Flame retardant bamboo-wood composite material and preparation method thereof

By preparing MgO-deposited SiO2/TiO2 nanospheres and modifying them with aminosilane coupling agents, combined with the reaction of benzaldehyde and DOPO, flame-retardant nanospheres were prepared. These nanospheres were then hot-pressed with bamboo and wood powders and coated with tung oil, solving the problems of flammability and uneven corrosion resistance in bamboo and wood materials. This resulted in a highly efficient, flame-retardant, and environmentally friendly bamboo and wood composite material.

CN118667284BActive Publication Date: 2024-11-26湖南鲁丽木业有限公司 +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411148172.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-26
Estimated Expiration
2044-08-21

AI Technical Summary

Technical Problem

Existing bamboo and wood materials suffer from uneven anti-corrosion treatment during preparation, high flammability, and potential pollution from traditional flame retardants.

Method used

Flame-retardant nanospheres were prepared by depositing SiO2/TiO2 nanospheres with MgO and modifying them with aminosilane coupling agents, and then reacting them with benzaldehyde and DOPO. The nanospheres were then added to acrylic resin emulsion and hot-pressed with bamboo and wood powder, and the surface was coated with tung oil to form a flame-retardant bamboo and wood composite material.

Benefits of technology

This research has resulted in bamboo-wood composite materials with excellent flame retardant properties, good mechanical properties, safety and environmental friendliness, waterproof and moisture-resistant properties, and good corrosion resistance, which have broad application prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention proposes a flame retardant bamboo-wood composite material and a preparation method thereof, and belongs to the technical field of flame retardant materials. After preparing MgO deposited SiO2 / TiO2 nanospheres, the surface is modified by an aminosilane coupling agent, reacted with benzaldehyde and 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide to obtain flame retardant nanospheres, the surface is modified by a double bond silane coupling agent, added to an acrylic monomer, heated to initiate a reaction to obtain a flame retardant acrylic resin emulsion, mixed with bamboo powder and wood powder, hot pressed, dried to obtain a bamboo-wood composite material, coated with a layer of tung oil on the surface, dried to obtain a flame retardant bamboo-wood composite material. The flame retardant bamboo-wood composite material prepared by the invention has good flame retardant properties, good mechanical properties, safety and environmental protection, waterproof and moisture resistant, good anticorrosive properties, good thermal stability, and has broad application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of flame retardant materials, and in particular to a flame retardant bamboo-wood composite material and a preparation method thereof. Background Art

[0002] Nowadays, people's living standards are getting higher and higher. Housing is a rigid demand for people. Everyone has this demand. However, when decorating a house, more and more chemicals are used. These chemicals will emit a series of chemical elements during use. Some of these elements are pollution-free. But some are highly polluting. Therefore, people begin to pay attention to environmental protection and the use of environmentally friendly products. Products such as bamboo, wood and hemp are natural products. They have no radiation and will not emit polluting elements. They are environmentally friendly products and can also make people feel close to nature. Products made from these raw materials are used in many places, such as curtains, floors or beds and chairs. However, these products themselves are flammable. Improper use at home can easily cause fires, especially thin items such as curtains, which are more likely to ignite. How to prepare products with good flame retardant properties will have far-reaching significance.

[0003] Chinese patent application CN1457964A discloses a flame-retardant formed bamboo material and its production method, which comprises the following steps: firstly splitting and sawing the bamboo material into bamboo pieces, then soaking each bamboo piece in a preservative for steaming and preservative treatment, then splitting the dried bamboo pieces into bamboo filaments, and then soaking the bamboo filaments in a flame-retardant liquid prepared from phosphate, boric acid or borax. Then, the bamboo filaments containing the flame-retardant liquid after drying are soaked and dried in a waterproof adhesive; the dried bamboo filaments containing the flame-retardant liquid are placed in a mold for compression shaping, and then the mold is placed in a drying kiln for demoulding after solidification, cooling and shaping. This treatment is a multi-step process, with two splitting processes, and the anti-corrosion treatment can generally form an anti-corrosion layer on the surface of the bamboo piece, but it may not penetrate into the inside of the bamboo piece. In this way, when the anti-corrosion treated bamboo piece is made into bamboo filaments, the parts that have not been treated with anti-corrosion inside may be completely exposed to the outside, and when the product is made, the anti-corrosion treatment of the part may not be in place to form corrosion points, thereby affecting the overall performance. Summary of the invention

[0004] The purpose of the present invention is to provide a flame retardant bamboo-wood composite material and a preparation method thereof, which has good flame retardant properties, good mechanical properties, safety and environmental protection, waterproof and moisture-resistant, good anti-corrosion properties, good thermal stability, and has broad application prospects.

[0005] The technical solution of the present invention is achieved in this way:

[0006] The invention provides a method for preparing a flame-retardant bamboo-wood composite material. The method comprises the following steps: preparing MgO deposited SiO2 / TiO2 nanospheres, modifying the surface of the nanospheres with an aminosilane coupling agent, reacting the nanospheres with benzaldehyde and 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide to obtain flame-retardant nanospheres, modifying the surface of the nanospheres with a double-bond silane coupling agent, adding the nanospheres to acrylic acid monomers, heating to initiate a reaction to obtain flame-retardant acrylic resin emulsion, mixing the nanospheres with bamboo powder and wood powder, hot pressing to form the nanospheres, drying the nanospheres, coating the nanospheres with a layer of tung oil, and drying the nanospheres to obtain flame-retardant bamboo-wood composite material.

[0007] As a further improvement of the present invention, the following steps are comprised:

[0008] S1. Preparation of MgO-deposited SiO2 / TiO2 nanospheres: The magnesium salt, ethanol, ammonia and water were mixed uniformly, tetraethyl orthosilicate and tetrabutyl titanate were added, the reaction was hydrolyzed, centrifuged, washed, dried, and calcined to obtain MgO-deposited SiO2 / TiO2 nanospheres;

[0009] S2 first silane coupling agent modification: The MgO deposited SiO2 / TiO2 nanospheres prepared in step S1 were added to an ethanol solution, a first silane coupling agent was added, the reaction was heated and stirred, centrifuged, washed, and dried to obtain modified MgO deposited SiO2 / TiO2 nanospheres;

[0010] S3 flame retardant modification: the modified MgO deposited SiO2 / TiO2 nanospheres obtained in step S2, benzaldehyde, sodium acetate were added to ethanol, heated under inert gas protection, reflux reaction, and then 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide was added, the reaction was continued, centrifuged, washed, and dried to obtain flame retardant nanospheres;

[0011] S4 second silane coupling agent modification: The flame retardant nanospheres obtained in step S3 were added to an ethanol solution, a second silane coupling agent was added, the reaction was heated and stirred, centrifuged, washed, and dried to obtain modified nanospheres;

[0012] S5 flame retardant acrylic resin emulsion preparation: the modified nanospheres prepared in step S4, methyl methacrylate, acrylic acid, butyl acrylate, styrene was added to water, stirred to mix, an initiator was added, the reaction was heated with stirring, the pH value of the solution was adjusted, a dispersant, a defoamer, a leveling agent was added, and stirring was continued to obtain a flame retardant acrylic resin emulsion;

[0013] S6 molding: The bamboo powder, wood powder mixed evenly, adding the flame retardant acrylic resin emulsion prepared in step S5, hot pressing, drying, to obtain a bamboo composite material;

[0014] S7. Preparation of flame-retardant bamboo-wood composite material: The surface of the bamboo-wood composite material obtained in step S6 is coated with a layer of tung oil and dried to obtain a flame-retardant bamboo-wood composite material.

[0015] As a further improvement of the present invention, the mass ratio of the magnesium salt, ethanol, ammonia water, water, tetraethyl orthosilicate and tetrabutyl titanate in step S1 is (3-5): (150-170): (2-4): (15-20): (10-12): (7-10), the magnesium salt is selected from at least one of magnesium chloride, magnesium sulfate and magnesium nitrate, the temperature of the hydrolysis reaction is 30-35°C, the time is 5-7h, and the calcination temperature is 500-700°C, and the time is 2-4h.

[0016] As a further improvement of the present invention, in step S2, the mass ratio of the MgO deposited SiO2 / TiO2 nanospheres and the first silane coupling agent is 100:(17-22), the first silane coupling agent is selected from at least one of KH550, KH602, and KH792, preferably, a mixture of KH602 and KH792, with a mass ratio of (5-7):(1-3), the temperature of the heating and stirring reaction is 40-50°C, and the time is 2-4h.

[0017] As a further improvement of the present invention, the mass ratio of the modified MgO deposited SiO2 / TiO2 nanospheres, benzaldehyde, sodium acetate, and 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide in step S3 is 100:(25-30):(1-3):(32-37), the heating reflux reaction time is 3-5 hours, and the continued reaction time is 10-12 hours.

[0018] As a further improvement of the present invention, the mass ratio of the flame retardant nanospheres and the second silane coupling agent in step S4 is 100:5-7, the second silane coupling agent is selected from at least one of KH570, A151, and A171, and the temperature of the heating and stirring reaction is 40-50° C. and the time is 1-3 hours.

[0019] As a further improvement of the present invention, the mass ratio of the modified nanospheres, methyl methacrylate, acrylic acid, butyl acrylate, styrene, dispersant, defoamer and leveling agent in step S5 is (15-20): (5-7): (3-5): (40-50): (20-40): (0.5-1): (0.1-0.2): (0.5-0.8), the initiator is selected from at least one of potassium persulfate, sodium persulfate and ammonium persulfate, the dispersant is BYK-190, the defoamer is BYK-024, the leveling agent is DAPRO W-77, the amount of the initiator added is 0.5-1wt% of the total mass of the system, the temperature of the heating and stirring reaction is 45-55°C, the time is 3-5h, the pH value of the solution is adjusted to 8-9, and the stirring time is 1-3h.

[0020] As a further improvement of the present invention, the mass ratio of bamboo powder, wood powder and flame retardant acrylic resin emulsion in step S6 is (15-20): (10-12): (17-22), the temperature of the hot pressing molding is 140-150°C, the pressure is 5.5-7Mpa, and the time is 10-20min; the coating amount of tung oil in step S7 is 0.03-0.05g / cm 2 .

[0021] As a further improvement of the present invention, specifically comprise the following steps:

[0022] S1. Preparation of MgO-deposited SiO2 / TiO2 nanospheres: 3-5 parts by weight of magnesium salt, 150-170 parts by weight of ethanol, 2-4 parts by weight of ammonia and 15-20 parts by weight of water were mixed uniformly, 10-12 parts by weight of ethyl orthosilicate and 7-10 parts by weight of tetrabutyl titanate were added, and the reaction was hydrolyzed at 30-35°C for 5-7h, centrifuged, washed, dried, and calcined at 500-700°C for 2-4h to obtain MgO-deposited SiO2 / TiO2 nanospheres;

[0023] S2. Modification of the first silane coupling agent: adding 100 parts by weight of the MgO-deposited SiO2 / TiO2 nanospheres obtained in step S1 to 500 parts by weight of a 70-80wt% ethanol solution, adding 17-22 parts by weight of the first silane coupling agent, heating to 40-50°C, stirring the reaction for 2-4h, centrifuging, washing, and drying to obtain modified MgO-deposited SiO2 / TiO2 nanospheres;

[0024] The first silane coupling agent is a mixture of KH602 and KH792, with a mass ratio of 5-7:1-3;

[0025] S3 flame retardant modification: 100 parts by weight of the modified MgO deposited SiO2 / TiO2 nanospheres obtained in step S2, 25-30 parts by weight of benzaldehyde, 1-3 parts by weight of sodium acetate were added to ethanol, and the reaction was heated under reflux under inert gas for 3-5h, and then 32-37 parts by weight of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide was added, and the reaction was continued for 10-12h, centrifuged, washed, and dried to obtain flame retardant nanospheres;

[0026] S4. Modification of the second silane coupling agent: 100 parts by weight of the flame-retardant nanospheres obtained in step S3 were added to an ethanol solution, 5-7 parts by weight of a second silane coupling agent were added, heated to 40-50 ° C, stirred for 1-3h, centrifuged, washed, and dried to obtain modified nanospheres;

[0027] S5. Preparation of flame retardant acrylic resin emulsion: 15-20 parts by weight of the modified nanospheres prepared in step S4, 5-7 parts by weight of methyl methacrylate, 3-5 parts by weight of acrylic acid, 40-50 parts by weight of butyl acrylate, 20-40 parts by weight of styrene are mixed and added to 300 parts by weight of water, stirred and mixed evenly, an initiator is added, wherein the initiator is added in an amount of 0.5-1wt% of the total mass of the system, heated to 45-55°C, stirred for 3-5h, the pH value of the solution is adjusted to 8-9, 0.5-1 parts by weight of dispersant BYK-190, 0.1-0.2 parts by weight of defoamer BYK-024, 0.5-0.8 parts by weight of leveling agent DAPRO W-77 are added, stirring is continued for 1-3h to obtain a flame retardant acrylic resin emulsion;

[0028] S6 molding: 15-20 parts by weight of bamboo powder, 10-12 parts by weight of wood powder mixed, added 17-22 parts by weight of the flame retardant acrylic resin emulsion prepared in step S5, a temperature of 140-150 ℃, a pressure of 5.5-7Mpa, hot pressing 10-20min, dried to obtain a bamboo composite material;

[0029] S7. Preparation of flame-retardant bamboo composite material: The surface of the bamboo composite material obtained in step S6 is coated with a layer of tung oil, the coating amount is 0.03-0.05g / cm 2 , and dried to obtain a flame retardant bamboo-wood composite material.

[0030] The present invention further protects a flame retardant bamboo-wood composite material prepared by the above preparation method.

[0031] The present invention has the following beneficial effects:

[0032] Compared with traditional flame retardants such as halogen flame retardants, metal flame retardants, and phosphorus flame retardants, nanocomposite flame retardant materials can significantly improve the mechanical properties, flame retardant properties, thermal stability, etc. of composite materials. The present invention prepares a MgO-deposited SiO2 / TiO2 nanosphere, which can form a magnesium oxide layer on the surface of the composite material under the MgO combustion condition. This magnesium oxide layer has the characteristics of being difficult to melt and difficult to volatilize, and can prevent the combustion material from continuing to burn to a certain extent; at the same time, the prepared SiO2 / TiO2 nanosphere can significantly improve the mechanical properties and thermal stability of the composite material, and at the same time, can also improve the antibacterial and anticorrosive properties of wood.

[0033] The obtained MgO deposited SiO2 / TiO2 nanospheres were coupled with a silane coupling agent with an amino group, so that the surface of the nanospheres was connected with an amino group, and the amino group further reacted with benzaldehyde to form an imine, and then reacted with the flame retardant intermediate 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide (DOPO) to obtain flame retardant nanospheres with phosphorus, nitrogen and silicon elements, which can synergistically flame retardant multiple elements and achieve better flame retardant effect. Among them, the flame retardant containing phosphorus and nitrogen elements can promote the formation of a stable carbon layer in the condensation phase, remove ·H and ·OH free radicals, protect the composite material from heat and oxygen, and also have the advantages of non-toxic, odorless, non-corrosive gas, low hygroscopicity and high thermal stability. At the same time, the silicon element can form a carbon protective layer on the surface of the material, produce free radical capture active intermediates, achieve flame retardant effect, have carbonization and smoke suppression effect, and have good flame retardancy and environmental friendliness.

[0034] Subsequently, the surface of the flame-retardant nanospheres is further modified with a silane coupling agent with double bonds, so that they can be connected to the polyacrylate polymer chain through polymerization reaction with acrylic monomers, so that the nanospheres can be evenly distributed inside the composite material, thereby improving the compatibility of the nanospheres, thereby effectively improving the flame retardant properties and mechanical properties of the bamboo-wood composite material. In the process of preparing the bamboo-wood composite material, bamboo powder, wood powder and acrylic emulsion are added for hot pressing molding, and no volatile organic compounds are produced in the whole process, which is safer and more environmentally friendly.

[0035] Finally, a layer of tung oil is coated on the surface of the prepared bamboo-wood composite material. The main component of tung oil is α-tung oil triglyceride, which contains multiple unsaturated conjugated double bonds in its molecular structure. After being coated on the surface of the bamboo-wood composite material, it can be cured into a film when reacting with oxygen in the air. The film has the properties of being waterproof and moisture-resistant, having strong adhesion, and being resistant to light, thereby greatly improving the waterproof and anti-corrosion properties of the bamboo-wood composite material. After the tung oil that has penetrated into the interior of the bamboo-wood composite material is cured in situ, it can strengthen and enhance the cell wall of the wood. It has the effects of stabilization, hydrophobicity, and wear resistance in the normal use of wooden products, and can further improve the flame retardant effect in the event of a fire.

[0036] The flame retardant bamboo-wood composite material prepared by the invention has good flame retardant performance, good mechanical properties, safety and environmental protection, waterproof and moisture-resistant, good anticorrosive performance, good thermal stability, and has broad application prospects. DETAILED DESCRIPTION

[0037] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0038] Example 1

[0039] This embodiment provides a method for preparing a flame retardant bamboo-wood composite material, which specifically comprises the following steps:

[0040] S1. Preparation of MgO-deposited SiO2 / TiO2 nanospheres: 3 parts by weight of magnesium chloride, 150 parts by weight of ethanol, 2 parts by weight of ammonia and 15 parts by weight of water were stirred and mixed for 20 min, 10 parts by weight of ethyl orthosilicate and 7 parts by weight of tetrabutyl titanate were added, and the reaction was hydrolyzed at 30°C for 5 h, centrifuged, washed, dried, and calcined at 500°C for 2 h to obtain MgO-deposited SiO2 / TiO2 nanospheres;

[0041] S2. Modification of the first silane coupling agent: 100 parts by weight of the MgO-deposited SiO2 / TiO2 nanospheres prepared in step S1 were added to 500 parts by weight of a 70wt% ethanol solution, 17 parts by weight of a first silane coupling agent were added, heated to 40°C, stirred for 2h, centrifuged, washed, and dried to obtain modified MgO-deposited SiO2 / TiO2 nanospheres;

[0042] The first silane coupling agent is a mixture of KH602 and KH792, with a mass ratio of 5:1;

[0043] S3 flame retardant modification: 100 parts by weight of the modified MgO deposited SiO2 / TiO2 nanospheres prepared in step S2, 25 parts by weight of benzaldehyde, 1 part by weight of sodium acetate were added to 500 parts by weight of ethanol, and the reaction was heated under reflux for 3 hours under nitrogen protection, and then 32 parts by weight of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide was added, and the reaction was continued for 10 hours, centrifuged, washed, and dried to obtain flame retardant nanospheres;

[0044] S4. Modification of the second silane coupling agent: 100 parts by weight of the flame-retardant nanospheres obtained in step S3 were added to 300 parts by weight of a 70wt% ethanol solution, 5 parts by weight of a silane coupling agent A151 were added, heated to 40 ° C, stirred for 1 h, centrifuged, washed, and dried to obtain modified nanospheres;

[0045] S5. Preparation of flame retardant acrylic resin emulsion: 15 parts by weight of the modified nanospheres prepared in step S4, 5 parts by weight of methyl methacrylate, 3 parts by weight of acrylic acid, 40 parts by weight of butyl acrylate, and 20 parts by weight of styrene were mixed and added to 300 parts by weight of water, stirred and mixed for 20 minutes, potassium persulfate was added, and the amount of potassium persulfate added was 0.5wt% of the total mass of the system, heated to 45°C, stirred and reacted for 3 hours, the pH value of the solution was adjusted to 8, 0.5 parts by weight of dispersant BYK-190, 0.1 parts by weight of defoamer BYK-024, and 0.5 parts by weight of leveling agent DAPRO W-77 were added, and stirring was continued for 1 hour to obtain a flame retardant acrylic resin emulsion;

[0046] S6 molding: 15 parts by weight of bamboo powder, 10 parts by weight of wood powder was stirred and mixed for 15min, 17 parts by weight of the flame retardant acrylic resin emulsion prepared in step S5 was added, the temperature was 140 ℃, the pressure was 5.5Mpa, hot pressing for 10min, and dried to obtain a bamboo composite material;

[0047] S7. Preparation of flame-retardant bamboo composite material: The surface of the bamboo composite material obtained in step S6 is coated with a layer of tung oil, the coating amount is 0.03g / cm 2 , and dried to obtain a flame retardant bamboo-wood composite material.

[0048] Example 2

[0049] This embodiment provides a method for preparing a flame retardant bamboo-wood composite material, which specifically comprises the following steps:

[0050] S1. Preparation of MgO-deposited SiO2 / TiO2 nanospheres: 5 parts by weight of magnesium sulfate, 170 parts by weight of ethanol, 4 parts by weight of ammonia and 20 parts by weight of water were stirred and mixed for 20 minutes, 12 parts by weight of ethyl orthosilicate and 10 parts by weight of tetrabutyl titanate were added, and the reaction was hydrolyzed at 35°C for 7 hours, centrifuged, washed, dried, and calcined at 700°C for 4 hours to obtain MgO-deposited SiO2 / TiO2 nanospheres;

[0051] S2. Modification of the first silane coupling agent: 100 parts by weight of the MgO-deposited SiO2 / TiO2 nanospheres prepared in step S1 were added to 500 parts by weight of an 80wt% ethanol solution, 22 parts by weight of the first silane coupling agent were added, heated to 50°C, stirred for 4h, centrifuged, washed, and dried to obtain modified MgO-deposited SiO2 / TiO2 nanospheres;

[0052] The first silane coupling agent is a mixture of KH602 and KH792, with a mass ratio of 7:3;

[0053] S3 flame retardant modification: 100 parts by weight of the modified MgO deposited SiO2 / TiO2 nanospheres prepared in step S2, 30 parts by weight of benzaldehyde, 3 parts by weight of sodium acetate were added to 500 parts by weight of ethanol, and the reaction was heated under reflux for 5 hours under nitrogen protection, and then 37 parts by weight of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide was added, and the reaction was continued for 12 hours, centrifuged, washed, and dried to obtain flame retardant nanospheres;

[0054] S4. Modification of the second silane coupling agent: 100 parts by weight of the flame-retardant nanospheres obtained in step S3 were added to 300 parts by weight of a 70wt% ethanol solution, 7 parts by weight of a silane coupling agent KH570 were added, heated to 50 ° C, stirred for 3h, centrifuged, washed, and dried to obtain modified nanospheres;

[0055] S5. Preparation of flame retardant acrylic resin emulsion: 20 parts by weight of the modified nanospheres prepared in step S4, 7 parts by weight of methyl methacrylate, 5 parts by weight of acrylic acid, 50 parts by weight of butyl acrylate, and 40 parts by weight of styrene were mixed and added to 300 parts by weight of water, stirred and mixed for 20 minutes, sodium persulfate was added, and the amount of sodium persulfate added was 1wt% of the total mass of the system, heated to 55 ° C, stirred and reacted for 5 hours, the pH value of the solution was adjusted to 9, 1 part by weight of dispersant BYK-190, 0.2 parts by weight of defoamer BYK-024, and 0.8 parts by weight of leveling agent DAPRO W-77 were added, and stirring was continued for 3 hours to obtain a flame retardant acrylic resin emulsion;

[0056] S6 molding: 20 parts by weight of bamboo powder, 12 parts by weight of wood powder was stirred and mixed for 15min, 22 parts by weight of the flame retardant acrylic resin emulsion prepared in step S5 was added, the temperature was 150 ℃, the pressure was 7Mpa, hot pressing for 20min, and dried to obtain a bamboo composite material;

[0057] S7. Preparation of flame-retardant bamboo composite material: The surface of the bamboo composite material obtained in step S6 is coated with a layer of tung oil, the coating amount is 0.04g / cm 2 , and dried to obtain a flame retardant bamboo-wood composite material.

[0058] Example 3

[0059] This embodiment provides a method for preparing a flame retardant bamboo-wood composite material, which specifically comprises the following steps:

[0060] S1. Preparation of MgO-deposited SiO2 / TiO2 nanospheres: 4 parts by weight of magnesium nitrate, 160 parts by weight of ethanol, 3 parts by weight of aqueous ammonia and 17 parts by weight of water were stirred and mixed for 20 minutes, 11 parts by weight of ethyl orthosilicate and 8.5 parts by weight of tetrabutyl titanate were added, and the reaction was hydrolyzed at 32°C for 6 hours, centrifuged, washed, dried, and calcined at 600°C for 3 hours to obtain MgO-deposited SiO2 / TiO2 nanospheres;

[0061] S2. Modification of the first silane coupling agent: 100 parts by weight of the MgO-deposited SiO2 / TiO2 nanospheres prepared in step S1 were added to 500 parts by weight of a 75wt% ethanol solution, 20 parts by weight of the first silane coupling agent were added, heated to 45°C, stirred for 3h, centrifuged, washed, and dried to obtain modified MgO-deposited SiO2 / TiO2 nanospheres;

[0062] The first silane coupling agent is a mixture of KH602 and KH792, with a mass ratio of 6:2;

[0063] S3 flame retardant modification: 100 parts by weight of the modified MgO deposited SiO2 / TiO2 nanospheres obtained in step S2, 27 parts by weight of benzaldehyde, 2 parts by weight of sodium acetate were added to 500 parts by weight of ethanol, and the reaction was heated under reflux for 4 hours under nitrogen protection, and then 35 parts by weight of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide was added, and the reaction was continued for 11 hours, centrifuged, washed, and dried to obtain flame retardant nanospheres;

[0064] S4. Modification of the second silane coupling agent: 100 parts by weight of the flame-retardant nanospheres obtained in step S3 were added to 300 parts by weight of a 70wt% ethanol solution, 6 parts by weight of a silane coupling agent KH570 were added, heated to 45 ° C, stirred for 2h, centrifuged, washed, and dried to obtain modified nanospheres;

[0065] S5. Preparation of flame retardant acrylic resin emulsion: 17 parts by weight of the modified nanospheres prepared in step S4, 6 parts by weight of methyl methacrylate, 4 parts by weight of acrylic acid, 45 parts by weight of butyl acrylate, and 30 parts by weight of styrene were mixed and added to 300 parts by weight of water, stirred and mixed for 20 minutes, and ammonium persulfate was added, wherein the amount of ammonium persulfate added was 0.7wt% of the total mass of the system, heated to 50°C, stirred and reacted for 4 hours, the pH value of the solution was adjusted to 8.5, 0.7 parts by weight of dispersant BYK-190, 0.15 parts by weight of defoamer BYK-024, and 0.65 parts by weight of leveling agent DAPRO W-77 were added, and stirring was continued for 2 hours to obtain a flame retardant acrylic resin emulsion;

[0066] S6 molding: 17 parts by weight of bamboo powder, 11 parts by weight of wood powder was stirred and mixed for 15min, 20 parts by weight of the flame retardant acrylic resin emulsion prepared in step S5 was added, the temperature was 145 ℃, the pressure was 6.4Mpa, hot pressing for 15min, and dried to obtain a bamboo composite material;

[0067] S7. Preparation of flame-retardant bamboo composite material: The surface of the bamboo composite material obtained in step S6 is coated with a layer of tung oil, the coating amount is 0.05g / cm 2 , and dried to obtain a flame retardant bamboo-wood composite material.

[0068] Example 4

[0069] Compared with Example 3, the difference is that the first silane coupling agent is a single KH602.

[0070] Example 5

[0071] Compared with Example 3, the difference is that the first silane coupling agent is a single KH792.

[0072] Comparative Example 1

[0073] Compared with Example 3, the difference is that magnesium nitrate is not added in step S1.

[0074] The details are as follows:

[0075] S1. Preparation of SiO2 / TiO2 nanospheres: 170 parts by weight of ethanol, 4 parts by weight of ammonia water and 20 parts by weight of water were stirred and mixed for 20 minutes, 12 parts by weight of ethyl orthosilicate and 10 parts by weight of tetrabutyl titanate were added, hydrolysis reaction was carried out at 35°C for 7 hours, centrifuged, washed, dried, and calcined at 700°C for 4 hours to obtain SiO2 / TiO2 nanospheres.

[0076] Comparative Example 2

[0077] Compared with Example 3, the difference is that tetrabutyl titanate is not added in step S1.

[0078] The details are as follows:

[0079] S1. Preparation of MgO-deposited SiO2 nanospheres: 5 parts by weight of magnesium sulfate, 170 parts by weight of ethanol, 4 parts by weight of ammonia water and 20 parts by weight of water were stirred and mixed for 20 minutes, 22 parts by weight of tetraethyl orthosilicate were added, hydrolysis reaction was carried out at 35°C for 7 hours, centrifuged, washed, dried, and calcined at 700°C for 4 hours to obtain MgO-deposited SiO2 nanospheres.

[0080] Comparative Example 3

[0081] Compared with Example 3, the difference is that step S2 and step S3 are not performed.

[0082] The details are as follows:

[0083] S1. Preparation of MgO-deposited SiO2 / TiO2 nanospheres: 4 parts by weight of magnesium nitrate, 160 parts by weight of ethanol, 3 parts by weight of aqueous ammonia and 17 parts by weight of water were stirred and mixed for 20 minutes, 11 parts by weight of ethyl orthosilicate and 8.5 parts by weight of tetrabutyl titanate were added, and the reaction was hydrolyzed at 32°C for 6 hours, centrifuged, washed, dried, and calcined at 600°C for 3 hours to obtain MgO-deposited SiO2 / TiO2 nanospheres;

[0084] S2. Modification of the second silane coupling agent: 100 parts by weight of the MgO-deposited SiO2 / TiO2 nanospheres prepared in step S1 were added to 300 parts by weight of a 70wt% ethanol solution, 6 parts by weight of a silane coupling agent KH570 were added, heated to 45 ° C, stirred for 2h, centrifuged, washed, and dried to obtain modified nanospheres;

[0085] S3. Preparation of flame retardant acrylic resin emulsion: 17 parts by weight of the modified nanospheres prepared in step S2, 6 parts by weight of methyl methacrylate, 4 parts by weight of acrylic acid, 45 parts by weight of butyl acrylate, and 30 parts by weight of styrene were mixed and added to 300 parts by weight of water, stirred and mixed for 20 minutes, and ammonium persulfate was added, wherein the amount of ammonium persulfate added was 0.7wt% of the total mass of the system, heated to 50°C, stirred and reacted for 4 hours, the pH value of the solution was adjusted to 8.5, 0.7 parts by weight of dispersant BYK-190, 0.15 parts by weight of defoamer BYK-024, and 0.65 parts by weight of leveling agent DAPRO W-77 were added, and stirring was continued for 2 hours to obtain a flame retardant acrylic resin emulsion;

[0086] S4 molding: 17 parts by weight of bamboo powder, 11 parts by weight of wood powder was stirred and mixed for 15min, 20 parts by weight of the flame retardant acrylic resin emulsion prepared in step S3 was added, the temperature was 145 ℃, the pressure was 6.4Mpa, hot pressing for 15min, and dried to obtain a bamboo composite material;

[0087] S5. Preparation of flame-retardant bamboo composite materials: The surface of the bamboo composite material obtained in step S4 was coated with a layer of tung oil, the coating amount was 0.05g / cm 2 , and dried to obtain a flame retardant bamboo-wood composite material.

[0088] Comparative Example 4

[0089] Compared with Example 3, the difference is that step S3 is not performed.

[0090] The details are as follows:

[0091] S1. Preparation of MgO-deposited SiO2 / TiO2 nanospheres: 4 parts by weight of magnesium nitrate, 160 parts by weight of ethanol, 3 parts by weight of aqueous ammonia and 17 parts by weight of water were stirred and mixed for 20 minutes, 11 parts by weight of ethyl orthosilicate and 8.5 parts by weight of tetrabutyl titanate were added, and the reaction was hydrolyzed at 32°C for 6 hours, centrifuged, washed, dried, and calcined at 600°C for 3 hours to obtain MgO-deposited SiO2 / TiO2 nanospheres;

[0092] S2. Modification of the first silane coupling agent: 100 parts by weight of the MgO-deposited SiO2 / TiO2 nanospheres prepared in step S1 were added to 500 parts by weight of a 75wt% ethanol solution, 20 parts by weight of the first silane coupling agent were added, heated to 45°C, stirred for 3h, centrifuged, washed, and dried to obtain modified MgO-deposited SiO2 / TiO2 nanospheres;

[0093] The first silane coupling agent is a mixture of KH602 and KH792, with a mass ratio of 6:2;

[0094] S3. Modification of the second silane coupling agent: 100 parts by weight of the modified MgO deposited SiO2 / TiO2 nanospheres prepared in step S2 were added to 300 parts by weight of a 70wt% ethanol solution, 6 parts by weight of a silane coupling agent KH570 were added, heated to 45 ° C, stirred for 2h, centrifuged, washed, and dried to obtain modified nanospheres;

[0095] S4. Preparation of flame retardant acrylic resin emulsion: 17 parts by weight of the modified nanospheres prepared in step S3, 6 parts by weight of methyl methacrylate, 4 parts by weight of acrylic acid, 45 parts by weight of butyl acrylate, and 30 parts by weight of styrene were mixed and added to 300 parts by weight of water, stirred and mixed for 20 minutes, and ammonium persulfate was added, wherein the amount of ammonium persulfate added was 0.7wt% of the total mass of the system, heated to 50°C, stirred and reacted for 4 hours, the pH value of the solution was adjusted to 8.5, 0.7 parts by weight of dispersant BYK-190, 0.15 parts by weight of defoamer BYK-024, and 0.65 parts by weight of leveling agent DAPRO W-77 were added, and stirring was continued for 2 hours to obtain a flame retardant acrylic resin emulsion;

[0096] S5 molding: 17 parts by weight of bamboo powder, 11 parts by weight of wood powder was stirred and mixed for 15min, 20 parts by weight of the flame retardant acrylic resin emulsion prepared in step S4 was added, the temperature was 145 ℃, the pressure was 6.4Mpa, hot pressing for 15min, and dried to obtain a bamboo composite material;

[0097] S6. Preparation of flame-retardant bamboo composite material: The surface of the bamboo composite material obtained in step S5 is coated with a layer of tung oil, the coating amount is 0.05g / cm 2 , and dried to obtain a flame retardant bamboo-wood composite material.

[0098] Comparative Example 5

[0099] Compared with Example 3, the difference is that step S4 is not performed.

[0100] The details are as follows:

[0101] S1. Preparation of MgO-deposited SiO2 / TiO2 nanospheres: 4 parts by weight of magnesium nitrate, 160 parts by weight of ethanol, 3 parts by weight of aqueous ammonia and 17 parts by weight of water were stirred and mixed for 20 minutes, 11 parts by weight of ethyl orthosilicate and 8.5 parts by weight of tetrabutyl titanate were added, and the reaction was hydrolyzed at 32°C for 6 hours, centrifuged, washed, dried, and calcined at 600°C for 3 hours to obtain MgO-deposited SiO2 / TiO2 nanospheres;

[0102] S2. Modification of the first silane coupling agent: 100 parts by weight of the MgO-deposited SiO2 / TiO2 nanospheres prepared in step S1 were added to 500 parts by weight of a 75wt% ethanol solution, 20 parts by weight of the first silane coupling agent were added, heated to 45°C, stirred for 3h, centrifuged, washed, and dried to obtain modified MgO-deposited SiO2 / TiO2 nanospheres;

[0103] The first silane coupling agent is a mixture of KH602 and KH792, with a mass ratio of 6:2;

[0104] S3 flame retardant modification: 100 parts by weight of the modified MgO deposited SiO2 / TiO2 nanospheres obtained in step S2, 27 parts by weight of benzaldehyde, 2 parts by weight of sodium acetate were added to 500 parts by weight of ethanol, and the reaction was heated under reflux for 4 hours under nitrogen protection, and then 35 parts by weight of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide was added, and the reaction was continued for 11 hours, centrifuged, washed, and dried to obtain flame retardant nanospheres;

[0105] S4. Preparation of flame-retardant acrylic resin emulsion: 17 parts by weight of the flame-retardant nanospheres prepared in step S3, 6 parts by weight of methyl methacrylate, 4 parts by weight of acrylic acid, 45 parts by weight of butyl acrylate, and 30 parts by weight of styrene were mixed and added to 300 parts by weight of water, stirred and mixed for 20 minutes, and ammonium persulfate was added, wherein the amount of ammonium persulfate added was 0.7wt% of the total mass of the system, heated to 50°C, stirred and reacted for 4 hours, the pH value of the solution was adjusted to 8.5, 0.7 parts by weight of dispersant BYK-190, 0.15 parts by weight of defoamer BYK-024, and 0.65 parts by weight of leveling agent DAPRO W-77 were added, and stirring was continued for 2 hours to obtain a flame-retardant acrylic resin emulsion;

[0106] S5 molding: 17 parts by weight of bamboo powder, 11 parts by weight of wood powder was stirred and mixed for 15min, 20 parts by weight of the flame retardant acrylic resin emulsion prepared in step S4 was added, the temperature was 145 ℃, the pressure was 6.4Mpa, hot pressing for 15min, and dried to obtain a bamboo composite material;

[0107] S6. Preparation of flame-retardant bamboo composite material: The surface of the bamboo composite material obtained in step S5 is coated with a layer of tung oil, the coating amount is 0.05g / cm 2 , and dried to obtain a flame retardant bamboo-wood composite material.

[0108] Comparative Example 6

[0109] Compared with Example 3, the difference is that no modified nanospheres are added in step S5.

[0110] The details are as follows:

[0111] S5. Preparation of acrylic resin emulsion: 6 parts by weight of methyl methacrylate, 4 parts by weight of acrylic acid, 45 parts by weight of butyl acrylate, and 30 parts by weight of styrene were mixed and added to 300 parts by weight of water, and the mixture was stirred for 20 minutes. Ammonium persulfate was added in an amount of 0.7 wt% of the total mass of the system. The mixture was heated to 50°C and stirred for 4 hours. The pH value of the solution was adjusted to 8.5. 0.7 parts by weight of dispersant BYK-190, 0.15 parts by weight of defoamer BYK-024, and 0.65 parts by weight of leveling agent DAPROW-77 were added. The mixture was stirred for 2 hours to obtain acrylic resin emulsion.

[0112] Comparative Example 7

[0113] Compared with the embodiment 3, the difference is that step S7 is not performed.

[0114] The details are as follows:

[0115] S1. Preparation of MgO-deposited SiO2 / TiO2 nanospheres: 4 parts by weight of magnesium nitrate, 160 parts by weight of ethanol, 3 parts by weight of aqueous ammonia and 17 parts by weight of water were stirred and mixed for 20 minutes, 11 parts by weight of ethyl orthosilicate and 8.5 parts by weight of tetrabutyl titanate were added, and the reaction was hydrolyzed at 32°C for 6 hours, centrifuged, washed, dried, and calcined at 600°C for 3 hours to obtain MgO-deposited SiO2 / TiO2 nanospheres;

[0116] S2. Modification of the first silane coupling agent: 100 parts by weight of the MgO-deposited SiO2 / TiO2 nanospheres prepared in step S1 were added to 500 parts by weight of a 75wt% ethanol solution, 20 parts by weight of the first silane coupling agent were added, heated to 45°C, stirred for 3h, centrifuged, washed, and dried to obtain modified MgO-deposited SiO2 / TiO2 nanospheres;

[0117] The first silane coupling agent is a mixture of KH602 and KH792, with a mass ratio of 6:2;

[0118] S3 flame retardant modification: 100 parts by weight of the modified MgO deposited SiO2 / TiO2 nanospheres obtained in step S2, 27 parts by weight of benzaldehyde, 2 parts by weight of sodium acetate were added to 500 parts by weight of ethanol, and the reaction was heated under reflux for 4 hours under nitrogen protection, and then 35 parts by weight of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide was added, and the reaction was continued for 11 hours, centrifuged, washed, and dried to obtain flame retardant nanospheres;

[0119] S4. Modification of the second silane coupling agent: 100 parts by weight of the flame-retardant nanospheres obtained in step S3 were added to 300 parts by weight of a 70wt% ethanol solution, 6 parts by weight of a silane coupling agent KH570 were added, heated to 45 ° C, stirred for 2h, centrifuged, washed, and dried to obtain modified nanospheres;

[0120] S5. Preparation of flame retardant acrylic resin emulsion: 17 parts by weight of the modified nanospheres prepared in step S4, 6 parts by weight of methyl methacrylate, 4 parts by weight of acrylic acid, 45 parts by weight of butyl acrylate, and 30 parts by weight of styrene were mixed and added to 300 parts by weight of water, stirred and mixed for 20 minutes, and ammonium persulfate was added, wherein the amount of ammonium persulfate added was 0.7wt% of the total mass of the system, heated to 50°C, stirred and reacted for 4 hours, the pH value of the solution was adjusted to 8.5, 0.7 parts by weight of dispersant BYK-190, 0.15 parts by weight of defoamer BYK-024, and 0.65 parts by weight of leveling agent DAPRO W-77 were added, and stirring was continued for 2 hours to obtain a flame retardant acrylic resin emulsion;

[0121] S6. Molding: 17 parts by weight of bamboo powder and 11 parts by weight of wood powder were stirred and mixed for 15 minutes, 20 parts by weight of the flame retardant acrylic resin emulsion prepared in step S5 were added, the temperature was 145 ° C, the pressure was 6.4 MPa, hot pressing for 15 minutes, and dried to obtain a bamboo-wood composite material, that is, a flame retardant bamboo-wood composite material.

[0122] Test Example 1

[0123] The antibacterial and anti-mildew properties of the flame-retardant bamboo-wood composite materials prepared in Examples 1-5 and Comparative Examples 1-7 were tested according to JC / T 2039-2010. The results are shown in Table 1.

[0124] Table 1

[0125]

[0126] It can be seen from the above table that the flame retardant bamboo-wood composite materials prepared in Examples 1-3 of the present invention have good antibacterial and anti-mildew properties.

[0127] Test Example 2

[0128] The flame retardant bamboo-wood composite materials prepared in Examples 1-5 and Comparative Examples 1-7 were tested for mechanical properties according to GB / T 4897-2015.

[0129] An evaluation team of 20 professionals evaluated the odor of the flame retardant bamboo-wood composite material. Odor evaluation level: Level 1: no odor; Level 2: slight odor; Level 3: odor, but not irritating; Level 4: irritating odor, or irritating odor, but strong; Level 5: strong irritating odor; Level 6: unbearable odor.

[0130] The results are shown in Table 2.

[0131] Table 2

[0132]

[0133] It can be seen from the above table that the flame retardant bamboo-wood composite materials prepared in Examples 1-3 of the present invention have good mechanical properties and less odor.

[0134] Test Example 3

[0135] The flame retardant properties of the flame retardant bamboo-wood composite materials prepared in Examples 1-5 and Comparative Examples 1-7 were tested. The results are shown in Table 3. The vertical burning test (UL94) was carried out in accordance with GB / T 2408-2021, and the sample size was 130×13×3 mm 3 . Determination method of limiting oxygen index (LOI): refer to GB / T 2406.2-2009, the specimen size is 150mm×5mm×5mm.

[0136] Table 3

[0137]

[0138] It can be seen from the above table that the flame retardant bamboo-wood composite materials prepared in Examples 1-3 of the present invention have good flame retardant properties.

[0139] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a flame retardant bamboo-wood composite material, characterized in that: The following steps are involved: S1. Preparation of MgO-deposited SiO2 / TiO2 nanospheres: The magnesium salt, ethanol, ammonia and water were mixed uniformly, tetraethyl orthosilicate and tetrabutyl titanate were added, the reaction was hydrolyzed, centrifuged, washed, dried, and calcined to obtain MgO-deposited SiO2 / TiO2 nanospheres; S2 first silane coupling agent modification: The MgO deposited SiO2 / TiO2 nanospheres prepared in step S1 were added to an ethanol solution, a first silane coupling agent was added, the reaction was heated and stirred, centrifuged, washed, and dried to obtain modified MgO deposited SiO2 / TiO2 nanospheres; S3 flame retardant modification: the modified MgO deposited SiO2 / TiO2 nanospheres obtained in step S2, benzaldehyde, sodium acetate were added to ethanol, heated under inert gas protection, reflux reaction, and then 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide was added, the reaction was continued, centrifuged, washed, and dried to obtain flame retardant nanospheres; S4 second silane coupling agent modification: The flame retardant nanospheres obtained in step S3 were added to an ethanol solution, a second silane coupling agent was added, the reaction was heated and stirred, centrifuged, washed, and dried to obtain modified nanospheres; S5 flame retardant acrylic resin emulsion preparation: the modified nanospheres prepared in step S4, methyl methacrylate, acrylic acid, butyl acrylate, styrene was added to water, stirred to mix, an initiator was added, the reaction was heated with stirring, the pH value of the solution was adjusted, a dispersant, a defoamer, a leveling agent was added, and stirring was continued to obtain a flame retardant acrylic resin emulsion; S6 molding: The bamboo powder, wood powder mixed evenly, adding the flame retardant acrylic resin emulsion prepared in step S5, hot pressing, drying, to obtain a bamboo composite material; S7. Preparation of flame-retardant bamboo-wood composite material: The surface of the bamboo-wood composite material obtained in step S6 is coated with a layer of tung oil and dried to obtain a flame-retardant bamboo-wood composite material.

2. The preparation method according to claim 1, characterized in that: The mass ratio of the magnesium salt, ethanol, ammonia water, water, tetraethyl orthosilicate and tetrabutyl titanate in step S1 is (3-5): (150-170): (2-4): (15-20): (10-12): (7-10), the magnesium salt is selected from at least one of magnesium chloride, magnesium sulfate and magnesium nitrate, the temperature of the hydrolysis reaction is 30-35°C, the time is 5-7h, and the temperature of the calcination is 500-700°C, and the time is 2-4h.

3. The preparation method according to claim 1, characterized in that: In step S2, the mass ratio of the MgO deposited SiO2 / TiO2 nanospheres and the first silane coupling agent is 100:(17-22), the first silane coupling agent is selected from at least one of KH550, KH602, and KH792, the temperature of the heating and stirring reaction is 40-50°C, and the time is 2-4h.

4. The preparation method according to claim 1, characterized in that: In step S3, the mass ratio of the modified MgO deposited SiO2 / TiO2 nanospheres, benzaldehyde, sodium acetate, and 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide is 100:(25-30):(1-3):(32-37), the heating reflux reaction time is 3-5 hours, and the continued reaction time is 10-12 hours.

5. The preparation method according to claim 1, characterized in that: In step S4, the mass ratio of the flame retardant nanospheres to the second silane coupling agent is 100:(5-7), the second silane coupling agent is selected from at least one of KH570, A151, and A171, and the temperature of the heating and stirring reaction is 40-50° C. and the time is 1-3 hours.

6. The preparation method according to claim 1, characterized in that The mass ratio of the modified nanospheres, methyl methacrylate, acrylic acid, butyl acrylate, styrene, dispersant, defoamer and leveling agent in step S5 is (15-20): (5-7): (3-5): (40-50): (20-40): (0.5-1): (0.1-0.2): (0.5-0.8), the initiator is selected from at least one of potassium persulfate, sodium persulfate and ammonium persulfate, the dispersant is BYK-190, the defoamer is BYK-024, the leveling agent is DAPRO W-77, the amount of the initiator added is 0.5-1wt% of the total mass of the system, the temperature of the heating and stirring reaction is 45-55°C, the time is 3-5h, the pH value of the solution is adjusted to 8-9, and the stirring time is 1-3h.

7. The preparation method according to claim 1, characterized in that: The mass ratio of bamboo powder, wood powder and flame retardant acrylic resin emulsion in step S6 is (15-20): (10-12): (17-22), the temperature of hot pressing is 140-150°C, the pressure is 5.5-7Mpa, and the time is 10-20min; the coating amount of tung oil in step S7 is 0.03-0.05g / cm 2 .

8. The preparation method according to claim 1, characterized in that: Specifically include the following steps: S1. Preparation of MgO-deposited SiO2 / TiO2 nanospheres: 3-5 parts by weight of magnesium salt, 150-170 parts by weight of ethanol, 2-4 parts by weight of ammonia and 15-20 parts by weight of water were mixed uniformly, 10-12 parts by weight of ethyl orthosilicate and 7-10 parts by weight of tetrabutyl titanate were added, and the reaction was hydrolyzed at 30-35°C for 5-7h, centrifuged, washed, dried, and calcined at 500-700°C for 2-4h to obtain MgO-deposited SiO2 / TiO2 nanospheres; S2. Modification of the first silane coupling agent: adding 100 parts by weight of the MgO-deposited SiO2 / TiO2 nanospheres obtained in step S1 to 500 parts by weight of a 70-80wt% ethanol solution, adding 17-22 parts by weight of the first silane coupling agent, heating to 40-50°C, stirring the reaction for 2-4h, centrifuging, washing, and drying to obtain modified MgO-deposited SiO2 / TiO2 nanospheres; The first silane coupling agent is a mixture of KH602 and KH792, with a mass ratio of 5-7:1-3; S3 flame retardant modification: 100 parts by weight of the modified MgO deposited SiO2 / TiO2 nanospheres obtained in step S2, 25-30 parts by weight of benzaldehyde, 1-3 parts by weight of sodium acetate were added to ethanol, and the reaction was heated under reflux under inert gas for 3-5h, and then 32-37 parts by weight of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide was added, and the reaction was continued for 10-12h, centrifuged, washed, and dried to obtain flame retardant nanospheres; S4. Modification of the second silane coupling agent: 100 parts by weight of the flame-retardant nanospheres obtained in step S3 were added to an ethanol solution, 5-7 parts by weight of a second silane coupling agent were added, heated to 40-50 ° C, stirred for 1-3h, centrifuged, washed, and dried to obtain modified nanospheres; S5. Preparation of flame retardant acrylic resin emulsion: 15-20 parts by weight of the modified nanospheres prepared in step S4, 5-7 parts by weight of methyl methacrylate, 3-5 parts by weight of acrylic acid, 40-50 parts by weight of butyl acrylate, 20-40 parts by weight of styrene are mixed and added to 300 parts by weight of water, stirred and mixed evenly, an initiator is added, the initiator is added in an amount of 0.5-1wt% of the total mass of the system, heated to 45-55 ° C, stirred for 3-5h, the pH value of the solution is adjusted to 8-9, 0.5-1 parts by weight of dispersant BYK-190, 0.1-0.2 parts by weight of defoamer BYK-024, 0.5-0.8 parts by weight of leveling agent DAPRO W-77 are added, stirring is continued for 1-3h to obtain a flame retardant acrylic resin emulsion; S6 molding: 15-20 parts by weight of bamboo powder, 10-12 parts by weight of wood powder mixed, added 17-22 parts by weight of the flame retardant acrylic resin emulsion prepared in step S5, a temperature of 140-150 ℃, a pressure of 5.5-7Mpa, hot pressing 10-20min, dried to obtain a bamboo composite material; S7. Preparation of flame-retardant bamboo composite material: The surface of the bamboo composite material obtained in step S6 is coated with a layer of tung oil, the coating amount is 0.03-0.05g / cm 2 , and dried to obtain a flame retardant bamboo-wood composite material.

9. A flame retardant bamboo-wood composite material obtained by the method for preparing a flame retardant bamboo-wood composite material according to any one of claims 1 to 8.