Adhesive composition for copper clad laminate and preparation method thereof
By using raw materials such as epoxy resin, silane coupling agent and other raw materials in the copper clad rubber composition, combined with the linking stabilizer and the modification reinforcement agent, the dielectric loss, mechanical properties and peeling properties in the prior art are solved. The dielectric loss, mechanical properties and peeling properties are difficult to coordinate in the prior art. The problem is that the thermal stability and acid-base resistance stability are significantly improved, and the overall performance of the product is improved.
Patent Information
- Application Number
- CN202411148252.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-08-21
AI Technical Summary
The dielectric loss, mechanical properties and peeling properties of existing copper clad rubber compositions are difficult to coordinately improve, and the thermal stability and acid-base resistance stability are poor, which limits the efficiency of the product.
Using raw materials such as epoxy resin, silane coupling agent, curing agent, accelerator, etc., the dispersion and activity of boron nitride are optimized by combining the joint stabilizer and the modification reinforcement agent, and combined with hydroxyapa. Materials such as stone, nano-silicon sol, enhance the dielectric loss, mechanical properties and peeling properties of the product, and improve thermal stability and acid-base resistance through specific preparation methods.
The coordinated improvement of dielectric loss, mechanical properties and peeling properties is achieved, while the thermal stability and acid-base resistance of the product are significantly improved, and the overall performance of the product is improved.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of copper clad laminate adhesives, and in particular to an adhesive composition for copper clad laminates and a preparation method thereof. Background Art
[0002] With the advancement of science and technology, the development of high-frequency communication has led to the development of wireless communication towards high frequency, with the frequency shifting from the MHz band to the GHz band, and information transmission entering the high-frequency field. The high-frequency and high-speed electronic information products have also placed higher requirements on the high-frequency characteristics of copper clad laminates.
[0003] The existing adhesive composition for copper clad laminates has poor dielectric loss performance, and it is difficult to coordinate and improve the dielectric loss, mechanical properties and peeling performance. At the same time, the product has poor thermal stability and acid and alkali stability, which further limits the use efficiency of the product. Based on this, the present invention further improves it. Summary of the invention
[0004] In view of the defects of the prior art, the purpose of the present invention is to provide an adhesive composition for copper clad laminates and a preparation method thereof, so as to solve the problems raised in the above background technology.
[0005] The present invention solves the technical problem by adopting the following technical solution:
[0006] The present invention provides an adhesive composition for a copper-clad laminate, comprising the following raw materials in parts by weight:
[0007] 35-40 parts of epoxy resin, 8-12 parts of bonding stabilizer, 5-7 parts of silane coupling agent, 4-6 parts of modifying reinforcing agent, 3-6 parts of curing agent, 1-3 parts of accelerator, and 30-35 parts of solvent.
[0008] Preferably, the adhesive composition for copper clad laminate comprises the following raw materials in parts by weight:
[0009] 37.5 parts of epoxy resin, 10 parts of bonding stabilizer, 6 parts of silane coupling agent, 5 parts of modifying reinforcing agent, 4.5 parts of curing agent, 2 parts of accelerator, and 32.5 parts of solvent.
[0010] Preferably, the epoxy resin is a bisphenol A epoxy resin, with an epoxy equivalent of 185 to 190 g / eq and a viscosity of 12000 to 15000 cps at 25°C;
[0011] The solvent is dimethylformamide; the accelerator is 2-methylimidazole; the curing agent is triethylenetetramine; and the silane coupling agent is silane coupling agent KH560.
[0012] Preferably, the preparation method of the bonding stabilizer is:
[0013] S01: irradiating the boron nitride flakes in a proton irradiation box, and obtaining an irradiated boron nitride agent after the irradiation is completed;
[0014] S02: Preparation of infusion agent:
[0015] Add 2 to 5 parts of 5% chitosan solution and 1 to 3 parts of phosphate buffer solution to 4 to 7 parts of 6% sodium dodecylbenzene sulfonate solution, then add 0.35 to 0.45 parts of silane coupling agent KH550, continue to mix thoroughly, and obtain an infusion agent;
[0016] S03: immersing the irradiated boron nitride agent into a soaking agent that is 3 to 5 times the total amount of the irradiated boron nitride agent for soaking and improvement treatment, and after the soaking and adjustment, filtering and drying are completed to obtain a soaked boron nitride body;
[0017] S04: The impregnated boron nitride body and the stabilizing modifier are mixed in a weight ratio of 5:3 and ball-milled at a ball-milling speed of 1000-1500 r / min for 2 hours. After the ball-milling is completed, the mixture is washed with water and dried to obtain the stabilizing modifier.
[0018] Preferably, the irradiation power of the irradiation treatment is 350-400W, and the irradiation time is 10-15 minutes; the pH value of the phosphate buffer solution is 5.0-6.0.
[0019] Preferably, the soaking power of the improved soaking treatment is 400-450W, and the soaking time is 5-10 minutes.
[0020] Preferably, the preparation method of the stabilizing modifier is:
[0021] 5 to 8 parts of hydroxyapatite, 1 to 3 parts of nano-silica sol, 3 to 5 parts of 5% by mass sodium lignin sulfonate solution, 0.25 to 0.35 parts of yttrium oxide and 1 to 2 parts of 8% by mass sodium alginate solution are fully mixed to obtain a stabilizing modifier.
[0022] Preferably, the preparation method of the modified reinforcing agent is:
[0023] S11: adding 1 to 3 parts of tetrabutyl titanate to 5 to 7 parts of ethanol solvent, and then adding 2 to 5 parts of sodium citrate solution and 2 to 4 parts of nano-silicon dioxide, stirring and mixing to obtain nano-silicon dioxide liquid;
[0024] S12: feeding the glass fiber into a lanthanum nitrate solution which is 3 to 5 times the total amount of the glass fiber and mixing well to obtain a glass fiber liquid;
[0025] The glass fiber liquid and the nano-silica liquid are mixed and ball-milled in a weight ratio of 5:3, the mixing ball mill speed is 1000-1500r / min, the mixing is carried out for 1h, and after the mixing is completed, the mixture is washed with water and dried to obtain a modified reinforcing agent.
[0026] Preferably, the mass fraction of the sodium citrate solution is 5-8%; the mass fraction of the lanthanum nitrate solution is 2-5%.
[0027] The present invention also provides a method for preparing an adhesive composition for copper-clad laminates, comprising the following steps: mixing raw materials according to a proportion and uniformly treating them to obtain the adhesive composition of the present invention.
[0028] Compared with the prior art, the present invention has the following beneficial effects:
[0029] The adhesive composition of the present invention adopts epoxy resin to match silane coupling agent, curing agent and accelerator raw materials, and the dielectric loss, mechanical property and peeling property of the product are coordinated and improved by adding a connection stabilizer and a modified reinforcing agent, and the thermal stability and acid-base stability performance of the product are significantly improved; the connection stabilizer adopts flaky boron nitride to be irradiated in a proton irradiation box in advance to optimize its activity efficiency, and then the chitosan solution, phosphate buffer solution, sodium dodecylbenzene sulfonate solution and silane coupling agent KH550 are mixed and blended to obtain an impregnation agent, and the raw materials in the impregnation agent are coordinated and matched with each other to optimize the dispersibility and activity of boron nitride, thereby enhancing the coordination effect of the impregnated boron nitride body and the connection stabilizer modifier, improving the performance effect of the product, and the connection stabilizer The modifier is fully prepared by blending hydroxyapatite, nano-silica sol, sodium lignin sulfonate solution, yttrium oxide and sodium alginate solution. Hydroxyapatite is used as a matrix, nano-silica sol and other raw materials are matched to improve the leached boron nitride body, so as to enhance the dielectric loss, mechanical properties and peeling properties of the product system to achieve coordinated improvement, and the thermal stability and acid and alkali resistance stability of the product are significantly improved; the modified reinforcing agent adopts nano-silica liquid and glass fiber liquid for coordinated improvement, with nano-silica and glass fiber as the matrix, and needle-shaped glass fiber is matched with nano-silica with a high specific surface area to fill the synergy, so as to enhance the performance effect of the product. At the same time, through the further improvement of the preparation method of the modified reinforcing agent of the present invention, the product performance is further improved. DETAILED DESCRIPTION
[0030] The following is a clear and complete description of the technical solutions in the embodiments of the present invention in conjunction with specific embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0031] The adhesive composition for a copper-clad laminate of this embodiment includes the following raw materials in parts by weight:
[0032] 35-40 parts of epoxy resin, 8-12 parts of bonding stabilizer, 5-7 parts of silane coupling agent, 4-6 parts of modifying reinforcing agent, 3-6 parts of curing agent, 1-3 parts of accelerator, and 30-35 parts of solvent.
[0033] The adhesive composition for the copper clad laminate of this embodiment includes the following raw materials in parts by weight:
[0034] 37.5 parts of epoxy resin, 10 parts of bonding stabilizer, 6 parts of silane coupling agent, 5 parts of modifying reinforcing agent, 4.5 parts of curing agent, 2 parts of accelerator, and 32.5 parts of solvent.
[0035] The epoxy resin of this embodiment is a bisphenol A epoxy resin, with an epoxy equivalent of 185 to 190 g / eq and a viscosity of 12000 to 15000 cps at 25°C;
[0036] The solvent is dimethylformamide; the accelerator is 2-methylimidazole; the curing agent is triethylenetetramine; and the silane coupling agent is silane coupling agent KH560.
[0037] The preparation method of the bonding stabilizer of this embodiment is:
[0038] S01: irradiating the boron nitride flakes in a proton irradiation box, and obtaining an irradiated boron nitride agent after the irradiation is completed;
[0039] S02: Preparation of infusion agent:
[0040] Add 2 to 5 parts of 5% chitosan solution and 1 to 3 parts of phosphate buffer solution to 4 to 7 parts of 6% sodium dodecylbenzene sulfonate solution, then add 0.35 to 0.45 parts of silane coupling agent KH550, continue to mix thoroughly, and obtain an infusion agent;
[0041] S03: immersing the irradiated boron nitride agent into a soaking agent that is 3 to 5 times the total amount of the irradiated boron nitride agent for soaking and improvement treatment, and after the soaking and adjustment is completed, filtering and drying are performed to obtain a soaked boron nitride body;
[0042] S04: The impregnated boron nitride body and the stabilizing modifier are mixed in a weight ratio of 5:3 and ball-milled at a ball-milling speed of 1000-1500 r / min for 2 hours. After the ball-milling is completed, the mixture is washed with water and dried to obtain the stabilizing modifier.
[0043] The irradiation power of the irradiation treatment in this embodiment is 350-400W, and the irradiation time is 10-15 minutes; the pH value of the phosphate buffer solution is 5.0-6.0.
[0044] The improved soaking and conditioning treatment of this embodiment has a soaking and conditioning power of 400-450W and a soaking and conditioning time of 5-10 minutes.
[0045] The preparation method of the stabilizing modifier of this embodiment is:
[0046] 5 to 8 parts of hydroxyapatite, 1 to 3 parts of nano-silica sol, 3 to 5 parts of 5% by mass sodium lignin sulfonate solution, 0.25 to 0.35 parts of yttrium oxide and 1 to 2 parts of 8% by mass sodium alginate solution are fully mixed to obtain a stabilizing modifier.
[0047] The preparation method of the modified reinforcing agent of this embodiment is:
[0048] S11: adding 1 to 3 parts of tetrabutyl titanate to 5 to 7 parts of ethanol solvent, and then adding 2 to 5 parts of sodium citrate solution and 2 to 4 parts of nano-silicon dioxide, stirring and mixing to obtain nano-silicon dioxide liquid;
[0049] S12: feeding the glass fiber into a lanthanum nitrate solution which is 3 to 5 times the total amount of the glass fiber and mixing well to obtain a glass fiber liquid;
[0050] The glass fiber liquid and the nano-silica liquid are mixed and ball-milled in a weight ratio of 5:3, the mixing ball mill speed is 1000-1500r / min, the mixing is carried out for 1h, and after the mixing is completed, the mixture is washed with water and dried to obtain a modified reinforcing agent.
[0051] The mass fraction of the sodium citrate solution in this embodiment is 5-8%; the mass fraction of the lanthanum nitrate solution is 2-5%.
[0052] The method for preparing an adhesive composition for a copper-clad laminate of the present embodiment comprises the following steps: the raw materials are mixed uniformly according to a proportion to obtain the adhesive composition of the present invention.
[0053] Example 1.
[0054] The adhesive composition for a copper-clad laminate of this embodiment includes the following raw materials in parts by weight:
[0055] 35 parts of epoxy resin, 8 parts of bonding stabilizer, 5 parts of silane coupling agent, 4 parts of modifying reinforcing agent, 3 parts of curing agent, 1 part of accelerator, and 30 parts of solvent.
[0056] The epoxy resin in this embodiment is a bisphenol A epoxy resin with an epoxy equivalent of 1850 g / eq and a viscosity of 12000 cps at 25°C;
[0057] The solvent is dimethylformamide; the accelerator is 2-methylimidazole; the curing agent is triethylenetetramine; and the silane coupling agent is silane coupling agent KH560.
[0058] The preparation method of the bonding stabilizer of this embodiment is:
[0059] S01: irradiating the boron nitride flakes in a proton irradiation box, and obtaining an irradiated boron nitride agent after the irradiation is completed;
[0060] S02: Preparation of infusion agent:
[0061] Add 2 parts of 5% chitosan solution and 1 part of phosphate buffer solution to 4 parts of 6% sodium dodecylbenzene sulfonate solution, then add 0.35 parts of silane coupling agent KH550, continue to mix thoroughly, and obtain an infusion agent;
[0062] S03: immersing the irradiated boron nitride agent into a soaking agent that is 3 times the total amount of the irradiated boron nitride agent for soaking and improvement treatment, and after the soaking and adjustment is completed, filtering and drying are performed to obtain a soaked boron nitride body;
[0063] S04: The impregnated boron nitride body and the stabilizing modifier are mixed in a weight ratio of 5:3 and ball-milled at a ball-milling speed of 1000 r / min for 2 h. After the ball-milling is completed, the mixture is washed with water and dried to obtain the stabilizing modifier.
[0064] The irradiation power of the irradiation treatment in this embodiment is 350W, and the irradiation time is 10 minutes; the pH value of the phosphate buffer solution is 5.0.
[0065] The immersion adjustment power of the improved immersion adjustment process in this embodiment is 400W, and the immersion adjustment time is 5 minutes.
[0066] The preparation method of the stabilizing modifier of this embodiment is:
[0067] 5 parts of hydroxyapatite, 1 part of nano-silica sol, 3 parts of 5% by mass sodium lignin sulfonate solution, 0.25 parts of yttrium oxide and 1 part of 8% by mass sodium alginate solution are fully blended to obtain a stabilizing modifier.
[0068] The preparation method of the modified reinforcing agent of this embodiment is:
[0069] S11: adding 1 part of tetrabutyl titanate to 5 parts of ethanol solvent, and then adding 2 parts of sodium citrate solution and 2 parts of nano-silicon dioxide, stirring and mixing to obtain nano-silicon dioxide liquid;
[0070] S12: feeding the glass fiber into a lanthanum nitrate solution having an amount three times the total amount of the glass fiber and mixing well to obtain a glass fiber liquid;
[0071] The glass fiber liquid and the nano-silica liquid were mixed and ball-milled in a weight ratio of 5:3, the mixing ball mill speed was 1000r / min, the mixing was performed for 1h, and after the mixing was completed, the mixture was washed with water and dried to obtain a modified reinforcing agent.
[0072] The mass fraction of the sodium citrate solution in this embodiment is 5%; the mass fraction of the lanthanum nitrate solution is 2%.
[0073] The method for preparing an adhesive composition for a copper-clad laminate of the present embodiment comprises the following steps: the raw materials are mixed uniformly according to a proportion to obtain the adhesive composition of the present invention.
[0074] Example 2.
[0075] The adhesive composition for a copper-clad laminate of this embodiment includes the following raw materials in parts by weight:
[0076] 40 parts of epoxy resin, 12 parts of bonding stabilizer, 7 parts of silane coupling agent, 6 parts of modifying reinforcing agent, 6 parts of curing agent, 3 parts of accelerator, and 35 parts of solvent.
[0077] The epoxy resin in this embodiment is a bisphenol A epoxy resin with an epoxy equivalent of 190 g / eq and a viscosity of 15000 cps at 25°C;
[0078] The solvent is dimethylformamide; the accelerator is 2-methylimidazole; the curing agent is triethylenetetramine; and the silane coupling agent is silane coupling agent KH560.
[0079] The preparation method of the bonding stabilizer of this embodiment is:
[0080] S01: irradiating the boron nitride flakes in a proton irradiation box, and obtaining an irradiated boron nitride agent after the irradiation is completed;
[0081] S02: Preparation of infusion agent:
[0082] Add 5 parts of 5% chitosan solution and 3 parts of phosphate buffer solution to 7 parts of 6% sodium dodecylbenzene sulfonate solution, then add 0.45 parts of silane coupling agent KH550, continue to mix thoroughly, and obtain an infusion agent;
[0083] S03: immersing the irradiated boron nitride agent into a soaking agent that is 5 times the total amount of the irradiated boron nitride agent for soaking and improvement treatment, and after the soaking and adjustment is completed, filtering and drying are performed to obtain a soaked boron nitride body;
[0084] S04: The impregnated boron nitride body and the stabilizing modifier are mixed in a weight ratio of 5:3 and ball-milled at a ball-milling speed of 1500 r / min for 2 h. After the ball-milling is completed, the mixture is washed with water and dried to obtain the stabilizing modifier.
[0085] The irradiation power of the irradiation treatment in this embodiment is 400 W, and the irradiation time is 15 min; the pH value of the phosphate buffer solution is 6.0.
[0086] The immersion adjustment power of the improved immersion adjustment process in this embodiment is 450W, and the immersion adjustment time is 10 minutes.
[0087] The preparation method of the stabilizing modifier of this embodiment is:
[0088] 8 parts of hydroxyapatite, 3 parts of nano-silica sol, 5 parts of 5% by mass sodium lignin sulfonate solution, 0.35 parts of yttrium oxide and 2 parts of 8% by mass sodium alginate solution were fully mixed to obtain a stabilizing modifier.
[0089] The preparation method of the modified reinforcing agent of this embodiment is:
[0090] S11: 3 parts of tetrabutyl titanate are added to 7 parts of ethanol solvent, and then 5 parts of sodium citrate solution and 4 parts of nano-silicon dioxide are added, and the mixture is stirred to obtain nano-silicon dioxide liquid;
[0091] S12: feeding the glass fiber into a lanthanum nitrate solution having an amount 5 times the total amount of the glass fiber and mixing well to obtain a glass fiber liquid;
[0092] The glass fiber liquid and the nano-silica liquid were mixed and ball-milled in a weight ratio of 5:3, the mixing ball mill speed was 1500r / min, the mixing was performed for 1h, and after the mixing was completed, the mixture was washed with water and dried to obtain a modified reinforcing agent.
[0093] The mass fraction of the sodium citrate solution in this embodiment is 8%; the mass fraction of the lanthanum nitrate solution is 5%.
[0094] The method for preparing an adhesive composition for a copper-clad laminate of the present embodiment comprises the following steps: the raw materials are mixed uniformly according to a proportion to obtain the adhesive composition of the present invention.
[0095] Example 3.
[0096] The adhesive composition for a copper-clad laminate of this embodiment includes the following raw materials in parts by weight:
[0097] 37.5 parts of epoxy resin, 10 parts of bonding stabilizer, 6 parts of silane coupling agent, 5 parts of modifying reinforcing agent, 4.5 parts of curing agent, 2 parts of accelerator, and 32.5 parts of solvent.
[0098] The epoxy resin in this embodiment is a bisphenol A epoxy resin, with an epoxy equivalent of 188 g / eq and a viscosity of 13500 cps at 25°C;
[0099] The solvent is dimethylformamide; the accelerator is 2-methylimidazole; the curing agent is triethylenetetramine; and the silane coupling agent is silane coupling agent KH560.
[0100] The preparation method of the bonding stabilizer of this embodiment is:
[0101] S01: irradiating the boron nitride flakes in a proton irradiation box, and obtaining an irradiated boron nitride agent after the irradiation is completed;
[0102] S02: Preparation of infusion agent:
[0103] 3.5 parts of 5% chitosan solution and 2 parts of phosphate buffer solution were added to 5.5 parts of 6% sodium dodecylbenzene sulfonate solution, and then 0.40 parts of silane coupling agent KH550 were added, and the mixture was mixed thoroughly to obtain an infusion agent;
[0104] S03: immersing the irradiated boron nitride agent into a soaking agent that is 4 times the total amount of the irradiated boron nitride agent for soaking and improvement treatment, and after the soaking and adjustment is completed, filtering and drying are performed to obtain a soaked boron nitride body;
[0105] S04: The impregnated boron nitride body and the stabilizing modifier are mixed in a weight ratio of 5:3 and ball-milled at a speed of 1250 r / min for 2 h. After the ball milling is completed, the mixture is washed with water and dried to obtain the stabilizing agent.
[0106] The irradiation power of the irradiation treatment in this embodiment is 370W, and the irradiation time is 12.5 minutes; the pH value of the phosphate buffer solution is 5.5.
[0107] The immersion adjustment power of the improved immersion adjustment process in this embodiment is 425W, and the immersion adjustment time is 7.5min.
[0108] The preparation method of the stabilizing modifier of this embodiment is:
[0109] 6.5 parts of hydroxyapatite, 2 parts of nano-silica sol, 4 parts of 5% by mass sodium lignin sulfonate solution, 0.30 parts of yttrium oxide and 1.5 parts of 8% by mass sodium alginate solution were fully mixed to obtain a stabilizing modifier.
[0110] The preparation method of the modified reinforcing agent of this embodiment is:
[0111] S11: adding 2 parts of tetrabutyl titanate to 6 parts of ethanol solvent, and then adding 3.5 parts of sodium citrate solution and 3 parts of nano-silicon dioxide, stirring and mixing to obtain nano-silicon dioxide liquid;
[0112] S12: feeding the glass fiber into a lanthanum nitrate solution having an amount four times the total amount of the glass fiber and mixing well to obtain a glass fiber liquid;
[0113] The glass fiber liquid and the nano-silica liquid were mixed and ball-milled in a weight ratio of 5:3, the mixing ball mill speed was 1250r / min, the mixing was performed for 1h, and after the mixing was completed, the mixture was washed with water and dried to obtain a modified reinforcing agent.
[0114] The mass fraction of the sodium citrate solution in this embodiment is 6.5%; the mass fraction of the lanthanum nitrate solution is 3.5%.
[0115] The method for preparing an adhesive composition for a copper-clad laminate of the present embodiment comprises the following steps: the raw materials are mixed uniformly according to a proportion to obtain the adhesive composition of the present invention.
[0116] Comparative Example 1.
[0117] The difference from Example 3 is that no bonding stabilizer is added.
[0118] Comparative Example 2.
[0119] The difference from Example 3 is that no soaking agent treatment is used in the preparation of the bonding stabilizer.
[0120] Comparative Example 3.
[0121] The difference from Example 3 is that the preparation method of the infusion agent is different. 2 parts of phosphate buffer solution are added to 5.5 parts of 6% by mass sodium dodecylbenzene sulfonate solution and mixed thoroughly to obtain the infusion agent.
[0122] Comparative Example 4.
[0123] The difference from Example 3 is that no stabilizing modifier is used in the preparation of the stabilizing agent.
[0124] Comparative Example 5.
[0125] The difference from Example 3 is that no modifying reinforcing agent is added.
[0126] Comparative Example 6.
[0127] The difference from Example 3 is that no glass fiber liquid is added in the preparation of the modified reinforcing agent.
[0128] Comparative Example 7.
[0129] The difference from Example 3 is that the glass fiber liquid is replaced by glass fiber.
[0130] Comparative Example 8.
[0131] The difference from Example 3 is that no nano-silicon dioxide liquid is added in the preparation of the modified reinforcing agent.
[0132] Comparative Example 9.
[0133] The difference from Example 3 is that the nano-silicon dioxide liquid is replaced by nano-silicon dioxide.
[0134] The products of Examples 1-3 and Comparative Examples 1-9 were soaked with ordinary glass fiber cloth and baked in an oven at 200°C for 5 minutes to obtain PP sheets with a glue content of 55%. Then, two PP sheets were stacked according to the requirements, and the upper and lower surfaces were covered with 18um copper foil. The copper clad laminate was obtained by hot pressing for 1.5 hours in a vacuum press at a pressure of 5MPa and a temperature of 150°C. The performance of the products was tested under normal conditions, and the products were placed at 65°C for 12 hours, and then placed under 2% hydrochloric acid mist conditions for 12 hours to test the heat resistance and acid resistance stability, and the products were placed at 65°C for 12 hours, and then placed under 2% sodium hydroxide alkaline mist conditions for 12 hours to test the heat resistance and acid resistance stability. The performance measurement results are as follows
[0135]
[0136] From Examples 1-3 and Comparative Examples 1-9, it can be concluded that
[0137] The product of Example 3 of the present invention has excellent dielectric loss, peel strength and tensile performance under normal conditions, and the three properties can be coordinated and improved. At the same time, the product has significant performance stability under heat resistance, acid resistance, heat resistance and alkali resistance conditions;
[0138] The invention adds a stabilizer but does not add a modifying and reinforcing agent, and the performance of the product has a significant tendency to deteriorate. The two are used in combination to synergistically enhance the performance, and the product performance effect is most significant.
[0139] No soaking agent treatment was used in the preparation of the bonding stabilizer, and the soaking agent preparation method was different. 2 parts of phosphate buffer solution were added to 5.5 parts of 6% sodium dodecylbenzene sulfonate solution and mixed thoroughly to obtain the soaking agent. No stabilizing modifier was used in the preparation of the bonding stabilizer. The performance of the products showed a trend of deterioration. The fact that no stabilizing modifier was used in the preparation of the bonding stabilizer had the greatest impact on the preparation of the bonding stabilizer.
[0140] When glass fiber liquid is not added in the preparation of the modified reinforcing agent, glass fiber liquid is replaced by glass fiber, nano-silicon dioxide liquid is not added in the preparation of the modified reinforcing agent, and nano-silicon dioxide liquid is replaced by nano-silicon dioxide, the performance of the product tends to deteriorate. Only the modified reinforcing agent prepared by combining the glass fiber liquid and nano-silicon dioxide liquid obtained by the method of the present invention has the most significant performance effect of the product. The effects of other methods are not as obvious as those of the present invention.
[0141] The preparation method of the stabilizing modifier is as follows:
[0142] 6.5 parts of hydroxyapatite, 2 parts of nano-silica sol, 4 parts of 5% by mass sodium lignin sulfonate solution, 0.30 parts of yttrium oxide and 1.5 parts of 8% by mass sodium alginate solution were fully mixed to obtain a stabilizing modifier.
[0143] From the above tests, it can be seen that the stabilizing modifier has a significant effect on the performance of the product. Based on this, the present invention further explores the performance of the product through the stabilizing modifier;
[0144] Experimental example 1.
[0145] The only difference from Example 3 is that hydroxyapatite is not added to the stabilizing modifier.
[0146] Experimental example 2.
[0147] The only difference from Example 3 is that yttrium oxide is not added to the stabilizing modifier.
[0148] Experimental Example 3.
[0149] The only difference from Example 3 is that no nano-silica sol and sodium alginate solution are added in the preparation of the stabilizing modifier.
[0150] Experimental Example 4.
[0151] The only difference from Example 3 is that the sodium lignin sulfonate solution is replaced by deionized water.
[0152] The product performance test results of Experimental Examples 1-4 are as follows:
[0153]
[0154] It can be seen from Experimental Examples 1-4 that when hydroxyapatite is not added to the stabilizing modifier, the performance of the product deteriorates significantly, followed by when yttrium oxide is not added, and the performance of the product also shows a significant deterioration trend. When nano-silica sol, sodium alginate solution, and sodium lignin sulfonate solution are not added in the preparation of the stabilizing modifier and deionized water is used instead, the performance of the product tends to deteriorate. At the same time, the combination of hydroxyapatite and yttrium oxide is proprietary, and other raw materials and processes are used in the preparation of the stabilizing modifier. The performance effects of the products are not as significant as those of the present invention. Only the stabilizing modifier obtained by the method of the present invention has the most significant product performance effect.
[0155] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be considered exemplary and non-restrictive in all respects, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims be included in the present invention.
[0156] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.
Claims
1. A glue composition for copper-clad laminates, characterized in that: It includes the following raw materials in parts by weight: 35-40 parts of epoxy resin, 8-12 parts of bonding stabilizer, 5-7 parts of silane coupling agent, 4-6 parts of modifying reinforcing agent, 3-6 parts of curing agent, 1-3 parts of accelerator, 30-35 parts of solvent; The preparation method of the bonding stabilizer is as follows: S01: irradiating the boron nitride flakes in a proton irradiation box, and obtaining an irradiated boron nitride agent after the irradiation is completed; S02: Preparation of infusion agent: Add 2 to 5 parts of 5% chitosan solution and 1 to 3 parts of phosphate buffer solution to 4 to 7 parts of 6% sodium dodecylbenzene sulfonate solution, then add 0.35 to 0.45 parts of silane coupling agent KH550, continue to mix thoroughly, and obtain an infusion agent; S03: immersing the irradiated boron nitride agent into a soaking agent that is 3 to 5 times the total amount of the irradiated boron nitride agent for soaking and improvement treatment, and after the soaking and adjustment is completed, filtering and drying are performed to obtain a soaked boron nitride body; S04: The leached boron nitride body and the stabilizing modifier are mixed and ball-milled in a weight ratio of 5:3, with a ball-milling speed of 1000-1500 r / min for 2 hours. After the ball-milling is completed, the mixture is washed with water and dried to obtain a stabilizing agent; The irradiation power of the irradiation treatment is 350-400W, and the irradiation time is 10-15 minutes; the pH value of the phosphate buffer solution is 5.0-6.0; The soaking power of the improved soaking treatment is 400-450W, and the soaking time is 5-10min; The preparation method of the stabilizing modifier is: 5 to 8 parts of hydroxyapatite, 1 to 3 parts of nano-silica sol, 3 to 5 parts of 5% by mass sodium lignin sulfonate solution, 0.25 to 0.35 parts of yttrium oxide and 1 to 2 parts of 8% by mass sodium alginate solution are fully mixed to obtain a stabilizing modifier; The preparation method of the modified reinforcing agent is: S11: adding 1 to 3 parts of tetrabutyl titanate to 5 to 7 parts of ethanol solvent, and then adding 2 to 5 parts of sodium citrate solution and 2 to 4 parts of nano-silicon dioxide, stirring and mixing to obtain nano-silicon dioxide liquid; S12: feeding the glass fiber into a lanthanum nitrate solution which is 3 to 5 times the total amount of the glass fiber and mixing well to obtain a glass fiber liquid; The glass fiber liquid and the nano-silica liquid are mixed and ball-milled in a weight ratio of 5:3, the mixing ball mill speed is 1000-1500r / min, the mixing is carried out for 1h, and after the mixing is completed, the mixture is washed with water and dried to obtain a modified reinforcing agent.
2. The adhesive composition for copper clad laminate according to claim 1, characterized in that: The adhesive composition for copper clad laminate comprises the following raw materials in parts by weight: 37.5 parts of epoxy resin, 10 parts of bonding stabilizer, 6 parts of silane coupling agent, 5 parts of modifying reinforcing agent, 4.5 parts of curing agent, 2 parts of accelerator, and 32.5 parts of solvent.
3. The adhesive composition for copper clad laminate according to claim 1, characterized in that: The epoxy resin is a bisphenol A epoxy resin with an epoxy equivalent of 185 to 190 g / eq and a viscosity of 12000 to 15000 cps at 25°C; The solvent is dimethylformamide; the accelerator is 2-methylimidazole; the curing agent is triethylenetetramine; and the silane coupling agent is silane coupling agent KH560.
4. The adhesive composition for copper clad laminate according to claim 1, characterized in that: The mass fraction of the sodium citrate solution is 5-8%; the mass fraction of the lanthanum nitrate solution is 2-5%.
5. A method for preparing the adhesive composition for copper clad laminates according to any one of claims 1 to 4, characterized in that: The following steps are involved: The adhesive composition can be obtained by uniformly mixing the raw materials according to the proportion.