A Roebel single-belt delamination strength test method
Through the Roebel single-band layered strength testing method, including welding, tensile test and Weibull distribution fitting, the stress failure and sample complexity problems of Roebel cable layered strength test were solved, quantitative description strength degradation was achieved, and testing efficiency was improved and reference basis, basic parameters are provided for the optimized design of Roebel cables.
Patent Information
- Application Number
- CN202411146644.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-08-21
AI Technical Summary
The prior art methods for testing the stratified strength of Roebel cables are prone to failure, complex sample production and position selection, lack of statistical quantitative description of strength degradation, and cannot accurately evaluate performance and safety.
Roebel single-band layered strength testing method is used, including preparing test samples and welding of anvil head, performing tensile tests, calculating peak load data, fitting strength statistical features using Weibull distribution function, and calculating strength degradation data.
It provides a simple and highly applicable layered strength testing technology, which can quantitatively describe the degree of strength degradation, improve experimental efficiency, and provide a more practical reference basis, providing a basic design for the optimized design of high-temperature superconducting Roebel cable structure. Parameter indicators.
Smart Images

Figure CN118655013B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of material strength testing, and in particular relates to a Roebel single-belt layered strength testing method. Background Art
[0002] Since the discovery of superconductivity, superconducting materials have continued to expand the boundaries of human cognition and the possibility of using clean energy. Among them, REBCO tapes have become the leader of commercial superconducting materials due to their high critical temperature. In order to meet the needs of large current transmission, Roebel cables stacked with REBCO tapes came into being. They have advantages such as high current density and low AC loss, and have great potential in the fields of electricity, physics, and aerospace. The flexible design of Roebel cables can adapt to different shape requirements, such as pancake or Rutherford structures, showing their wide potential. However, existing technologies face several key shortcomings:
[0003] First, the Roebel tape is susceptible to stress when operating in the liquid nitrogen temperature range, resulting in delamination damage and critical current degradation, but its delamination strength at room temperature and liquid nitrogen temperature is still unclear;
[0004] Secondly, the Roebel single tape has complex transposition geometry and cutting state, which leads to challenges in sample preparation, position selection and representativeness in strength testing. The test plan needs to take into account both applicability and efficiency.
[0005] Finally, in terms of data processing, there is a lack of statistically based methods to quantitatively describe the degradation of delamination strength, making it impossible to accurately evaluate the performance and safety of Roebel cables;
[0006] In summary, the existing technology for the research and evaluation of the delamination strength of Roebel cables is insufficient and needs to be further improved and optimized. Summary of the invention
[0007] The purpose of the present invention is to provide a Roebel single-belt delamination strength testing method to solve the problems existing in the above-mentioned prior art.
[0008] To achieve the above object, the present invention provides a Roebel single tape delamination strength testing method, comprising:
[0009] Step 1: Prepare several Roebel single-belt test samples;
[0010] Step 2: prepare a plurality of anvil heads, and weld each of the anvil heads and each of the Roebel single-strip test samples one by one to obtain a plurality of peeling specimens to be tested;
[0011] Step 3: performing a tensile test on each of the peeling samples to be tested based on a set temperature and a set test position, and calculating peak load data of each of the peeling samples to be tested in the tensile test;
[0012] Step 4: Calculate the corresponding strength value data based on the peak load data of each peeling sample to be tested, and fit each strength value data based on the Weibull distribution function to obtain strength statistical characteristics;
[0013] Step 5: Calculate the intensity degradation data of the Roebel single band based on the intensity statistical characteristics.
[0014] Optionally, the step 1 specifically includes:
[0015] A REBCO superconducting tape is obtained, and the REBCO superconducting tape is cut by a laser marking machine based on preset sample geometry data to obtain the Roebel single tape test sample.
[0016] Optionally, the step 2 specifically includes:
[0017] S1: prepare the upper anvil and the lower anvil;
[0018] S2: welding the upper anvil and the lower anvil to the Roebel single-strip test sample based on a preset welding position;
[0019] S3: Repeat S1 to S2 until a preset number of peeling specimens to be tested are prepared.
[0020] Optionally, the upper anvil head and the lower anvil head are both made of oxygen-free copper.
[0021] Optionally, the width of the upper anvil is the same as the width of the corresponding position of the Roebel single-belt test sample; the length and width of the lower anvil are not less than the length and width of the upper anvil, respectively.
[0022] Optionally, welding the upper anvil and the lower anvil to the Roebel single-strip test sample based on a preset welding position specifically includes:
[0023] The contact surfaces of the upper anvil head and the lower anvil head with the Roebel single-strip test sample are polished, cleaned and smeared with solder in sequence to obtain an initial sample;
[0024] The initial sample is placed on a heating table for heating, and after heating is completed, excess solder is removed to obtain the peeling sample to be tested.
[0025] Optionally, calculating the peak load data of each peeling specimen to be tested in the tensile test specifically includes:
[0026] In the tensile test, the load-displacement curve corresponding to each of the peeling samples to be tested is recorded until the sample is damaged, and the corresponding peak load data is calculated based on the load-displacement curve corresponding to each of the peeling samples to be tested.
[0027] Optionally, the corresponding strength value data is calculated based on the peak load data of each peeling sample to be tested, and the specific calculation formula is:
[0028] ;
[0029] In the formula, is the intensity value, is the welding area, The peak load data.
[0030] Optionally, the intensity value data are fitted based on the Weibull distribution function, and the specific calculation formula is:
[0031] ;
[0032] ;
[0033] In the formula, is the Weibull distribution function, is the scale parameter, is the shape parameter, is a positional parameter, is the natural exponential function, is the intensity value, is the reliability function.
[0034] Optionally, the step five specifically includes:
[0035] The intensity degradation data of the Roebel single band at different temperatures and different positions are calculated according to the relative error formula and the intensity statistical characteristics.
[0036] The technical effects of the present invention are:
[0037] The present invention provides a delamination strength testing technology for a high-temperature superconducting Roebel single tape with simple steps and strong applicability, as well as a method for quantitatively describing the degree of strength degradation based on test data; the present invention has high experimental efficiency, and multiple groups of peeled samples to be tested can be prepared at the same time as needed, and experiments can be carried out in parallel to save time costs; the data processing of the present invention is based on Weibull statistics and introduces a reliability evaluation system, which provides a more practical reference basis for engineers; the test technical solution of this embodiment can provide a basic parameter indicator for the industrial application of a high-temperature superconducting Roebel cable structure, and guide the optimal design of the structure. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0039] The drawings constituting a part of the present application are used to provide a further understanding of the present application. The illustrative embodiments and descriptions of the present application are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:
[0040] Figure 1 Schematic diagram of the core steps of the test scheme in an embodiment of the present invention;
[0041] Figure 2 A schematic diagram of the core steps of data collection and processing in an embodiment of the present invention;
[0042] Figure 3 This is a flow chart of the Roebel single-belt delamination strength test in an embodiment of the present invention. DETAILED DESCRIPTION
[0043] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0044] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0045] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those of ordinary skill in the art generally understood by the present invention. Although the present invention describes only preferred methods, any method similar or equivalent to that described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods related to the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.
[0046] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present application description and examples are exemplary only.
[0047] The words “include,” “including,” “have,” “contain,” etc. used in this article are open-ended terms, meaning including but not limited to.
[0048] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present application will be described in detail below with reference to the accompanying drawings and in combination with the embodiments.
[0049] Embodiment 1
[0050] like Figure 1 - Figure 3 As shown, a Roebel single tape delamination strength test method is provided in this embodiment, including: preparing a plurality of Roebel single tape test samples; preparing a plurality of anvils, and welding each of the anvils and each of the Roebel single tape test samples one by one to obtain a plurality of peeling specimens to be tested; performing a tensile test on each of the peeling specimens to be tested based on a set temperature and a set test position, and calculating the peak load data of each of the peeling specimens to be tested in the tensile test; calculating corresponding strength value data based on the peak load data of each of the peeling specimens to be tested, and fitting each of the strength value data based on the Weibull distribution function to obtain strength statistical characteristics; and calculating the strength degradation data of the Roebel single tape based on the strength statistical characteristics.
[0051] This embodiment provides a layered strength test technology for high-temperature superconducting Roebel single tape with simple steps and strong applicability, as well as a method for quantitatively describing the degree of strength degradation based on test data. The preparation process of the Roebel single tape test sample is easy to implement, and the process is applicable to commercial superconducting tapes of different sizes. The raw materials of the anvil are environmentally friendly and easy to obtain, and the anvil can be used repeatedly at different temperatures.
[0052] The experiment is highly efficient, and multiple groups of peeled samples to be tested can be prepared at the same time as needed, and experiments can be carried out in parallel to save time and cost. The data processing of this embodiment is based on Weibull statistics and introduces a reliability evaluation system, which provides a more practical reference basis for engineers; the test technology solution of this embodiment can provide a basic parameter index for the industrial application of high-temperature superconducting Roebel cable structure and guide the optimal design of the structure.
[0053] The specific implementation process of this embodiment is as follows:
[0054] Step 1. Prepare the Roebel single-strip test sample. First, select a 12mm wide REBCO superconducting tape, import the sample geometry file drawn in CAD software into the laser marking machine, and then form a 2mm-6mm wide, 5cm-8cm long narrow strip with transposition characteristics by laser cutting at room temperature.
[0055] Step 2. Production of upper and lower anvils. The anvils are made of oxygen-free copper. The width of the upper anvil should be determined according to the width of the corresponding position of the narrow strip sample after cutting. The length and width of the lower anvil should not be less than the length and width of the upper anvil, respectively. The lower surface of the upper anvil should be consistent with the geometry of the sample.
[0056] Step 3. Preparation of the peeling specimen to be tested. Grind the upper surface of the anvil and the sample to be welded (300-400 mesh), and then clean the sample and the anvil surface with anhydrous ethanol or acetone. Evenly apply solder to the lower surface of the upper anvil, the upper and lower surfaces of the sample, and the upper surface of the lower anvil. Finally, fix the upper anvil, sample and lower anvil in relative positions, remove excess solder and install them on the welding fixture. The composition of the solder paste is Sn96.5 / Ag3.0 / Cu0.5, and the melting point is about 217°C.
[0057] Step 4. Place the welding fixture together with the sample to be peeled on the heating table, and when the temperature rises to 217℃-227℃, remove the excess solder that has seeped out to prevent the upper and lower anvil heads from being welded together.
[0058] Step 5. Turn off the heating table, leave the welding fixture and the peeled sample to be tested to stand and cool naturally to room temperature (about 3-4 hours).
[0059] Step 6. Experimental test of peeling specimen to be tested (strength test): Remove the sample that has been welded and cooled to room temperature from the welding fixture and install it in the fixture of the tensile testing machine. Test at room temperature or liquid nitrogen temperature zone and use displacement loading control at a rate of 0.1mm / min. Collect the load-displacement curve during the stretching process until the sample is destroyed, and record and save the peak load. After destruction, remove the sample from the tensile testing machine and observe the cross-sectional morphology.
[0060] Step 7. Perform strength tests on no less than 30 samples at different positions of the Roebel tape. The specific process of the strength test is as follows: Figure 1 Repeat the test several times as detailed in step 6.
[0061] Step 8. Layered intensity data processing: Figure 2 As shown, the peak load data for each test is obtained from the collected experimental data set. , and follow Calculate the corresponding intensity value ,in Represents the welding area. The mean and variance of the strength at room temperature and 77K are calculated for all test samples, and then the Weibull distribution is used to fit the strength value. Then the statistical characteristics of the strength under different conditions are determined. The cumulative distribution function of the three-parameter Weibull distribution is: ,in, is the Weibull distribution function, represents the scale parameter, represents the shape parameter, Represents positional parameters, is a natural exponential function. These three parameters can be uniquely determined according to the experimental results under the same conditions, among which the position parameter should be determined first. , followed by the scale parameter and shape parameters Then determine it through linear regression analysis. After fitting is completed, the reliability function is introduced , and draw the reliability functions under different situations respectively.
[0062] Step 9. According to the statistical characteristics, the strength degradation of the Roebel strip at different test temperatures and different positions relative to the strength of the uncut strip is calculated, the positions in the Roebel strip that are more prone to damage are determined, and the strength degradation at different reliability levels is given. The degradation is described by the defined relative error:
[0063] ;
[0064] In the formula, Represents different cutting states, Represents uncut REBCO strip, RT represents room temperature, Cutting represents the strip cutting state, Temperature represents the temperature change factor, Degradation (.) represents the degree of strength degradation, represents the strength value at a corresponding temperature and cutting state; therefore, formulas (1)-(4) represent the degradation of the Roebel ribbon at 77K relative to that at room temperature, the degradation of the Roebel ribbon at room temperature relative to the uncut REBCO ribbon at room temperature, the degradation of the Roebel ribbon at 77K relative to the uncut REBCO ribbon at 77K, and the degradation of the Roebel ribbon at 77K relative to the uncut REBCO ribbon at room temperature. The significance of obtaining the degradation situation is that the conclusion of this experiment can be appropriately extended to the Roebel ribbons prepared by other manufacturers and the same process. Under the same reliability, the corresponding strength value is substituted into the above relative error formula to evaluate the strength degradation of the Roebel ribbon.
[0065] The above is only a preferred specific implementation of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present application should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.
Claims
1. A Roebel single tape delamination strength test method, characterized in that: include: Step 1: Obtain a REBCO superconducting tape, and cut the REBCO superconducting tape by a laser marking machine based on preset sample geometry data to obtain a number of Roebel single tape test samples; Step 2: prepare a plurality of anvil heads, and weld each of the anvil heads and each of the Roebel single-strip test samples one by one to obtain a plurality of peeling specimens to be tested; Step 3: performing a tensile test on each of the peeling samples to be tested based on a set temperature and a set test position, and calculating peak load data of each of the peeling samples to be tested in the tensile test; Step 4: Calculate the corresponding strength value data based on the peak load data of each peeling sample to be tested, and fit each strength value data based on the Weibull distribution function to obtain strength statistical characteristics; The intensity value data are fitted based on the Weibull distribution function, and the specific calculation formula is: ; ; In the formula, is the Weibull distribution function, is the scale parameter, is the shape parameter, is a positional parameter, is the natural exponential function, is the intensity value, is the reliability function; Step 5: Calculate the strength degradation data of the Roebel single band at different temperatures and different positions according to the relative error formula and the strength statistical characteristics. The specific calculation formula is: ; In the formula, Represents different cutting states, represents uncut REBCO strip, RT represents room temperature, Cutting represents the strip cutting state, Temperature represents the temperature change factor; Degradation() represents the degree of degradation of the strength value, represents the strength value at a corresponding temperature and cutting state; formulas (1)-(4) respectively represent the degradation of the Roebel ribbon at 77K relative to that at room temperature, the degradation of the Roebel ribbon at room temperature relative to the uncut REBCO ribbon at room temperature, the degradation of the Roebel ribbon at 77K relative to the uncut REBCO ribbon at 77K, and the degradation of the Roebel ribbon at 77K relative to the uncut REBCO ribbon at room temperature.
2. A Roebel single tape delamination strength test method according to claim 1, characterized in that: The step 2 specifically includes: S1: prepare the upper anvil and the lower anvil; S2: welding the upper anvil and the lower anvil to the Roebel single-strip test sample based on a preset welding position; S3: Repeat S1 to S2 until a preset number of peeling specimens to be tested are prepared.
3. A Roebel single tape delamination strength test method according to claim 2, characterized in that: The upper anvil head and the lower anvil head are both made of oxygen-free copper.
4. A Roebel single tape delamination strength test method according to claim 2, characterized in that: The width of the upper anvil is the same as the width of the corresponding position of the Roebel single-belt test sample; the length and width of the lower anvil are not less than the length and width of the upper anvil respectively.
5. A Roebel single tape delamination strength test method according to claim 2, characterized in that: Welding the upper anvil and the lower anvil on the Roebel single-strip test sample based on a preset welding position specifically includes: The contact surfaces of the upper anvil head and the lower anvil head with the Roebel single-strip test sample are polished, cleaned and smeared with solder in sequence to obtain an initial sample; The initial sample is placed on a heating table for heating, and after heating is completed, excess solder is removed to obtain the peeling sample to be tested.
6. A Roebel single tape delamination strength test method according to claim 1, characterized in that: Calculating the peak load data of each peeling specimen to be tested in the tensile test, specifically includes: In the tensile test, the load-displacement curve corresponding to each of the peeling samples to be tested is recorded until the sample is damaged, and the corresponding peak load data is calculated based on the load-displacement curve corresponding to each of the peeling samples to be tested.
7. A Roebel single tape delamination strength test method according to claim 1, characterized in that: The corresponding strength value data is calculated based on the peak load data of each peeling sample to be tested, and the specific calculation formula is: ; In the formula, is the intensity value, is the welding area, The peak load data.