Energy-saving sealant production process

By dividing raw materials into two categories according to thermal stability and particle size characteristics, and controlling them through specific addition order and stirring parameters, the problems of poor uniformity of raw materials and excessive temperature in sealant production are solved, and the sealant is realized Uniform quality and efficient production.

CN118652644BActive Publication Date: 2024-11-05TIANJIN JINGDABAOGUANG AUTOMOBILE SPARE PART CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411110448.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-05
Estimated Expiration
2044-08-14

AI Technical Summary

Technical Problem

Under high yield conditions, the existing sealant production process has poor raw material uniformity and excessive temperature leading to uneven product quality and waste of raw materials.

Method used

According to the thermal stability and particle size characteristics of the raw material, it is divided into two types of mixtures A and B, and it is uniformly mixed, and the raw material is uniformly dispersed through specific addition order and stirring parameters (such as speed, time, and temperature control), and finally the Mixture B is added to Mixture A and mixed to reduce the temperature influence.

Benefits of technology

The quality uniformity and efficient production of sealant are achieved, raw material waste is reduced, production efficiency and product fineness are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118652644B_ABST
    Figure CN118652644B_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of sealants, and discloses an energy-saving sealant production process, wherein raw materials that begin to change viscosity at temperatures below 45°C are mixed to obtain a mixture B; raw materials used to obtain the mixture B are removed, and the remaining raw materials are mixed to obtain a mixture A; mixture B is added to mixture A to obtain a sealant; for mixture A, the addition amount of the raw materials is judged, and when a raw material with an addition amount not greater than 2% of the total amount of the raw materials is selected to be added first, whether the raw materials have viscosity is judged, and the raw materials are added in the order of increasing adhesion of the raw materials; when a raw material with an addition amount greater than 2% of the total amount of the raw materials is selected to be added later, the average particle size of the raw materials is judged, and the raw materials with an average particle size not greater than 5 μm are added before the raw materials with an average particle size greater than 5 μm. The sealant production process of the invention can promote uniform mixing between the raw materials used to produce the sealant.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of sealants, and in particular to an energy-saving sealant production process. Background Art

[0002] In recent years, with the rapid development of the automobile industry, especially the rapid rise of new energy vehicles, the demand for various types of sealants for automobiles has also increased year by year. Therefore, sealant manufacturers must also continuously increase their production capacity.

[0003] In the face of industrial production, the existing production process, due to the large output of sealants produced, firstly, it is difficult to evenly distribute the raw materials during the preparation of the sealants, especially the raw materials with characteristics such as small dosage, small particle size, and high viscosity, which ultimately results in poor uniformity of product quality; secondly, in order to promote uniform mixing between the raw materials and improve the uniformity of product quality, the existing process generally increases the stirring rate, but causes the production temperature to be too high (over 40°C), which is particularly significant in summer, and ultimately causes some temperature-sensitive raw materials in the raw materials, such as raw materials with high viscosity, to become more difficult to disperse, resulting in a decline in the quality of the products produced and uneven quality.

[0004] Therefore, in order to improve the quality of sealants, improving the production process of sealants is the only way to promote the commercialization of sealants, especially for sealant production processes with an output of more than 5.5 tons. Summary of the invention

[0005] In order to solve the above technical problems, the present invention provides an energy-saving sealant production process. The sealant production process of the present invention can not only promote the uniform mixing of the raw materials for producing the sealant, thereby facilitating the acquisition of products with uniform quality; but also the production process of the present invention can also reduce the waste of raw materials, and is an energy-saving and efficient production process.

[0006] The present invention provides an energy-saving sealant production process, comprising the following steps:

[0007] According to the thermal stability of the raw materials, the raw materials whose viscosity begins to change below 45° C. are mixed to obtain a mixture B; the raw materials used to obtain the mixture B are removed, and the remaining raw materials are mixed to obtain a mixture A; the mixture B is added to the mixture A and mixed evenly to obtain a sealant;

[0008] When obtaining mixture A, determine the amount of raw materials to be added, select raw materials whose amount is not greater than 2% of the total amount of raw materials to be added first, and then select raw materials whose amount is greater than 2% of the total amount of raw materials to be added later;

[0009] When the raw material whose addition amount is not more than 2% of the total amount of raw materials is selected to be added first, it is determined whether the raw material has viscosity, and the raw materials are added in the order of increasing adhesion of the raw materials;

[0010] When a raw material with an addition amount greater than 2% of the total amount of raw materials is selected for addition, the average particle size of the raw materials is judged, and the raw material with an average particle size of no greater than 5 μm is added before the raw material with an average particle size greater than 5 μm;

[0011] The raw materials include diisononyl phthalate, fumed silica HL-200, solvent oil D-100, low molecular weight polyamide SY-530E, low molecular weight polyamide SY-532, zinc oxide, titanium dioxide MA-55, nano calcium carbonate CCS-25, nano calcium carbonate JB-25, nano calcium carbonate JB-05, calcium oxide CGX-3, heavy calcium carbonate CC-500, PVC paste resin PSM-31, PVC chloroacetic acid paste resin PCMA-12, and PVC blended resin SB-100.

[0012] Furthermore, the sum of the mass proportions of the masses of the various raw materials in the total amount of raw materials added is 100%.

[0013] Furthermore, when the mixture A is obtained, 0.9% to 1.5% of the total amount of raw materials of non-viscous fumed silica HL-200 is first added.

[0014] Furthermore, before adding the fumed silica HL-200, first add 9.3%-9.9% of diisononyl phthalate based on the total amount of raw materials, then add the fumed silica HL-200, and finally add 6.1%-6.7% of diisononyl phthalate based on the total amount of raw materials and 3.7%-4.3% of solvent oil D-100 based on the total amount of raw materials.

[0015] Furthermore, after adding 9.3%-9.9% of the total amount of raw materials of diisononyl phthalate and then adding fumed silica HL-200, the fumed silica HL-200 is immersed in the diisononyl phthalate for 2.5min-3.5min, and the speed of the frame stirring paddle is 45rpm-55rpm; after adding 6.1%-6.7% of the total amount of raw materials of diisononyl phthalate and 3.7%-4.3% of the total amount of raw materials of solvent oil D-100, two fast dispersing stirring paddles with a speed of 290rpm-310rpm are added, and the stirring time is 2.5min-3.5min.

[0016] Furthermore, before adding the raw material with viscosity in an amount not exceeding 2% of the total amount of the raw materials, 0.7%-1.3% of the total amount of the raw materials of low molecular weight polyamide SY-530E and 0.9%-1.5% of the total amount of the raw materials of low molecular weight polyamide SY-532 were added, and then the mixture was evenly mixed with two fast dispersing stirring paddles at a rotation speed of 290rpm-310rpm for a stirring time of 2.5min-3.5min.

[0017] Furthermore, after adding low molecular weight polyamide SY-530E and low molecular weight polyamide SY-532, 0.9%-1.5% of the total raw material amount and viscous zinc oxide, 0.5%-1.1% of the total raw material amount and viscous titanium dioxide MA-55 are added in sequence. After adding zinc oxide and titanium dioxide MA-55, two fast dispersing stirring paddles with a rotation speed of 290rpm-310rpm are used, and the stirring time is 2.5min-3.5min to mix evenly.

[0018] Furthermore, nano calcium carbonate CCS-25, nano calcium carbonate JB-25 and nano calcium carbonate JB-05 are added in an amount greater than 2% of the total amount of raw materials and with an average particle size of no more than 5 μm, wherein the amount of nano calcium carbonate CCS-25 added is 4.7%-5.3% of the total amount of raw materials added, the amount of nano calcium carbonate JB-25 added is 7.7%-8.3% of the total amount of raw materials added, and the amount of nano calcium carbonate JB-05 added is 9.7%-10.3% of the total amount of raw materials added, and then two fast dispersing stirring paddles with a rotation speed of 490rpm-510rpm are used for the stirring time of 9min-11min. During stirring, the stirring tool also needs to be cooled.

[0019] Furthermore, when calcium oxide CGX-3 and heavy calcium carbonate CC-500 are added in an amount greater than 2% of the total amount of raw materials and with an average particle size greater than 5 μm, diisononyl phthalate is also added, wherein the amount of calcium oxide CGX-3 added is 3.3%-3.9% of the total amount of raw materials added, the amount of heavy calcium carbonate CC-500 added is 6.3%-6.9% of the total amount of raw materials added, and the amount of diisononyl phthalate added is 1.3%-1.9% of the total amount of raw materials added. First, use a frame stirring paddle with a rotation speed of 145rpm-155rpm and two rapid dispersion stirring paddles with a rotation speed of 490rpm-510rpm, and the stirring time is 9min-11min; turn off the two rapid dispersion stirring paddles, and then adjust the speed of the frame stirring paddle to 45rpm-55rpm, and stir for 45min-55min.

[0020] Furthermore, when obtaining mixture B, 13.7%-14.3% of the total amount of raw materials of PVC paste resin PSM-31 and 7.7%-8.3% of the total amount of raw materials of PVC chloroacetic acid paste resin PCMA-12 are first stirred for 4min-6min with a frame stirring paddle at a rotation speed of 145rpm-150rpm, and then 7.7%-8.3% of the total amount of raw materials of diisononyl phthalate are added and stirred for 4min-6min with a frame stirring paddle at a rotation speed of 145rpm-150rpm.

[0021] Furthermore, when obtaining mixture B, PVC blending resin SB-100 was finally added, and the addition amount of PVC blending resin SB-100 was 4.7%-5.3% of the total amount of raw materials. When adding PVC blending resin SB-100, 4.5%-5.1% of diisononyl phthalate of the total amount of raw materials was also added. The rotation speed of the frame stirring paddle was 145rpm-150rpm, the rotation speed of the two fast dispersion stirring paddles was 290rpm-310rpm, and the stirring time was 9min-11min.

[0022] Furthermore, the mixture B is added to the mixture A for uniform mixing, and the frame stirring paddle is turned on at a speed of 145rpm-150rpm, and two high-speed dispersing stirring paddles are turned on at 290rpm-310rpm, and the mixture is stirred for 9min-11min, and the mixture is poured up and down and stirred for 25min-35min until all the materials are uniformly mixed, and the fineness of the mixture is tested. When the fineness of the mixture is not higher than 35, it is stirred for another 9min-11min.

[0023] The invention also provides a sealant produced by the production process.

[0024] The embodiments of the present invention have the following technical effects:

[0025] 1. The production process of the present invention can realize the production of no less than 5.5 tons of sealant, and the produced sealant has the characteristics of uniform quality and good quality.

[0026] 2. The production process of the present invention, in order to achieve good uniformity of the formed sealant, the order of addition between the raw materials is considered according to the characteristics of the raw materials and the amount of the raw materials in the production process, so that the raw materials can achieve good uniformity. In the present invention, the raw materials with a lower mass ratio and lower viscosity are added first before the raw materials with higher viscosity. On the one hand, it can ensure that the raw materials with a smaller amount of addition can be fully dispersed, and secondly, it can prevent the raw materials with lower viscosity from flying during the stirring process, causing the loss of raw materials; when adding raw materials with a larger mass ratio of raw materials, the average particle size of the raw materials is considered. The raw materials with a larger average particle size have better dispersibility themselves, so they are easy to disperse, so they are added at the end, and finally a uniformly dispersed mixture A can be obtained. Mixture B is to mix the raw materials with poor thermal stability with mixture A separately, and then mix mixture B with mixture A. In the process of obtaining mixture A, due to multiple stirring processes and a long production process time, the temperature in the preparation process rises, thereby affecting the raw materials with poor thermal stability in mixture B. Therefore, mixture B is prepared separately and finally mixed with mixture A, so that the quality of the sealant finally obtained can be improved.

[0027] 3. In the production process of the present invention, fumed silica HL-200 with a relatively low mass ratio is added first. Fumed silica HL-200 is in a powder state and has a high specific surface area, which causes its surface energy to be large and is difficult to disperse. Therefore, in the present invention, the fumed silica HL-200 is first dispersed and immersed in diisononyl phthalate. On the one hand, it can avoid the powdered fumed silica HL-200 from flying around, causing the loss of raw materials and reducing the quality of the final product. On the other hand, it can reduce the surface energy between the fumed silica HL-200 powders, which is beneficial to the dispersion effect in the later production. In the dispersion process, diisononyl phthalate and solvent oil are further added to reduce the mass concentration of fumed silica HL-200 in the mixture. On the one hand, it can promote the complete immersion of silica HL-200, thereby improving the uniformity of dispersion of fumed silica HL-200 and preventing the occurrence of powder agglomeration. On the other hand, it is to pave the way for adding low molecular weight polyamide SY-530E and low molecular weight polyamide SY-532 with viscous substances. First, low molecular weight polyamide SY-530E and low molecular weight polyamide SY-532 have poor dispersibility in the mixture. Diisononyl phthalate and solvent oil can reduce the viscosity between the raw materials after mixing. Second, it is to prevent the poor dispersibility between low molecular weight polyamide SY-530E and low molecular weight polyamide SY-532 and silica HL-200, and avoid agglomeration. Third, it prevents the occurrence of stratification and mesh structure of low molecular weight polyamide SY-530E and low molecular weight polyamide SY-532. Then add the viscous zinc oxide and titanium dioxide in turn. Zinc oxide and titanium dioxide have high viscosity and are added in small amounts. It is easier to achieve uniform dispersion by adding them first. Before adding zinc oxide and titanium dioxide, adding low molecular weight polyamide SY-530E and low molecular weight polyamide SY-532 can avoid the situation where the powders clump together and are difficult to disperse after adding zinc oxide and titanium dioxide. Then add nano calcium carbonate CCS-25, nano calcium carbonate JB-25, and nano calcium carbonate JB-05 with a smaller average particle size. Nano calcium carbonate has poor dispersibility and also releases heat. Therefore, when dispersing, it is necessary not only to adjust the stirring speed and time, but also to cool the stirring tools to prevent the increase in temperature from affecting other raw materials. Finally, calcium oxide CGX-3 and heavy calcium carbonate CC-500 with larger average particle size were added. In order to promote the uniformity between calcium oxide CGX-3, heavy calcium carbonate CC-500 and the mixed mixture, diisononyl phthalate was added during the stirring process, and the stirring tool was further cooled, and finally a uniformly dispersed mixture A was obtained.

[0028] In mixture B, PVC paste resin PSM-31, PVC chloroacetyl paste resin PCMA-12, and PVC blending resin SB-100 are added in sequence, among which PVC blending resin SB-100 can be added last due to its larger average particle size.

[0029] 4. The sealant production process of the present invention can not only promote uniform mixing of the raw materials for producing the sealant, thereby facilitating obtaining products of uniform quality; but also the production process of the present invention can reduce the waste of raw materials, and is an energy-saving and efficient production process. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0031] Figure 1 is the fineness test result of the sealant of the embodiment of the present invention, wherein Figure 1 (a) is the test result of the sealant fineness of comparative example 1. Figure 1 (b) is the test result of the sealant fineness of comparative example 2. Figure 1 (c) is the test result of the sealant fineness of Example 1.

[0032] Figure 2 is a test of the elongation at break of the embodiments and comparative examples, wherein Figure 2 (a) is a physical picture of the elongation at break of comparative example 1 after the test. Figure 2 (b) is a physical picture of the elongation at break of comparative example 2 after the test. Figure 2 (c) is a real picture of Example 1 after the elongation at break test.

[0033] Figure 3 This is the test data of elongation at break of comparative example 1. Figure 3 The results correspond to those in Table 2.

[0034] Figure 4 This is the test data of elongation at break of comparative example 2. Figure 4 The results correspond to those in Table 3.

[0035] Figure 5 is the test data of elongation at break of Example 1, Figure 5 The results correspond to those in Table 4. DETAILED DESCRIPTION

[0036] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work belong to the scope of protection of the present invention.

[0037] In a first aspect, the present invention provides an energy-saving sealant production process, comprising the following steps:

[0038] According to the thermal stability of the raw materials, the raw materials whose viscosity begins to change below 45° C. are mixed to obtain a mixture B; the raw materials used to obtain the mixture B are removed, and the remaining raw materials are mixed to obtain a mixture A; the mixture B is added to the mixture A and mixed evenly to obtain a sealant;

[0039] When obtaining mixture A, determine the amount of raw materials to be added, select raw materials whose amount is not greater than 2% of the total amount of raw materials to be added first, and then select raw materials whose amount is greater than 2% of the total amount of raw materials to be added later;

[0040] When the raw material whose addition amount is not more than 2% of the total amount of raw materials is selected to be added first, it is determined whether the raw material has viscosity, and the raw materials are added in the order of increasing adhesion of the raw materials;

[0041] When a raw material with an addition amount greater than 2% of the total amount of raw materials is selected for addition, the average particle size of the raw materials is judged, and the raw material with an average particle size of no greater than 5 μm is added before the raw material with an average particle size greater than 5 μm;

[0042] The raw materials include diisononyl phthalate, fumed silica HL-200, solvent oil D-100, low molecular weight polyamide SY-530E, low molecular weight polyamide SY-532, zinc oxide, titanium dioxide MA-55, nano calcium carbonate CCS-25, nano calcium carbonate JB-25, nano calcium carbonate JB-05, calcium oxide CGX-3, heavy calcium carbonate CC-500, PVC paste resin PSM-31, PVC chloroacetic acid paste resin PCMA-12, and PVC blended resin SB-100.

[0043] In some embodiments, the sum of the mass proportions of the masses of the various raw materials in the total amount of raw materials added is 100%.

[0044] In some embodiments, when the mixture A is obtained, 0.9% to 1.5% of the total amount of raw materials of non-viscous fumed silica HL-200 is first added.

[0045] In some embodiments, before adding the fumed silica HL-200, 9.3%-9.9% of diisononyl phthalate is added based on the total amount of raw materials, and then the fumed silica HL-200 is added, and finally 6.1%-6.7% of diisononyl phthalate and 3.7%-4.3% of solvent oil D-100 are added based on the total amount of raw materials.

[0046] In some embodiments, 9.3%-9.9% of the total raw material amount of diisononyl phthalate is first added, and then after adding the fumed silica HL-200, the fumed silica HL-200 is first added to the diisononyl phthalate and soaked for 2.5min-3.5min, and the frame stirring paddle speed is 45rpm-55rpm; after adding 6.1%-6.7% of the total raw material amount of diisononyl phthalate and 3.7%-4.3% of the total raw material amount of solvent oil D-100, two fast dispersing stirring paddles with a rotation speed of 290rpm-310rpm are added, and the stirring time is 2.5min-3.5min.

[0047] In some embodiments, before adding a raw material with viscosity in an amount not exceeding 2% of the total amount of raw materials, 0.7%-1.3% of the total amount of raw materials of low molecular weight polyamide SY-530E and 0.9%-1.5% of the total amount of raw materials of low molecular weight polyamide SY-532 are added, and then two fast dispersing stirring paddles with a rotation speed of 290rpm-310rpm are used for stirring for 2.5min-3.5min to mix evenly.

[0048] In some embodiments, after adding low molecular weight polyamide SY-530E and low molecular weight polyamide SY-532, 0.9%-1.5% of the total raw material amount and viscous zinc oxide, 0.5%-1.1% of the total raw material amount and viscous titanium dioxide MA-55 are added in sequence. After adding zinc oxide and titanium dioxide MA-55, two fast dispersing stirring paddles with a rotation speed of 290rpm-310rpm are used, and the stirring time is 2.5min-3.5min to mix them evenly.

[0049] In some embodiments, nano calcium carbonate CCS-25, nano calcium carbonate JB-25, and nano calcium carbonate JB-05 are added in an amount greater than 2% of the total amount of raw materials and with an average particle size of no more than 5 μm, wherein the amount of nano calcium carbonate CCS-25 added is 4.7%-5.3% of the total amount of raw materials added, the amount of nano calcium carbonate JB-25 added is 7.7%-8.3% of the total amount of raw materials added, and the amount of nano calcium carbonate JB-05 added is 9.7%-10.3% of the total amount of raw materials added. Then, two fast dispersing stirring paddles with a rotation speed of 490rpm-510rpm are used for the stirring time of 9min-11min. During stirring, the stirring tool also needs to be cooled.

[0050] In some embodiments, when calcium oxide CGX-3 and heavy calcium carbonate CC-500 are added in an amount greater than 2% of the total amount of raw materials and with an average particle size greater than 5 μm, diisononyl phthalate is also added, wherein the amount of calcium oxide CGX-3 added is 3.3%-3.9% of the total amount of raw materials added, the amount of heavy calcium carbonate CC-500 added is 6.3%-6.9% of the total amount of raw materials added, and the amount of diisononyl phthalate added is 1.3%-1.9% of the total amount of raw materials added. First, a frame stirring paddle with a rotation speed of 145rpm-155rpm and two rapid dispersion stirring paddles with a rotation speed of 490rpm-510rpm are used for stirring for 9min-11min; the two rapid dispersion stirring paddles are turned off, and then the rotation speed of the frame stirring paddle is adjusted to 45rpm-55rpm, and the stirring time is 45min-55min.

[0051] In some embodiments, when obtaining mixture B, 13.7%-14.3% of the total raw material amount of PVC paste resin PSM-31 and 7.7%-8.3% of the total raw material amount of PVC chloroacetic acid paste resin PCMA-12 are first stirred for 4min-6min with a frame stirring paddle at a rotation speed of 145rpm-150rpm, and then 7.7%-8.3% of the total raw material amount of diisononyl phthalate is added and stirred for 4min-6min with a frame stirring paddle at a rotation speed of 145rpm-150rpm.

[0052] In some embodiments, when obtaining mixture B, PVC blending resin SB-100 is finally added, and the addition amount of PVC blending resin SB-100 is 4.7%-5.3% of the total amount of raw materials. When adding PVC blending resin SB-100, 4.5%-5.1% of diisononyl phthalate of the total amount of raw materials is also added. The rotation speed of the frame stirring paddle is 145rpm-150rpm, the rotation speed of the two fast dispersion stirring paddles is 290rpm-310rpm, and the stirring time is 9min-11min.

[0053] In the present invention, the PVC paste resin PSM-31, PVC chloroacetate paste resin PCMA-12 and PVC blended resin SB-100 in the raw materials are more sensitive to temperature. At 40 degrees, their viscosity changes slowly, and at 45 degrees, their viscosity changes increase. Therefore, when obtaining mixture B, the temperature of the production process needs to be controlled below 40 degrees.

[0054] In some embodiments, the mixture B is added to the mixture A for uniform mixing, and the frame stirring paddle is turned on at a speed of 145rpm-150rpm, and two high-speed dispersion stirring paddles are turned on at 290rpm-310rpm, and the mixture is stirred for 9min-11min, and the mixture is poured up and down and stirred for 25min-35min until all the materials are evenly mixed. The fineness of the mixture is tested, and when the fineness of the mixture is not higher than 35, it is stirred for another 9min-11min.

[0055] In a second aspect, some embodiments of the present invention also provide a sealant produced by the production process.

[0056] The following is explained in conjunction with specific embodiments:

[0057] Embodiment 1:

[0058] First, add 480g of diisononyl phthalate to the stirring tank, add 60g of fumed silica HL-200, wait for the fumed silica HL-200 to soak in diisononyl phthalate, slowly open the frame stirring paddle, the speed is 50rpm, the stirring time is 3min, and the fumed silica HL-200 is fully immersed in diisononyl phthalate. Add 320g diisononyl phthalate and 200g solvent oil D-100, turn on two fast dispersing stirring paddles at 300rpm, and stir for 3min. Add 50g low molecular weight polyamide SY-530E and 60g low molecular weight polyamide SY-532, two fast dispersing stirring paddles at 300rpm, and stir for 3min. Add 60g zinc oxide, two fast dispersing stirring paddles at 300rpm, stir for 3min, and then add 40g titanium dioxide MA-55, two fast dispersing stirring paddles at 300rpm, and stir for 3min. Add 250g of nano calcium carbonate CCS-25 and 400g of nano calcium carbonate JB-25, turn on the frame stirring paddle, the speed is 150rpm, and turn on two high-speed dispersing stirring paddles at 500rpm at the same time, stir for 10min. When turning on the high-speed stirring paddle, turn on the cooling water in the agitator jacket to cool the agitator. Add 500g of nano calcium carbonate JB-05, turn on the frame stirring paddle, the speed is 150rpm, and turn on two high-speed dispersing stirring paddles at 500rpm at the same time, and stir for 10min. Add 180g of calcium oxide CGX-3, 330g of heavy calcium carbonate CC-500, and 80g of diisononyl phthalate, turn on the frame stirring paddle, the speed is 150rpm, and turn on two high-speed dispersing stirring paddles at 500rpm at the same time, stir for 10min. After dispersion is completed, turn off the two fast stirring paddles, adjust the speed of the frame stirring paddle to 50rpm, and stir for about 40min, which can reduce the temperature of the stirring tank to below 35°C to obtain mixture A.

[0059] First, add 400g of diisononyl phthalate, then add 700g of PVC paste resin PSM-31 and 400g of PVC chloroacetate paste resin PCMA-12, turn on the frame stirring paddle, the speed is 150rpm, stir for 5min to preliminarily disperse the PVC paste resin PSM-31 and PVC chloroacetate paste resin PCMA-12 into diisononyl phthalate. Then add 250g of PVC blending resin SB-100 and 240g of diisononyl phthalate, turn on the frame stirring paddle, the speed is 150rpm, and turn on two high-speed dispersing stirring paddles at 300rpm, and stir for 10min. Mixture B is obtained.

[0060] Add mixture B to mixture A, turn on the frame stirring paddle at 150 rpm, turn on two high-speed dispersing stirring paddles at 300 rpm, and stir for 10 minutes. Use the circulation pump provided by the stirrer to pour the materials up and down, stir for 30 minutes, until all the materials are mixed evenly, test the fineness of the mixture, and when the fineness of the mixture is not higher than 35, stir for another 10 minutes to obtain a sealant with a rotational viscosity of 100,000 cp.

[0061] Comparative Example 1:

[0062] Add 1600g of diisononyl phthalate, 200g of solvent oil D-100, 60g of fumed silica HL-200, 50g of low molecular weight polyamide SY-530E, 60g of low molecular weight polyamide SY-532, 50g of titanium dioxide MA-55, 50g of zinc oxide, and 180g of calcium oxide CGX-3, and stir at a speed of 300rpm for 5min.

[0063] Then add 400g of PVC chloroacetyl paste resin PCMA-12, 700g of PVC paste resin PSM-31 and 250g of PVC blended resin SB-100, and stir at a speed of 300rpm for 10min.

[0064] Then add 250g of nano calcium carbonate CCS-25 and 500g of nano calcium carbonate JB-05, and stir at a rotation speed of 300rpm for 10min; then add 400g of nano calcium carbonate JB-25, and stir at a rotation speed of 300rpm for 15min.

[0065] Add 250 g of heavy calcium carbonate CC-500 and stir at 300 rpm for 20 min.

[0066] The mixed slurry obtained above was poured from the transfer tank into the grinder by a material pouring pump and ground for 4 hours to obtain a sealant with a rotational viscosity of 100,000 cp.

[0067] Comparative Example 2:

[0068] Add 1600g of diisononyl phthalate, 200g of solvent oil D-100, 60g of fumed silica HL-200, 50g of low molecular weight polyamide SY-530E, 60g of low molecular weight polyamide SY-532, 50g of titanium dioxide MA-55, 50g of zinc oxide, and 180g of calcium oxide CGX-3, and stir at a speed of 300rpm for 10min.

[0069] Then add 400g of PVC chloroacetyl paste resin PCMA-12, 700g of PVC paste resin PSM-31 and 250g of PVC blended resin SB-100, and stir at a speed of 300rpm for 20min.

[0070] Then add 250g of nano calcium carbonate CCS-25 and 500g of nano calcium carbonate JB-05, and stir at a rotation speed of 300rpm for 20min; then add 400g of nano calcium carbonate JB-25, and stir at a rotation speed of 300rpm for 20min.

[0071] Add 250 g of heavy calcium carbonate CC-500 and stir at 300 rpm for 20 min.

[0072] The mixed slurry obtained above was poured up and down using the circulation pump provided in the stirrer and stirred for 1.5 hours until all the materials were evenly mixed and no particles were visible to the naked eye. The mixture was then stirred for another 35 minutes to obtain a sealant with a rotational viscosity of 100,000 cp.

[0073] Rating standards for sealant adhesion: Level 1: The sealant has no adhesion, the adhesive layer has no adhesion to the substrate or is very soft and completely detached from the substrate; Level 2: Part of the adhesive layer adheres to the substrate and remains on the substrate; Level 3: Sufficient adhesion, more than 90% of the adhesive layer remains on the substrate, with only a small amount of detachment; Level 4: Good adhesion, 100% of the adhesive layer remains on the substrate, and the adhesive layer tears itself.

[0074] Detection of sealant fineness: The fineness is tested in accordance with GB / T 1724-2019 standard.

[0075] Testing of elongation at break of sealant: According to GB / T 528-2009 standard, three groups of parallel experiments were conducted for the embodiment and comparative example respectively, and the final result was the average of the results of the three groups of parallel experiments.

[0076] Results and Analysis:

[0077] Table 1 Performance test results of the sealants of Example 1 and Comparative Example 1

[0078]

[0079] Table 2 Test results of elongation at break of comparative example 1

[0080]

[0081] Table 3 Test results of elongation at break of comparative example 2

[0082]

[0083] Table 4 Test results of elongation at break of Example 1

[0084]

[0085] The results of comparing the sealant obtained by the process of the present invention with the sealant obtained by Comparative Examples 1 and 2 are shown in Table 1. It can be found that the sealant of Example 1 of the present invention has better fineness, shear strength, elongation at break and adhesion, as shown in Tables 1 and Figure 1 In the prior art, grinding is often used to improve the fineness of sealants, but the effect of grinding is not as significant as the technical effect of the present invention. It can be seen that according to the characteristics of the raw materials themselves, a suitable addition sequence is selected, which can promote the full and uniform dispersion of the raw materials during the preparation of the sealant, thereby improving the performance of the sealant.

[0086] The sealants obtained from Example 1 and Comparative Examples 1-2 of the present invention were subjected to shear strength tests. The test results are shown in Tables 1-4 and Figure 2-Figure 5 It can be found that the sealant of the present invention has better shear strength than that of Comparative Examples 1 and 2, and Figure 2 It can also be seen from (c) that the fracture mode of the sealant of the present invention is completely different from that of comparative example 2. The fracture mode of comparative example 2 is direct disconnection from the surface. Therefore, it can also be reversely proved that the present invention can select the appropriate addition sequence and stirring time according to the characteristics of the raw materials themselves, and control the temperature in the production process to obtain a sealant with better performance.

[0087] In the existing traditional process of producing sealants, grinding for 4 hours is used to promote the uniform dispersion of raw materials and reduce the fineness of the product, such as in Comparative Example 1; there is also the use of pouring materials up and down to stir for 1.5 hours to improve the dispersion between raw materials, such as in Comparative Example 2. The production process of the present invention combines the characteristics of the raw materials. Under the entire production process, the time used to achieve uniform dispersion between raw materials is no more than 152 minutes, and the fineness and mechanical properties of the obtained sealant products meet the standards; compared with the traditional production process, the production process of the present invention is at least 30% more efficient in time (the production time of Comparative Example 1 is 300 minutes, and the production time of Comparative Example 2 is 210 minutes). In addition, in the traditional process, more thinner (diisononyl phthalate) is added to promote uniform dispersion between raw materials with poor thermal stability. In the present invention, by mixing raw materials with poor thermal stability separately and controlling the temperature during stirring within 40°C, the use of 1.5%-2% diisononyl phthalate is reduced, and the quality of the sealant is also guaranteed.

[0088] In summary, the production process of the present invention is particularly suitable for the raw materials in the present invention, and the production process of the present invention can produce at least 5.5 tons of sealant at a time, and the obtained sealant is not only uniform and has good fineness, but also has good shear strength and elongation at break.

[0089] It should be noted that the terms used in the present invention are only for describing specific embodiments, rather than limiting the scope of the present application. As shown in the present specification, unless the context clearly indicates an exception, the words "one", "a", "a kind of" and / or "the" do not specifically refer to the singular, but may also include the plural. The terms "include", "comprise" or any other variant thereof are intended to cover non-exclusive inclusion, so that the process, method or device including a series of elements includes not only those elements, but also includes other elements not explicitly listed, or also includes elements inherent to such process, method or device. In the absence of more restrictions, the elements defined by the sentence "include one..." do not exclude the presence of other identical elements in the process, method or device including the elements.

[0090] It should also be noted that the terms "center", "up", "down", "left", "right", "vertical", "horizontal", "inside", "outside", etc., indicating the orientation or positional relationship, are based on the orientation or positional relationship shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention. Unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", etc. should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be an indirect connection through an intermediate medium, or it can be a connection between the two elements. For those of ordinary skill in the art, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0091] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the technical solutions of the embodiments of the present invention.

Claims

1. An energy-saving sealant production process, characterized in that: The steps include: According to the thermal stability of the raw materials, the raw materials whose viscosity begins to change below 45° C. are mixed to obtain a mixture B; the raw materials used to obtain the mixture B are removed, and the remaining raw materials are mixed to obtain a mixture A; the mixture B is added to the mixture A and mixed evenly to obtain a sealant; When obtaining mixture A, determine the amount of raw materials to be added, select raw materials whose amount is not greater than 2% of the total amount of raw materials to be added first, and then select raw materials whose amount is greater than 2% of the total amount of raw materials to be added later; When the raw material whose addition amount is not more than 2% of the total amount of raw materials is selected to be added first, it is determined whether the raw material has viscosity, and the raw materials are added in the order of increasing adhesion of the raw materials; When a raw material with an addition amount greater than 2% of the total amount of raw materials is selected for addition, the average particle size of the raw materials is judged, and the raw material with an average particle size of no greater than 5 μm is added before the raw material with an average particle size greater than 5 μm; The raw materials include diisononyl phthalate, fumed silica HL-200, solvent oil D-100, low molecular weight polyamide SY-530E, low molecular weight polyamide SY-532, zinc oxide, titanium dioxide MA-55, nano calcium carbonate CCS-25, nano calcium carbonate JB-25, nano calcium carbonate JB-05, calcium oxide CGX-3, heavy calcium carbonate CC-500, PVC paste resin PSM-31, PVC chloroacetic acid paste resin PCMA-12, PVC blended resin SB-100; When obtaining mixture A, first add 0.9%-1.5% of the total raw material of non-viscous fumed silica HL-200, Before adding fumed silica HL-200, first add 9.3%-9.9% of the total raw materials of diisononyl phthalate, then add fumed silica HL-200, and finally add 6.1%-6.7% of the total raw materials of diisononyl phthalate and 3.7%-4.3% of the total raw materials of solvent oil D-100. The first step is to add 9.3%-9.9% of the total amount of raw materials to diisononyl phthalate, and then add fumed silica HL-200, and then the fumed silica HL-200 is soaked in the first diisononyl phthalate for 2.5min-3.5min, and the frame stirring paddle speed is 45rpm-55rpm; after adding 6.1%-6.7% of the total amount of raw materials to diisononyl phthalate and 3.7%-4.3% of the total amount of raw materials to solvent oil D-100, two fast dispersing stirring paddles with a rotation speed of 290rpm-310rpm are added, and the stirring time is 2.5min-3.5min; Before adding the raw materials with viscosity in an amount not exceeding 2% of the total amount of raw materials, 0.7%-1.3% of the total amount of raw materials of low molecular weight polyamide SY-530E and 0.9%-1.5% of the total amount of raw materials of low molecular weight polyamide SY-532 were added, and then two fast dispersing stirring paddles with a speed of 290rpm-310rpm were used for stirring for 2.5min-3.5min to mix evenly. After adding low molecular weight polyamide SY-530E and low molecular weight polyamide SY-532, 0.9%-1.5% of the total amount of raw materials and viscous zinc oxide are added in sequence; The total amount of raw materials is 0.5%-1.1%, and the viscous titanium dioxide MA-55 is added. After zinc oxide and titanium dioxide MA-55 are added, two fast dispersing stirring paddles with a speed of 290rpm-310rpm are used for stirring for 2.5min-3.5min to mix evenly; Add nano calcium carbonate CCS-25, nano calcium carbonate JB-25, and nano calcium carbonate JB-05 in an amount greater than 2% of the total amount of raw materials and with an average particle size of no more than 5 μm, wherein the amount of nano calcium carbonate CCS-25 is 4.7%-5.3% of the total amount of raw materials, the amount of nano calcium carbonate JB-25 is 7.7%-8.3% of the total amount of raw materials, and the amount of nano calcium carbonate JB-05 is 9.7%-10.3% of the total amount of raw materials, and then use two fast dispersing stirring paddles with a rotation speed of 490 rpm-510 rpm for a stirring time of 9 min-11 min, and during stirring, the stirring tool needs to be cooled; When calcium oxide CGX-3 and heavy calcium carbonate CC-500 are added in an amount greater than 2% of the total amount of raw materials and with an average particle size greater than 5 μm, diisononyl phthalate is also added, wherein the amount of calcium oxide CGX-3 added is 3.3%-3.9% of the total amount of raw materials added, the amount of heavy calcium carbonate CC-500 added is 6.3%-6.9% of the total amount of raw materials added, and the amount of diisononyl phthalate added is 1.3%-1.9% of the total amount of raw materials added. First, a frame stirring paddle with a rotation speed of 145rpm-155rpm and two fast dispersing stirring paddles with a rotation speed of 490rpm-510rpm are used for stirring for 9min-11min; the two fast dispersing stirring paddles are turned off, and then the rotation speed of the frame stirring paddle is adjusted to 45rpm-55rpm, and the stirring time is 45min-55min; When obtaining mixture B, firstly stir 13.7%-14.3% of the total raw material amount of PVC paste resin PSM-31 and 7.7%-8.3% of the total raw material amount of PVC chloroacetate paste resin PCMA-12 with a frame stirring paddle at a rotation speed of 145rpm-150rpm for 4min-6min, and then add 7.7%-8.3% of the total raw material amount of diisononyl phthalate, and stir with a frame stirring paddle at a rotation speed of 145rpm-150rpm for 4min-6min; When obtaining mixture B, PVC blending resin SB-100 is finally added. The addition amount of PVC blending resin SB-100 is 4.7%-5.3% of the total amount of raw materials. When adding PVC blending resin SB-100, 4.5%-5.1% of diisononyl phthalate of the total amount of raw materials is also added. The rotation speed of the frame stirring paddle is 145rpm-150rpm, the rotation speed of the two fast dispersion stirring paddles is 290rpm-310rpm, and the stirring time is 9min-11min.

2. The production process according to claim 1, characterized in that: The mixture B is added to the mixture A for uniform mixing, and the frame stirring paddle is turned on at a speed of 145rpm-150rpm, and two high-speed dispersing stirring paddles are turned on at 290rpm-310rpm, and the mixture is stirred for 9min-11min, and the mixture is poured up and down and stirred for 25min-35min until all the materials are uniformly mixed. The fineness of the mixture is tested, and when the fineness of the mixture is not higher than 35, it is stirred for another 9min-11min.