyltin dilaurate catalyst, heat to 70-75° C., react for 3-4 hours, and obtain a polyurethane prepolymer.
[0015] More optimally, the curing agent is m-phenylenediamine.
[0016] Compared with the prior art, the beneficial effects achieved by the present invention are:
[0017] (1) The present invention adds modified polyurethane to the adhesive to improve the high temperature resistance and waterproof performance of the PET label. The modified polyurethane is mixed with a thiolated silica-halloysite nanotube composite and an epoxidized polyurethane. Halloysite nanotubes are nanoparticles with a hollow nanorod-like microstructure and a large surface area. The present invention generates silica on the halloysite nanotubes by adding ethyl orthosilicate to enhance its specific surface area, and then improves the hydrophobicity of the silica-halloysite nanotube composite by adding 1H, 1H, 2H, 2H-perfluorooctyltriethoxysilane for modification, thereby enhancing the waterproof performance of the PET label.
[0018] (2) The present invention prepares a polyurethane with good heat resistance, and then performs epoxidation treatment on it so that it has a large number of epoxy groups. Then, the silica-halloysite nanotube composite is thiolated by using 3-mercaptopropyltriethoxysilane, and the thiol group reacts with the epoxy group, so that a cross-linked network is formed between the thiolated silica-halloysite nanotube composite and the epoxidized polyurethane, thereby enhancing the bonding force and compatibility between the two, thereby improving the heat resistance and waterproofness of the adhesive, so that the PET label has high peel strength, good adhesion, and excellent high temperature stability and waterproof properties. DETAILED DESCRIPTION
[0019] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0020] All raw materials and their sources involved in the present invention are not particularly limited, and exemplary include:
[0021] Halloysite nanotubes: diameter: 50-300 nm, length: 1-10 μm; epoxy resin: model: E-44, which can be purchased from Shandong Yousuo Chemical Technology Co., Ltd.; ink: model: UV161, which can be purchased from Hanghua Ink Co., Ltd.
[0022] Embodiment 1: A process for preparing a high temperature resistant and waterproof PET label, comprising the following steps:
[0023] Step 1: Preparation of epoxidized polyurethane:
[0024] S1: Take 335g of castor oil polyol, 27g of dimethylol propionic acid, 25g of trimethylol propane, 90g of acetone, and 175g of toluene diisocyanate, heat to 63°C, add 1g of dibutyltin dilaurate catalyst, heat to 73°C, react for 3.5h, and obtain a polyurethane prepolymer;
[0025] S2: Take a polyurethane prepolymer, add 7g 2,3-epoxy-1-propanol, react at 63°C for 5.5h, add 20g N,N-dimethylethanolamine dropwise, add 820g deionized water dropwise within 2h, react for 1.5h, heat to 83°C, and distill under reduced pressure to obtain epoxidized polyurethane;
[0026] Step 2: Preparation of silica-halloysite nanotube composite:
[0027] Take 8g of halloysite nanotubes and 100mL of 95% anhydrous ethanol, ultrasonically disperse them, add 5mL of 25wt% ammonia water, ultrasonically disperse them at 32°C for 25min, drop 0.2mL of dibutyltin dilaurate, stir at 43°C for 35min, then drop 4g of ethyl orthosilicate, stir at 42°C for 3.5h, add 0.2g of 1H, 1H, 2H, 2H-perfluorooctyltriethoxysilane, stir for 3.5h, centrifuge, wash and dry to obtain a silica-halloysite nanotube composite;
[0028] Step 3: Preparation of thiolated silica-halloysite nanotube composite:
[0029] Take 400 mL of ethanol and 100 mL of deionized water, stir evenly, add 5 g of silica-halloysite nanotube complex, disperse by ultrasonic, add 0.25 g of 3-mercaptopropyltriethoxysilane, stir evenly, add acetic acid dropwise to adjust the pH value to 5.5, stir for 35 min, centrifuge and wash to obtain thiolated silica-halloysite nanotube complex;
[0030] Step 4: Preparation of modified polyurethane:
[0031] Take 10 g of thiolated silica-halloysite nanotube composite, 35 g of epoxidized polyurethane, and 1 g of triethylamine, stir evenly to obtain modified polyurethane;
[0032] Step 5: Preparation method of high temperature resistant and waterproof PET label:
[0033] Take modified polyurethane and epoxy resin, heat until melted, add curing agent m-phenylenediamine, dioctyl phthalate and acetone, stir evenly to obtain adhesive;
[0034] The adhesive comprises the following components, by weight: 2.5 parts of modified polyurethane, 11 parts of epoxy resin, 6 parts of curing agent m-phenylenediamine, 0.35 parts of dioctyl phthalate, and 1.5 parts of acetone;
[0035] Take a PET film with a thickness of 12 μm, and apply the ink on the PET film to a thickness of 2 μm;
[0036] The adhesive is evenly coated on the release surface of the PET release paper with a thickness of 75 μm to a coating thickness of 10 μm, and cured to obtain a release paper coated with the adhesive;
[0037] The side of the release paper coated with the adhesive is laminated with the side of the PET film not coated with the ink to obtain a high temperature resistant and waterproof PET label.
[0038] Embodiment 2: A process for preparing a high temperature resistant and waterproof PET label, comprising the following steps:
[0039] Step 1: Preparation of epoxidized polyurethane:
[0040] S1: Take 335g of castor oil polyol, 27g of dimethylol propionic acid, 25g of trimethylol propane, 90g of acetone, and 175g of toluene diisocyanate, heat to 60°C, add 1g of dibutyltin dilaurate catalyst, heat to 70°C, and react for 3h to obtain a polyurethane prepolymer;
[0041] S2: Take a polyurethane prepolymer, add 7g of 2,3-epoxy-1-propanol, react at 60°C for 5h, add 20g of N,N-dimethylethanolamine dropwise, add 820g of deionized water dropwise within 2h, react for 1h, heat to 80°C, and distill under reduced pressure to obtain epoxidized polyurethane;
[0042] Step 2: Preparation of silica-halloysite nanotube composite:
[0043] Take 8g of halloysite nanotubes and 100mL of 95% anhydrous ethanol, ultrasonically disperse them, add 5mL of 25wt% ammonia water, ultrasonically disperse them at 30°C for 20min, drop 0.2mL of dibutyltin dilaurate, stir at 40°C for 30min, then drop 4g of ethyl orthosilicate, stir at 40°C for 3h, add 0.2g of 1H, 1H, 2H, 2H-perfluorooctyltriethoxysilane, stir for 3h, centrifuge, wash and dry to obtain a silica-halloysite nanotube composite;
[0044] Step 3: Preparation of thiolated silica-halloysite nanotube composite:
[0045] Take 400 mL of ethanol and 100 mL of deionized water, stir evenly, add 5 g of silica-halloysite nanotube complex, disperse by ultrasonic, add 0.25 g of 3-mercaptopropyltriethoxysilane, stir evenly, add acetic acid dropwise to adjust the pH value to 5, stir for 30 min, centrifuge and wash to obtain thiolated silica-halloysite nanotube complex;
[0046] Step 4: Preparation of modified polyurethane:
[0047] Take 10 g of thiolated silica-halloysite nanotube composite, 35 g of epoxidized polyurethane, and 1 g of triethylamine, stir evenly to obtain modified polyurethane;
[0048] Step 5: Preparation method of high temperature resistant and waterproof PET label:
[0049] Take modified polyurethane and epoxy resin, heat until melted, add curing agent m-phenylenediamine, dioctyl phthalate and acetone, stir evenly to obtain adhesive;
[0050] The adhesive comprises the following components, by weight: 2 parts of modified polyurethane, 10 parts of epoxy resin, 5 parts of curing agent m-phenylenediamine, 0.3 parts of dioctyl phthalate, and 1 part of acetone;
[0051] Take a PET film with a thickness of 12 μm, and apply the ink on the PET film to a thickness of 2 μm;
[0052] The adhesive is evenly coated on the release surface of the PET release paper with a thickness of 75 μm to a coating thickness of 10 μm, and cured to obtain a release paper coated with the adhesive;
[0053] The side of the release paper coated with the adhesive is laminated with the side of the PET film not coated with the ink to obtain a high temperature resistant and waterproof PET label.
[0054] Embodiment 3: A process for preparing a high temperature resistant and waterproof PET label, comprising the following steps:
[0055] Step 1: Preparation of epoxidized polyurethane:
[0056] S1: Take 335g of castor oil polyol, 27g of dimethylol propionic acid, 25g of trimethylol propane, 90g of acetone, and 175g of toluene diisocyanate, heat to 65°C, add 1g of dibutyltin dilaurate catalyst, heat to 75°C, react for 4h, and obtain a polyurethane prepolymer;
[0057] S2: Take a polyurethane prepolymer, add 7g 2,3-epoxy-1-propanol, react at 65°C for 6h, add 20g N,N-dimethylethanolamine dropwise, add 820g deionized water dropwise within 2h, react for 2h, heat to 85°C, and distill under reduced pressure to obtain epoxidized polyurethane;
[0058] Step 2: Preparation of silica-halloysite nanotube composite:
[0059] Take 8g of halloysite nanotubes and 100mL of 95% anhydrous ethanol, ultrasonically disperse them, add 5mL of 25wt% ammonia water, ultrasonically disperse them at 35°C for 30min, drop 0.2mL of dibutyltin dilaurate, stir at 45°C for 40min, then drop 4g of ethyl orthosilicate, stir at 45°C for 4h, add 0.2g of 1H, 1H, 2H, 2H-perfluorooctyltriethoxysilane, stir for 4h, centrifuge, wash and dry to obtain a silica-halloysite nanotube composite;
[0060] Step 3: Preparation of thiolated silica-halloysite nanotube composite:
[0061] Take 400 mL of ethanol and 100 mL of deionized water, stir evenly, add 5 g of silica-halloysite nanotube complex, disperse by ultrasonic, add 0.25 g of 3-mercaptopropyltriethoxysilane, stir evenly, add acetic acid dropwise to adjust the pH value to 6, stir for 40 min, centrifuge and wash to obtain thiolated silica-halloysite nanotube complex;
[0062] Step 4: Preparation of modified polyurethane:
[0063] Take 10 g of thiolated silica-halloysite nanotube composite, 35 g of epoxidized polyurethane, and 1 g of triethylamine, stir evenly to obtain modified polyurethane;
[0064] Step 5: Preparation method of high temperature resistant and waterproof PET label:
[0065] Take modified polyurethane and epoxy resin, heat until melted, add curing agent m-phenylenediamine, dioctyl phthalate and acetone, stir evenly to obtain adhesive;
[0066] The adhesive comprises the following components, by weight: 3 parts of modified polyurethane, 12 parts of epoxy resin, 7 parts of curing agent m-phenylenediamine, 0.4 parts of dioctyl phthalate, and 2 parts of acetone;
[0067] Take a PET film with a thickness of 12 μm, and apply the ink on the PET film to a thickness of 2 μm;
[0068] The adhesive is evenly coated on the release surface of the PET release paper with a thickness of 75 μm to a coating thickness of 10 μm, and cured to obtain a release paper coated with the adhesive;
[0069] The side of the release paper coated with the adhesive is laminated with the side of the PET film not coated with the ink to obtain a high temperature resistant and waterproof PET label.
[0070] Comparative Example 1: No silica was loaded, and the rest was the same as Example 1:
[0071] Step 1: Preparation of epoxidized polyurethane:
[0072] S1: Take 335g of castor oil polyol, 27g of dimethylol propionic acid, 25g of trimethylol propane, 90g of acetone, and 175g of toluene diisocyanate, heat to 63°C, add 1g of dibutyltin dilaurate catalyst, heat to 73°C, react for 3.5h, and obtain a polyurethane prepolymer;
[0073] S2: Take a polyurethane prepolymer, add 7g 2,3-epoxy-1-propanol, react at 63°C for 5.5h, add 20g N,N-dimethylethanolamine dropwise, add 820g deionized water dropwise within 2h, react for 1.5h, heat to 83°C, and distill under reduced pressure to obtain epoxidized polyurethane;
[0074] Step 2: Preparation of modified halloysite nanotubes:
[0075] Take 8g of halloysite nanotubes and 100mL of 95% anhydrous ethanol, ultrasonically disperse them, add 5mL of 25wt% ammonia water, ultrasonically disperse them at 32°C for 25min, drop 0.2mL of dibutyltin dilaurate, stir for 35min at 43°C, add 0.2g of 1H, 1H, 2H, 2H-perfluorooctyltriethoxysilane, stir for 3.5h, centrifuge, wash and dry to obtain modified halloysite nanotubes;
[0076] Step 3: Preparation of thiolated halloysite nanotube composites:
[0077] Take 400 mL of ethanol and 100 mL of deionized water, stir evenly, add 5 g of modified halloysite nanotube composite, disperse by ultrasonic, add 0.25 g of 3-mercaptopropyltriethoxysilane, stir evenly, add acetic acid dropwise to adjust the pH value to 5.5, stir for 35 min, centrifuge and wash to obtain the thiolated halloysite nanotube composite;
[0078] Step 4: Preparation of modified polyurethane:
[0079] Take 10 g of thiolated silica-halloysite nanotube composite, 35 g of epoxidized polyurethane, and 1 g of triethylamine, stir evenly to obtain modified polyurethane;
[0080] Step 5: Preparation method of high temperature resistant and waterproof PET label:
[0081] Take modified polyurethane and epoxy resin, heat until melted, add curing agent m-phenylenediamine, dioctyl phthalate and acetone, stir evenly to obtain adhesive;
[0082] The adhesive comprises the following components, by weight: 2.5 parts of modified polyurethane, 11 parts of epoxy resin, 6 parts of curing agent m-phenylenediamine, 0.35 parts of dioctyl phthalate, and 1.5 parts of acetone;
[0083] Take a PET film with a thickness of 12 μm, and apply the ink on the PET film to a thickness of 2 μm;
[0084] The adhesive is evenly coated on the release surface of the PET release paper with a thickness of 75 μm to a coating thickness of 10 μm, and cured to obtain a release paper coated with the adhesive;
[0085] The side of the release paper coated with the adhesive is laminated with the side of the PET film not coated with the ink to obtain a high temperature resistant and waterproof PET label.
[0086] Comparative Example 2: 3-mercaptopropyltriethoxysilane was not used to perform thiol modification on the silica-halloysite nanotube composite, and the rest was the same as Example 1:
[0087] Step 1: Preparation of epoxidized polyurethane:
[0088] S1: Take 335g of castor oil polyol, 27g of dimethylol propionic acid, 25g of trimethylol propane, 90g of acetone, and 175g of toluene diisocyanate, heat to 63°C, add 1g of dibutyltin dilaurate catalyst, heat to 73°C, react for 3.5h, and obtain a polyurethane prepolymer;
[0089] S2: Take a polyurethane prepolymer, add 7g 2,3-epoxy-1-propanol, react at 63°C for 5.5h, add 20g N,N-dimethylethanolamine dropwise, add 820g deionized water dropwise within 2h, react for 1.5h, heat to 83°C, and distill under reduced pressure to obtain epoxidized polyurethane;
[0090] Step 2: Preparation of silica-halloysite nanotube composite:
[0091] Take 8g of halloysite nanotubes and 100mL of 95% anhydrous ethanol, ultrasonically disperse them, add 5mL of 25wt% ammonia water, ultrasonically disperse them at 32°C for 25min, drop 0.2mL of dibutyltin dilaurate, stir at 43°C for 35min, then drop 4g of ethyl orthosilicate, stir at 42°C for 3.5h, add 0.2g of 1H, 1H, 2H, 2H-perfluorooctyltriethoxysilane, stir for 3.5h, centrifuge, wash and dry to obtain a silica-halloysite nanotube composite;
[0092] Step 3: Preparation of modified polyurethane:
[0093] Take 10 g of silica-halloysite nanotube composite, 35 g of epoxidized polyurethane, and 1 g of triethylamine, stir evenly to obtain modified polyurethane;
[0094] Step 4: Preparation method of high temperature resistant and waterproof PET label:
[0095] Take modified polyurethane and epoxy resin, heat until melted, add curing agent m-phenylenediamine, dioctyl phthalate and acetone, stir evenly to obtain adhesive;
[0096] The adhesive comprises the following components, by weight: 2.5 parts of modified polyurethane, 11 parts of epoxy resin, 6 parts of curing agent m-phenylenediamine, 0.35 parts of dioctyl phthalate, and 1.5 parts of acetone;
[0097] Take a PET film with a thickness of 12 μm, and apply the ink on the PET film to a thickness of 2 μm;
[0098] The adhesive is evenly coated on the release surface of the PET release paper with a thickness of 75 μm to a coating thickness of 10 μm, and cured to obtain a release paper coated with the adhesive;
[0099] The side of the release paper coated with the adhesive is laminated with the side of the PET film not coated with the ink to obtain a high temperature resistant and waterproof PET label.
[0100] Comparative Example 3: No epoxy polyurethane was added, and the rest was the same as Example 1:
[0101] Step 1: Preparation of silica-halloysite nanotube composite:
[0102] Take 8g of halloysite nanotubes and 100mL of 95% anhydrous ethanol, ultrasonically disperse them, add 5mL of 25wt% ammonia water, ultrasonically disperse them at 32°C for 25min, drop 0.2mL of dibutyltin dilaurate, stir at 43°C for 35min, then drop 4g of ethyl orthosilicate, stir at 42°C for 3.5h, add 0.2g of 1H, 1H, 2H, 2H-perfluorooctyltriethoxysilane, stir for 3.5h, centrifuge, wash and dry to obtain a silica-halloysite nanotube composite;
[0103] Step 2: Preparation of thiolated silica-halloysite nanotube composite:
[0104] Take 400 mL of ethanol and 100 mL of deionized water, stir evenly, add 5 g of silica-halloysite nanotube complex, disperse by ultrasonic, add 0.25 g of 3-mercaptopropyltriethoxysilane, stir evenly, add acetic acid dropwise to adjust the pH value to 5.5, stir for 35 min, centrifuge and wash to obtain thiolated silica-halloysite nanotube complex;
[0105] Step 3: Preparation method of high temperature resistant and waterproof PET label:
[0106] Take epoxy resin, heat it until it is melted, add curing agent m-phenylenediamine, dioctyl phthalate and acetone, stir evenly to obtain an adhesive;
[0107] The adhesive comprises the following components, by weight: 13.5 parts of epoxy resin, 6 parts of curing agent m-phenylenediamine, 0.35 parts of dioctyl phthalate, and 1.5 parts of acetone;
[0108] Take a PET film with a thickness of 12 μm, and apply the ink on the PET film to a thickness of 2 μm;
[0109] The adhesive is evenly coated on the release surface of the PET release paper with a thickness of 75 μm to a coating thickness of 10 μm, and cured to obtain a release paper coated with the adhesive;
[0110] The side of the release paper coated with the adhesive is laminated with the side of the PET film not coated with the ink to obtain a high temperature resistant and waterproof PET label.
[0111] experiment:
[0112] The high temperature resistant and waterproof PET labels prepared in Examples 1-3 and Comparative Examples 1-3 were used for performance testing. The PET labels were pasted on plastic bottles and then placed at 60°C for 48 hours. The high temperature resistance of the PET labels was evaluated based on the appearance of the PET labels. The adhesives prepared in Examples 1-3 and Comparative Examples 1-3 were coated on a glass plate with a coating thickness of 10 μm, cured, and the water contact angles thereof were tested. The peel strength with a stainless steel plate at 180° was tested according to the reference standard GB / T2792, and the adhesive coating thickness was 10 μm. The data obtained are shown in the following table:
[0113]
[0114]
[0115] Conclusion: From the comparison of the data in the table, it can be seen that comparative example 1 does not load silica, and the viscosity peel strength deteriorates. Comparative example 2 does not use 3-mercaptopropyltriethoxysilane to thiol-modify the silica-halloysite nanotube composite, and the compatibility between the silica-halloysite nanotube composite and epoxidized polyurethane is poor, and the performance of the PET label is reduced. Comparative example 3 does not add epoxidized polyurethane, and the binding force and compatibility between the silica-halloysite nanotube composite and epoxidized polyurethane are poor, and the performance of the PET label is reduced. Examples 1 to 3 add modified polyurethane to the adhesive to improve the high temperature resistance and waterproof performance of the PET label. By adding ethyl orthosilicate to generate silica on the halloysite nanotubes, its specific surface area is enhanced, and then by adding 1H, 1H, 2H, 2H-perfluorooctyltriethoxysilane for modification, the hydrophobicity of the silica-halloysite nanotube composite is improved, thereby enhancing the waterproof performance of the PET label. The polyurethane is epoxidized to carry a large number of epoxy groups. Then, the silica-halloysite nanotube composite is thiolated by using 3-mercaptopropyltriethoxysilane. The thiol group reacts with the epoxy group, so that a cross-linked network is formed between the thiolated silica-halloysite nanotube composite and the epoxidized polyurethane, which enhances the bonding force and compatibility between the two, thereby improving the heat resistance and waterproofness of the adhesive, so that the PET label has high peel strength, good adhesion, high temperature stability and excellent waterproof performance.
[0116] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A preparation process of a high temperature resistant and waterproof PET label, characterized in that: The following steps are involved: Step 1: taking a thiolated silica-halloysite nanotube composite, epoxidized polyurethane, and triethylamine, and stirring them evenly to obtain a modified polyurethane; Step 2: Take modified polyurethane and epoxy resin, heat until melted, add curing agent, dioctyl phthalate and acetone, stir evenly to obtain adhesive; Step 3: Take a PET film and apply ink on the PET film; apply adhesive on the release surface of the PET release paper, solidify it, and obtain a release paper coated with adhesive; laminate the side of the release paper coated with adhesive and the side of the PET film not coated with ink to obtain a high temperature resistant and waterproof PET label; The adhesive comprises the following components, by weight: 2-3 parts of modified polyurethane, 10-12 parts of epoxy resin, 5-7 parts of curing agent, 0.3-0.4 parts of dioctyl phthalate, and 1-2 parts of acetone; The preparation method of the thiolated silica-halloysite nanotube composite is as follows: ethanol and deionized water are mixed evenly, the silica-halloysite nanotube composite is added, ultrasonic dispersion is performed, 3-mercaptopropyltriethoxysilane is added, the composite is mixed evenly, acetic acid is added dropwise to adjust the pH value to 5-6, the composite is mixed for 30-40 minutes, centrifuged, and washed to obtain the thiolated silica-halloysite nanotube composite; The preparation method of the silica-halloysite nanotube composite is as follows: taking halloysite nanotubes and anhydrous ethanol, ultrasonically dispersing them, adding ammonia water, ultrasonically dispersing them at 30-35° C. for 20-30 minutes, dripping dibutyltin dilaurate, stirring at 40-45° C. for 30-40 minutes, then dripping ethyl orthosilicate, stirring at 40-45° C. for 3-4 hours, adding 1H, 1H, 2H, 2H-perfluorooctyltriethoxysilane, stirring for 3-4 hours, centrifuging, washing, and drying to obtain the silica-halloysite nanotube composite; The preparation method of the epoxidized polyurethane is as follows: taking a polyurethane prepolymer, adding 2,3-epoxy-1-propanol, reacting at 60-65° C. for 5-6 hours, dropping N,N-dimethylethanolamine, dropping deionized water, reacting for 1-2 hours, heating to 80-85° C., and distilling under reduced pressure to obtain the epoxidized polyurethane.
2. The process for preparing a high temperature resistant and waterproof PET label according to claim 1, characterized in that: The preparation method of the polyurethane prepolymer is as follows: castor oil polyol, dimethylol propionic acid, trimethylol propane, acetone, and toluene diisocyanate are taken, heated to 60-65° C., dibutyltin dilaurate catalyst is added, heated to 70-75° C., and reacted for 3-4 hours to obtain the polyurethane prepolymer.
3. The preparation process of a high temperature resistant and waterproof PET label according to claim 1, characterized in that: The curing agent is m-phenylenediamine.
4. A high temperature resistant and waterproof PET label prepared according to the preparation process of a high temperature resistant and waterproof PET label according to any one of claims 1 to 3.