A negative electrode composite material, a negative electrode sheet and a battery
By using a boron-doped carbon material in NiS particles to form a negative electrode composite with a spherical structure, the problems of poor composite uniformity between NiS and carbon materials and particle agglomeration in the prior art are solved, and the electrochemical performance and cycle life are improved.
Patent Information
- Application Number
- CN202411127592.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-08-16
AI Technical Summary
In the prior art, NiS and carbon materials have poor composite uniformity, the carbon layer affects lithium ion migration, and particles are prone to agglomeration during the cycle, resulting in poor NiS rate performance and cycle life.
Boron-doped carbon material is used as a sheet-like porous framework, NiS particles are embedded to form a negative electrode composite material with a spherical structure, and the dispersion and structure of the carbon material are controlled through a specific preparation method to improve the conductivity and electron transfer rate.
It improves the electrochemical dynamics of the negative electrode composite material, reduces the particle agglomeration phenomenon, and improves the rate performance and cycle life.
Smart Images

Figure CN118676352B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of new energy batteries, and in particular to a negative electrode composite material, a negative electrode sheet and a battery. Background Art
[0002] Nickel sulfide (NiS) has attracted much attention as a negative electrode material for batteries due to its advantages such as high theoretical specific capacity and appropriate voltage platform. However, during the cycle, NiS materials will produce severe volume changes, leading to structural collapse and shortened cycle life; NiS has low intrinsic conductivity, which is not conducive to the rapid transfer of electrons and poor rate performance. In order to alleviate the above problems, NiS is compounded with carbon materials, which can effectively alleviate excessive volume changes and particle aggregation during the cycle, and improve electron / ion transmission efficiency and structural integrity.
[0003] In the prior art, there are studies on improving the performance of NiS sodium negative electrode with the help of composite carbon materials. Patent document CN112018344A discloses a carbon-coated nickel sulfide electrode material and its preparation method and application, which specifically discloses preparing an ethylene glycol aqueous solution first; adding glucose to the ethylene glycol aqueous solution until it is completely dissolved to obtain an ethylene glycol-glucose mixed solution; adding a nickel source and a sulfur source to the ethylene glycol-glucose mixed solution in sequence until they are completely dissolved, and performing a hydrothermal reaction until the reaction is completed to obtain a hydrothermal reaction product; separating the hydrothermal reaction product into solid and liquid, washing the obtained solid separation, drying, and calcining under a protective atmosphere to obtain a carbon-coated nickel sulfide electrode material, and the electrical performance of the NiS material after carbon coating is significantly improved. However, this coating method has poor composite uniformity of carbon materials, the carbon layer affects the migration of lithium ions, and the particles are easy to agglomerate during the cycle.
[0004] Therefore, while the field uses carbon materials to improve the rate performance and cycle life of NiS, it is still necessary to further uniformly composite carbon materials without affecting sodium ion migration and reducing particle agglomeration. Summary of the invention
[0005] In view of this, the present invention is committed to providing a negative electrode composite material, a negative electrode plate and a battery to solve the problems in the prior art of poor uniformity of NiS and carbon material composite, carbon layer affecting lithium ion migration, and easy agglomeration of particles during the cycle.
[0006] A first aspect of the present invention provides a negative electrode composite material having a flower ball-like structure formed by stacking a plurality of sheet layers;
[0007] The sheet layer includes a sheet-like porous skeleton and NiS particles embedded in the sheet-like porous skeleton, wherein the sheet-like porous skeleton is a carbon material doped with boron atoms.
[0008] Optionally, the average lateral size of the negative electrode composite material is 3-5 μm; and / or the specific surface area of the negative electrode composite material is 400-800 m 2 / g.
[0009] Optionally, the sheet diameter of the flaky porous skeleton is 1~2μm; and / or, the thickness of the flaky porous skeleton is 30~40nm; and / or, the pore diameter of the flaky porous skeleton is 10~30nm; and / or, the porosity of the flaky porous skeleton is 15~30%; and / or, in the flaky porous skeleton, the molar ratio of boron element to carbon element is 1:7~9.
[0010] Optionally, the average particle size of the NiS particles is 10-30 nm; and / or, based on the total mass of the negative electrode composite material, the content of the NiS particles is 60-80 wt %.
[0011] A second aspect of the present invention provides a method for preparing a negative electrode composite material, the method comprising the following steps:
[0012] S1, adding nickel salt, complexing agent, hexose and boron source into a solvent for mixing to obtain a first material; performing hydrothermal treatment on the first material to obtain a second material;
[0013] S2, centrifuging the second material, collecting the precipitate, washing it, and drying it to obtain a precursor;
[0014] S3, carbonizing the precursor to obtain a carbonized precursor; mixing the carbonized precursor with sulfur powder and performing a sulfurization treatment.
[0015] Optionally, the nickel salt is selected from at least one of nickel nitrate, nickel sulfate, nickel chloride and nickel acetate; and / or the complexing agent is selected from at least one of nitrilotriacetic acid, ethylenediaminetetraacetic acid, hexamethylenetetramine, diisopropyltetramine and tetrahydroxypropylethylenediamine; and / or the hexose is selected from at least one of glucose, maltose, sucrose and galactose; and / or the boron source is selected from at least one of sodium tetraborate decahydrate, sodium tetraborate pentahydrate and anhydrous sodium tetraborate; and / or the solvent is water.
[0016] Optionally, the molar ratio of the nickel salt, the complexing agent, the hexose and the boron source is 1:3~7:1~4:0.1~1.5; and / or the mass ratio of the nickel salt to the solvent is 1:150~250; and / or the molar ratio of the carbonized precursor to the sulfur powder is 1:1~5.
[0017] Optionally, in step S1, the mixing treatment is magnetic stirring; the conditions of the magnetic stirring include: stirring time of 20~40min, stirring speed of 200~400r / min; and / or, the hydrothermal treatment is carried out in a polytetrafluoroethylene reactor; and / or, the conditions of the hydrothermal treatment include: temperature of 160~200℃, time of 6~12h; and / or, in step S2, the washing liquid used for washing is selected from anhydrous ethanol and / or water; and / or, the conditions of the drying treatment include: temperature of 50~70℃, time of 18~36h; and / or, in step S3, the carbonization treatment and the vulcanization treatment are carried out in a protective atmosphere; and / or, the conditions of the carbonization treatment include: carbonization temperature of 500~650℃, carbonization time of 1~3h; and / or, the conditions of the vulcanization treatment include: vulcanization temperature of 280~350℃, vulcanization time of 1~3h.
[0018] A third aspect of the present invention provides a negative electrode plate, comprising a current collector and a negative electrode composite material arranged on the surface of the current collector, wherein the negative electrode composite material comprises the above-mentioned negative electrode composite material and / or the negative electrode composite material prepared according to the above-mentioned method.
[0019] A fourth aspect of the present invention provides a battery, comprising the negative electrode plate described above.
[0020] Through the above technical solution, the beneficial technical effects of the present invention are:
[0021] (1) The negative electrode composite material provided by the present invention has a flower ball-like structure formed by stacking a number of sheets. The flower ball-like structure material with uniform morphology of the present invention is conducive to improving the ion diffusion rate, reducing the particle agglomeration phenomenon, and thus improving the electrochemical kinetic performance of the material. Among them, the sheet layer in the present invention includes a sheet-like porous skeleton and NiS particles embedded in the sheet-like porous skeleton. Due to the presence of uniform carbon material, the conductivity of the composite material is increased, and boron doping further increases the electron transfer rate, the rate performance of the negative electrode composite material is improved, and the cycle life is increased.
[0022] (2) The preparation method of the negative electrode composite material of the present invention is to add a boron source during the preparation of the precursor, and further control the amount of the hexose carbon source and the boron source, thereby adjusting the boron-containing precursor with uniform morphology, and then placing the precursor in a tube furnace for carbonization and then sulfurization to obtain a nickel sulfide composite boron-doped carbon flower ball material (NiS / BC) with uniform morphology. Hexose will isomerize into fructose that is easier to dehydrate during the hydrothermal process, and at the same time produce a part of hydroxymethylfurfural (HMF). HMF will catalyze the hexose to further convert into fructose through acetal reaction, and fructose will be dehydrated to form HMF (this process consumes part of HMF), and then HMF will polymerize to form carbon material. The boron source can replace HMF and hexose to undergo acetal reaction, reducing the consumption of HMF, so that the hexose produces a large amount of HMF during the hydrothermal process. The increase of HMF will produce a large number of nucleation points, so the obtained carbon material is evenly dispersed. During the hydrothermal process, carbon materials undergo decomposition reactions and generate some acidic substances, which lead to unstable pH during the hydrothermal preparation of precursors, which is not conducive to the formation of a flower-ball-like structure. By controlling the amount of hexose and boron source added, the effect of acidic substances on the nucleation and growth of the precursor nickel hydroxide can be reduced, which is beneficial to the formation of a flower-ball shape of the precursor.
[0023] Other features and advantages of the present invention will be described in detail in the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] The accompanying drawings are used to provide further understanding of the present invention and constitute a part of the specification. Together with the following specific embodiments, they are used to explain the present invention, but do not constitute a limitation of the present invention.
[0025] Figure 1 Shown is an electron microscope scanning image of the negative electrode composite material prepared in Example 1. DETAILED DESCRIPTION
[0026] The present invention discloses a negative electrode composite material, a negative electrode sheet and a battery. Those skilled in the art can refer to the content of this article and appropriately improve the process parameters to achieve it. It should be particularly noted that all similar substitutions and modifications are obvious to those skilled in the art, and they are all considered to be included in the present invention. The method and application of the present invention have been described through preferred embodiments, and relevant personnel can obviously modify or appropriately change and combine the methods and applications described herein without departing from the content, spirit and scope of the present invention to implement and apply the technology of the present invention.
[0027] In the description of the present invention, a list of items connected by the term "at least one of" or other similar terms may mean any combination of the listed items. For example, if items A, B are listed, the phrase "at least one of A, B" means only A; only B; or A and B. In another example, if items A, B, C are listed, the phrase "at least one of A, B, C" means only A; or only B; only C; A and B (excluding C); A and C (excluding B); B and C (excluding A); or all of A, B, and C. Item A may include a single element or multiple elements. Item B may include a single element or multiple elements. Item C may include a single element or multiple elements.
[0028] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range or the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0029] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.
[0030] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.
[0031] If there is no special explanation, the "include" and "comprising" mentioned in this application are open-ended or closed-ended. For example, the "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.
[0032] In order to solve the problems in the prior art that the composite uniformity of NiS and carbon materials is poor, the carbon layer affects the migration of lithium ions, and the particles are easy to agglomerate during the cycle, the present invention adopts the following technical solutions:
[0033] The first aspect of the present invention provides a negative electrode composite material, such as Figure 1 As shown, the negative electrode composite material has a flower ball-like structure formed by stacking a number of sheets;
[0034] The sheet layer includes a sheet-like porous skeleton and NiS particles embedded in the sheet-like porous skeleton, wherein the sheet-like porous skeleton is a carbon material doped with boron atoms.
[0035] The flower ball-shaped structural material with uniform morphology provided by the present invention is conducive to improving the ion diffusion rate, reducing the particle agglomeration phenomenon, and thus improving the electrochemical kinetic performance of the material. Among them, the sheet layer in the present invention includes a flaky porous skeleton and NiS particles embedded in the flaky porous skeleton. Due to the presence of uniform carbon material, the conductivity of the composite material increases, and boron doping further increases the electron transmission rate, the rate performance of the NiS / BC composite material is improved, and the cycle life is improved.
[0036] According to the present invention, the average lateral size of the negative electrode composite material is 3~5μm. In the present invention, "the average lateral size of the negative electrode composite material" can be defined as: the negative electrode composite material with a flower ball structure is regarded as a spherical particle and / or an ellipsoidal particle as a whole, and the average value of the diameter of the spherical particle and / or the long diameter of the ellipsoidal particle is the average lateral size of the negative electrode composite material in the present invention. Negative electrode active materials with uniform morphology are conducive to improving the ion diffusion rate and reducing the particle agglomeration phenomenon. Exemplarily, the average lateral size of the negative electrode active material can be any value among 3μm, 3.5μm, 3.8μm, 4μm, 4.2μm, 4.5μm and 5μm, or any value within the range of any two of the above values. Preferably, the average lateral size of the negative electrode active material is 3.5~4.5μm, and the ion diffusion rate of the negative electrode active material within this lateral size range is further improved.
[0037] According to the present invention, the negative electrode composite material has a large specific surface area. Optionally, the specific surface area of the negative electrode composite material can be 400-800 m 2 / g; For example, the specific surface area of the negative electrode composite material can be 400 m 2 / g、500m 2 / g, 600 m 2 / g, 700 m 2 / g and 800 m 2 Preferably, in order to further improve the channel for ion migration, shorten the migration path, and improve the rate performance of the battery, the specific surface area of the negative electrode composite material is 600-800m 2 / g.
[0038] In the present invention, the appropriate sheet diameter and thickness of the sheet-like porous skeleton are beneficial to controlling the particle uniformity of the negative electrode composite material.
[0039] According to the present invention, the sheet diameter of the flaky porous skeleton may be 1-2 μm; in the present invention, "the sheet diameter of the flaky porous skeleton" may be defined as the extension dimension of the flaky porous skeleton in the extension direction of the flaky porous skeleton as the radial direction. Exemplarily, the sheet diameter of the flaky porous skeleton may be any value among 1 μm, 1.2 μm, 1.4 μm, 1.6 μm, 1.8 μm and 2 μm, or any value within the range of any two of the above values. Preferably, in order to further improve the structural stability of the composite material, the sheet diameter of the flaky porous skeleton may be 1-1.5 μm.
[0040] According to the present invention, the thickness of the sheet-like porous skeleton can be 30-40 nm; in the present invention, "the thickness of the sheet-like porous skeleton" can be defined as the dimension of the sheet-like porous skeleton perpendicular to the extension direction of the sheet-like porous skeleton as the radial direction. Exemplarily, the thickness of the sheet-like porous skeleton can be any value among 30 nm, 32 nm, 34 nm, 36 nm, 38 nm and 40 nm or any value within the range of values composed of any two of the above values. Preferably, in order to further shorten the ion and electron transport path of the porous skeleton, the thickness of the sheet-like porous skeleton can be 30-35 nm.
[0041] According to the present invention, the reasonable pore size distribution of the sheet-like porous skeleton can balance the charge and discharge rate and the cycle life, and improve the overall performance of the battery. The pore size of the sheet-like porous skeleton can be 10-30 nm; illustratively, the pore size of the sheet-like porous skeleton can be any value among 10 nm, 15 nm, 20 nm, 25 nm and 30 nm, or any value within the range of any two of the above values. Preferably, in order to further improve the ion and electron transport efficiency of the porous skeleton, the pore size of the sheet-like porous skeleton can be 10-20 nm.
[0042] According to the present invention, the sheet-like porous skeleton has a larger porosity to accommodate more active materials and electrolytes, thereby increasing the energy density of the battery. The porosity of the sheet-like porous skeleton can be 15-30%; illustratively, the porosity of the sheet-like porous skeleton can be any value among 15%, 20%, 25% and 30% or any value within the range of any two of the above values. Preferably, in order to further stabilize the structure and increase the ion transmission path, the porosity of the sheet-like porous skeleton can be 20-30%.
[0043] According to the present invention, in the lamellar porous skeleton, a reasonable boron-carbon ratio is conducive to forming a uniformly morphological NiS / BC flower ball structure material, and the molar ratio of boron to carbon can be 1:7~9. Exemplarily, the molar ratio of boron to carbon can be any value among 1:7, 1:7.5, 1:8, 1:8.5 and 1:9, or any value within the range of any two of the above values. Preferably, an appropriate amount of boron doping can enable the doped carbon material to obtain the best electrical conductivity. In the lamellar porous skeleton, the molar ratio of boron to carbon is 1:8~9.
[0044] According to the present invention, in order not to affect sodium ion migration, reduce particle agglomeration and improve NiS rate performance and cycle life, the average particle size of the NiS particles can be 10-30 nm; illustratively, the average particle size of the NiS particles can be any value among 10 nm, 15 nm, 20 nm, 25 nm and 30 nm or any value within the range of any two of the above values. Preferably, the suitable NiS particle size can ensure the contact area and ion transfer speed with the electrolyte, and the average particle size of the NiS particles can be 10-20 nm.
[0045] According to the present invention, in order to improve the theoretical specific capacity of the battery, the negative electrode composite material of the present invention contains more NiS particles. Based on the total mass of the negative electrode composite material, the content of the NiS particles can be 60-80wt%; illustratively, the content of the NiS particles can be any value among 60 wt%, 65 wt%, 70 wt%, 75 wt% and 80 wt% or any value within the range of any two of the above values. Preferably, the content of an appropriate amount of NiS particles can ensure sufficient capacity, and there is sufficient boron-doped carbon material to increase the stability and conductivity of the system, and enhance the cycle and rate capacity of the negative electrode composite material. The content of the NiS particles can be 70-80wt%.
[0046] A second aspect of the present invention provides a method for preparing a negative electrode composite material, the method comprising the following steps:
[0047] S1, adding nickel salt, complexing agent, hexose and boron source into a solvent for mixing to obtain a first material; performing hydrothermal treatment on the first material to obtain a second material;
[0048] S2, centrifuging the second material, collecting the precipitate, washing it, and drying it to obtain a precursor;
[0049] S3, carbonizing the precursor to obtain a carbonized precursor; mixing the carbonized precursor with sulfur powder and performing a sulfurization treatment.
[0050] According to the present invention, in the precursor in step S2, the carbon material mainly exists between the layered nickel hydroxide sheets after the hydrothermal process, and the nickel hydroxide nanosheets are stacked into a flower ball-like structure (the flower ball-like structure at this time provides a template for the porous nanosheets to form a flower ball-like structure after carbonization); after the precursor is carbonized in step S3, the carbon source becomes a boron-doped porous carbon nanosheet, the porous nanosheets form a flower ball-like carbon skeleton, and the nickel hydroxide becomes a nickel intermediate phase (no longer a lamellar structure, but attached to the porous nanosheets); during the sulfurization process of the carbonized precursor, the nickel sulfide particles crystallize, nucleate and grow on the porous nanosheets (from the nickel intermediate phase to nickel sulfide) and are partially embedded in the porous carbon nanosheets, and finally a nickel sulfide-modified porous carbon nanosheet is formed, and the porous nanosheets form a flower ball-like structure.
[0051] In the preparation method of the present invention, hexose will isomerize into fructose that is easier to dehydrate during the hydrothermal process, and a portion of hydroxymethylfurfural (HMF) will be produced at the same time. HMF will catalyze the hexose to further convert into fructose through acetalization reaction, and fructose will be dehydrated to form HMF (this process consumes part of HMF, and the consumed HMF does not disappear, but is converted into other substances; HMF is used as a nucleation site, the number of HMF decreases, the nucleation sites also decrease, and the carbon composite effect will decrease), and then HMF will be polymerized to form a carbon material. The boron source can replace HMF and hexose to undergo acetalization reaction, which can reduce the consumption of HMF, so that the hexose produces a large amount of HMF during the hydrothermal process, and the increase of HMF will produce a large number of nucleation points, so the obtained carbon material is evenly dispersed. During the hydrothermal process, carbon materials undergo decomposition reactions and generate acidic substances, which lead to unstable pH during the hydrothermal preparation of precursors, which is not conducive to the formation of a flower-ball-like structure. By controlling the amount of hexose and boron source added, the effect of acidic substances on the nucleation and growth of the precursor nickel hydroxide can be reduced, which is beneficial for the precursor to form a flower-ball-like shape.
[0052] According to the present invention, the nickel salt may be selected from at least one of nickel nitrate, nickel sulfate, nickel chloride and nickel acetate.
[0053] According to the present invention, the complexing agent can be selected from at least one of nitrilotriacetic acid, ethylenediaminetetraacetic acid, hexamethylenetetramine, diisopropyltetramine and tetrahydroxypropylethylenediamine.
[0054] According to the present invention, the hexose can be selected from at least one of glucose, maltose, sucrose and galactose.
[0055] According to the present invention, the boron source can be selected from at least one of sodium tetraborate decahydrate, sodium tetraborate pentahydrate and anhydrous sodium tetraborate, wherein the sodium source in the boron source can form a SEI film in the subsequent first cycle of charge and discharge, provide additional sodium ions for the SEI film, reduce the loss of sodium ions, and improve the first cycle coulombic efficiency.
[0056] According to the present invention, the solvent is water.
[0057] According to the present invention, during the hydrothermal process, the complexing agent hydrolyzes hydroxide, and nickel ions combine with it to form nickel hydroxide. The appropriate content of hexose and boron source will promote the hydrothermal nucleation of nickel hydroxide and improve the cycle life of the battery. Optionally, the molar ratio of the nickel salt, the complexing agent, the hexose and the boron source can be 1:3~7:1~4:0.1~1.5; preferably, the molar ratio of the nickel salt, the complexing agent, the hexose and the boron source can be 1:4~6:1~2:0.1~0.5; preferably, the molar ratio of the nickel salt, the complexing agent, the hexose and the boron source can be 1:5:1~2:0.1~0.5.
[0058] According to the present invention, the mass ratio of the nickel salt to the solvent may be 1:150-250; illustratively, the mass ratio of the nickel salt to the solvent may be any one of 1:150, 1:175, 1:200, 1:225 and 1:250 or any value within the range of any two of the above values. Preferably, in order to better disperse the materials in the solvent, the mass ratio of the nickel salt to the solvent may be 1:180-220.
[0059] According to the present invention, in order to avoid the accumulation of excessive sulfur on the surface of the negative electrode material, thereby affecting the material properties, the molar ratio of the carbonized precursor and the sulfur powder can be 1:1-5; illustratively, the molar ratio of the carbonized precursor and the sulfur powder can be any value among 1:1, 1:2, 1:3, 1:4 and 1:5 or any value within the range of any two of the above values. Preferably, the molar ratio of the carbonized precursor and the sulfur powder can be 1:2-4.
[0060] In an optional embodiment of the present invention, in step S1, the mixing treatment can be magnetic stirring; the conditions of the magnetic stirring can include: a stirring time of 20 to 40 minutes, a stirring speed of 200 to 400 r / min; and / or, the hydrothermal treatment can be carried out in a polytetrafluoroethylene reactor; and / or, the conditions of the hydrothermal treatment can include: a temperature of 160 to 200°C, a time of 6 to 12 hours, preferably 8 to 12 hours.
[0061] In an optional embodiment of the present invention, in step S2, the washing liquid used in the washing can be selected from anhydrous ethanol and / or water; illustratively, the washing of the present invention can be washing three times with water and ethanol respectively to remove excess growth and unstable impurities. Preferably, the drying conditions may include: a temperature of 50-70°C and a time of 18-36 hours.
[0062] In an optional embodiment of the present invention, in step S3, the carbonization treatment and the sulfurization treatment can be carried out in a protective atmosphere to prevent air from entering, wherein the protective atmosphere can be one of nitrogen, argon, neon, helium, xenon and krypton. And / or, the conditions of the carbonization treatment may include: a carbonization temperature of 500-650°C and a carbonization time of 1-3h; preferably, the carbonization temperature is 550-600°C, and this temperature range can produce uniform amorphous carbon. And / or, the conditions of the sulfurization treatment may include: a sulfurization temperature of 280-350°C and a sulfurization time of 1-3h.
[0063] A third aspect of the present invention provides a negative electrode plate, comprising a current collector and a negative electrode composite material arranged on the surface of the current collector, wherein the negative electrode composite material comprises the above-mentioned negative electrode composite material and / or the negative electrode composite material prepared according to the above-mentioned method.
[0064] As an example, the negative electrode current collector has two surfaces facing each other in its thickness direction, and the negative electrode active material layer is disposed on the side in contact with the separator so that the negative electrode active material reacts with ions released from the positive electrode.
[0065] The present application has no particular restrictions on the material of the negative electrode current collector, as long as the purpose of the present application can be achieved, and it can be selected according to actual needs. For example, in some embodiments, the negative electrode current collector includes common copper foil (the copper foil can be modified, such as the setting of a carbon coating layer, screen-printed copper foil, porous copper foil, copper mesh, etc.), or the negative electrode current collector can adopt a composite current collector structure (such as a composite current collector structure containing a polymer layer and a metal layer), and those skilled in the art can make adaptive selections according to actual needs.
[0066] In some embodiments, the negative electrode active material layer includes the negative electrode composite material described above and also includes a basic negative electrode material, that is, the negative electrode active material of the negative electrode active material layer may be composed of the negative electrode composite material of this embodiment and a conventional negative electrode material. Optionally, the basic negative electrode material (conventional negative electrode material) may be a carbon material. As an example, the basic negative electrode material may be conventional negative electrode materials such as artificial graphite, natural graphite, soft carbon, and hard carbon.
[0067] In some embodiments, the negative electrode active material layer also includes a conductive agent, a binder and a solvent. The present application has no particular restrictions on the type of conductive agent, which can also be selected by conventional technology. As an example, the conductive agent includes but is not limited to a combination of one or more of superconducting carbon, conductive graphite, conductive carbon black (including acetylene black, Ketjen black, etc.), carbon nanotubes (including single-walled carbon nanotubes and / or multi-walled carbon nanotubes), graphene or carbon fiber. The present application has no particular restrictions on the type of conductive agent, which can also be selected by conventional technology. As an example, the binder includes but is not limited to a combination of one or more of polyvinylidene fluoride (PVDF), styrene butadiene rubber (SBR), sodium carboxymethyl cellulose (CMC), polyacrylate (LA), polyacrylic acid binder (PAA), etc. The present application has no particular restrictions on the type of negative electrode solvent, which can also be selected by conventional technology. As an example, the negative electrode solvent can be N-methylpyrrolidone (NMP).
[0068] In a preferred embodiment of the present invention, the preparation method of the negative electrode sheet may include: pouring the negative electrode composite material, the binder, and the conductive agent into an agate mortar in a certain proportion in sequence, mixing and grinding until the powder is evenly mixed and fine. Then pour it into a small weighing bottle, and drop the negative electrode solvent while stirring magnetically until the powder is evenly infiltrated and the drop is stopped. Then magnetic stirring and ultrasonic treatment are performed, and this process is repeated 1 to 3 times. The mixed slurry is evenly coated and flattened on the current collector aluminum foil with a coater, and then placed in a drying oven for drying. Then the pole piece is cut into a circular pole piece with a slicer, and the circular pole piece is compacted with a tablet press and weighed to obtain a negative pole piece. Exemplarily, the mixing mass ratio of the negative electrode composite material, the binder, and the conductive agent can be (6 to 10): (0.8 to 1.2): 1, for example, it can be 8: 1: 1.
[0069] A fourth aspect of the present invention provides a battery, comprising the negative electrode plate described above.
[0070] In the embodiment of the present invention, the battery structure includes but is not limited to button batteries, soft-pack batteries, cylindrical batteries, etc.
[0071] The present invention is further described in detail by way of examples. The raw materials used in the examples can be obtained through commercial sources. The binder used in the examples and comparative examples is PVDF, and the conductive agent is conductive carbon black (Super P).
[0072] Example 1
[0073] (1) Weigh 0.04 mol of nickel nitrate hexahydrate, 0.2 mol of ethylenediaminetetraacetic acid, 0.06 mol of glucose, and 0.01 mol of sodium tetraborate pentahydrate into a beaker with a magnet and 2000 mL of distilled water, and stir for 30 min at a stirring speed of 300 r / min to obtain a first material. Then add the first material into a polytetrafluoroethylene reactor, place the reactor in an oven for hydrothermal reaction, control the hydrothermal temperature at 180°C, and the hydrothermal time for 8 h to obtain a second material.
[0074] (2) The second material was centrifuged at high speed, and the precipitate was collected and washed three times with anhydrous ethanol and deionized water respectively. Finally, the precipitate was dried in a drying oven at a constant temperature of 60° C. for 24 hours to obtain a precursor.
[0075] (3) The precursor is first carbonized at a carbonization temperature of 550°C for 2 hours. After the carbonization is completed, the carbonized precursor and sulfur powder are mixed in a molar ratio of 1:3 and placed in a magnetic boat. The magnetic boat is then placed in a tubular furnace for sulfurization at a temperature of 300°C for 2 hours. The carbonization and sulfurization are carried out in a protective atmosphere (the protective atmosphere in this embodiment is nitrogen). Finally, the negative electrode composite material of this embodiment is obtained.
[0076] (4) Preparation of negative electrode sheet: The prepared negative electrode composite material, binder and conductive agent are poured into an agate mortar in a mass ratio of 8:1:1, and mixed and ground for 30 min until the powder is evenly mixed and fine. Then pour it into a small weighing bottle, and add N-methylpyrrolidone solvent while stirring magnetically until the powder is evenly soaked and then stop adding. Then stir magnetically for 20 min and then ultrasonically treat for 15 min, and repeat this process 3 times. The mixed slurry is evenly coated and scraped on one side of the current collector aluminum foil with a coater, and then placed in a drying oven, set to a constant temperature of 80°C, and taken out after drying for 12 h. Then use a slicer to cut the electrode sheet into a circular electrode sheet with a radius of 6 mm, and the circular electrode sheet is compacted with a tablet press and weighed to obtain the negative electrode sheet.
[0077] (5) Preparation of half-cell: The prepared negative electrode composite material was used as the working electrode, the metal sodium sheet was used as the reference electrode, Whatman GF / D glass fiber was used as the separator, nickel foam was used as the gasket, and 1 mol·L -1 The diglycol methyl ether (diglyme) solution of NaPF6 was used as the electrolyte of the sodium ion battery and was added dropwise. The half-cell was assembled in the order of the positive electrode shell, the negative electrode sheet, the separator, the sodium sheet, the nickel foam and the negative electrode shell. The assembled half-cell was clamped on the packaging machine with insulating tweezers for sealing. Finally, the packaged battery was taken out of the glove box and left to stand for 24 hours to allow the electrolyte to fully infiltrate before conducting relevant electrochemical tests.
[0078] Example 2
[0079] (1) Weigh 0.04 mol of nickel nitrate hexahydrate, 0.2 mol of ethylenediaminetetraacetic acid, 0.04 mol of sucrose, and 0.016 mol of sodium tetraborate pentahydrate into a beaker with a magnet and 2000 mL of distilled water, and stir for 30 min at a stirring speed of 300 r / min to obtain a first material. Then add the first material into a polytetrafluoroethylene reactor, and place the reactor in an oven for hydrothermal reaction. Control the hydrothermal temperature at 180°C and the hydrothermal time for 8 h to obtain a second material.
[0080] (2) The second material was centrifuged at high speed, and the precipitate was collected and washed three times with anhydrous ethanol and deionized water respectively. Finally, the precipitate was dried in a drying oven at a constant temperature of 60°C for 24 hours to obtain a precursor.
[0081] (3) The precursor is first carbonized at a carbonization temperature of 600°C for 2 hours. After the carbonization is completed, the carbonized precursor and sulfur powder are mixed in a molar ratio of 1:3 and placed in a magnetic boat. The magnetic boat is then placed in a tubular furnace for sulfurization at a temperature of 300°C for 2 hours. The carbonization and sulfurization are carried out in a protective atmosphere (the protective atmosphere in this embodiment is nitrogen). Finally, the negative electrode composite material of this embodiment is obtained.
[0082] The manufacturing method of the negative electrode sheet and the sodium ion button half-cell of this embodiment is the same as that of Embodiment 1.
[0083] Example 3
[0084] (1) Weigh 0.04 mol of nickel nitrate hexahydrate, 0.2 mol of ethylenediaminetetraacetic acid, 0.08 mol of galactose, and 0.02 mol of sodium tetraborate pentahydrate into a beaker with a magnetic rod and 2000 mL of distilled water, and stir for 30 min at a stirring speed of 300 r / min to obtain a first material. Then add the first material into a polytetrafluoroethylene reactor, and place the reactor in an oven for hydrothermal reaction. The hydrothermal temperature is controlled at 180°C and the hydrothermal time is 8 h to obtain a second material.
[0085] (2) The second material was centrifuged at high speed, and the precipitate was collected and washed three times with anhydrous ethanol and deionized water respectively. Finally, the precipitate was dried in a drying oven at a constant temperature of 60°C for 24 hours to obtain a precursor.
[0086] (3) The precursor is first carbonized at a carbonization temperature of 500°C for 2 hours. After the carbonization is completed, the carbonized precursor and sulfur powder are mixed in a molar ratio of 1:3 and placed in a magnetic boat. The magnetic boat is then placed in a tubular furnace for sulfurization at a temperature of 300°C for 2 hours. The carbonization and sulfurization are carried out in a protective atmosphere (the protective atmosphere in this embodiment is nitrogen). Finally, the negative electrode composite material of this embodiment is obtained.
[0087] The manufacturing method of the negative electrode sheet and the sodium ion button half-cell of this embodiment is the same as that of Embodiment 1.
[0088] Example 4
[0089] (1) Weigh 0.04 mol of nickel nitrate hexahydrate, 0.2 mol of ethylenediaminetetraacetic acid, 0.12 mol of galactose, and 0.04 mol of sodium tetraborate pentahydrate into a beaker with a magnetic rod and 2000 mL of distilled water, and stir for 30 min at a stirring speed of 300 r / min to obtain a first material. Then add the first material into a polytetrafluoroethylene reactor, and place the reactor in an oven for hydrothermal reaction. Control the hydrothermal temperature at 180°C and the hydrothermal time for 8 h to obtain a second material.
[0090] (2) The second material was centrifuged at high speed, and the precipitate was collected and washed three times with anhydrous ethanol and deionized water respectively. Finally, the precipitate was dried in a drying oven at a constant temperature of 60°C for 24 hours to obtain a precursor.
[0091] (3) The precursor is first carbonized at a carbonization temperature of 500°C for 2 hours. After the carbonization is completed, the carbonized precursor and sulfur powder are mixed in a molar ratio of 1:3 and placed in a magnetic boat. The magnetic boat is then placed in a tubular furnace for sulfurization at a temperature of 300°C for 2 hours. The carbonization and sulfurization are carried out in a protective atmosphere (the protective atmosphere in this embodiment is nitrogen). Finally, the negative electrode composite material of this embodiment is obtained.
[0092] The manufacturing method of the negative electrode sheet and the sodium ion button half-cell of this embodiment is the same as that of Embodiment 1.
[0093] Example 5
[0094] (1) Weigh 0.04 mol of nickel nitrate hexahydrate, 0.2 mol of ethylenediaminetetraacetic acid, 0.02 mol of galactose, and 0.002 mol of sodium tetraborate pentahydrate into a beaker with a magnetic rod and 2000 mL of distilled water, and stir for 30 min at a stirring speed of 300 r / min to obtain a first material. Then add the first material into a polytetrafluoroethylene reactor, and place the reactor in an oven for hydrothermal reaction. The hydrothermal temperature is controlled at 180°C and the hydrothermal time is 8 h to obtain a second material.
[0095] (2) The second material was centrifuged at high speed, and the precipitate was collected and washed three times with anhydrous ethanol and deionized water respectively. Finally, the precipitate was dried in a drying oven at a constant temperature of 60°C for 24 hours to obtain a precursor.
[0096] (3) The precursor is first carbonized at a carbonization temperature of 500°C for 2 hours. After the carbonization is completed, the carbonized precursor and sulfur powder are mixed in a molar ratio of 1:3 and placed in a magnetic boat. The magnetic boat is then placed in a tubular furnace for sulfurization at a temperature of 300°C for 2 hours. The carbonization and sulfurization are carried out in a protective atmosphere (the protective atmosphere in this embodiment is nitrogen). Finally, the negative electrode composite material of this embodiment is obtained.
[0097] The manufacturing method of the negative electrode sheet and the sodium ion button half-cell of this embodiment is the same as that of Embodiment 1.
[0098] Comparative Example 1
[0099] (1) Weigh 0.04 mol of nickel nitrate hexahydrate and 0.2 mol of ethylenediaminetetraacetic acid, add them into a beaker with a magnet and 2000 mL of distilled water, and stir for 30 min to obtain a first material. Then add the first material into a polytetrafluoroethylene reactor, put the reactor into an oven for hydrothermal reaction, control the hydrothermal temperature at 180°C, and the hydrothermal time for 8 h to obtain a second material.
[0100] (2) The second material was centrifuged at high speed, and the precipitate was collected and washed three times with anhydrous ethanol and deionized water respectively. Finally, the precipitate was dried in a drying oven at a constant temperature of 60°C for 24 hours to obtain a precursor.
[0101] (3) The precursor and sulfur powder are mixed in a molar ratio of 1:3, put into a magnetic boat, and the magnetic boat is placed in a tube furnace for vulcanization. The vulcanization temperature is 300°C, the vulcanization time is 2 hours, and a powder composite material is obtained after the vulcanization is completed.
[0102] The manufacturing method of the negative electrode sheet and the sodium ion button half-cell of this comparative example is the same as that of Example 1.
[0103] Comparative Example 2
[0104] (1) Weigh 0.04 mol of nickel nitrate hexahydrate, 0.2 mol of ethylenediaminetetraacetic acid, and 0.06 mol of glucose, add them into a beaker with a magnet and 2000 mL of distilled water, and stir for 30 min to obtain a first material. Then add the first material into a polytetrafluoroethylene reactor, put the reactor into an oven for hydrothermal reaction, control the hydrothermal temperature at 180°C, and the hydrothermal time for 8 h to obtain a second material.
[0105] (2) The second material was centrifuged at high speed, and the precipitate was collected and washed three times with anhydrous ethanol and deionized water respectively. Finally, the precipitate was dried in a drying oven at a constant temperature of 60°C for 24 hours to obtain a precursor.
[0106] (3) The precursor is first carbonized at a carbonization temperature of 550°C for 2 hours. After the carbonization is completed, the carbonized precursor and sulfur powder are mixed in a molar ratio of 1:3 and placed in a magnetic boat. The magnetic boat is then placed in a tubular furnace for sulfurization at a temperature of 300°C for 2 hours. The carbonization and sulfurization are carried out in a protective atmosphere (the protective atmosphere in this comparative example is nitrogen). Finally, the negative electrode composite material of this comparative example is obtained.
[0107] The manufacturing method of the negative electrode sheet and the sodium ion button half-cell of this comparative example is the same as that of Example 1.
[0108] Test Example 1
[0109] First cycle capacity test: The sodium ion button half-cells prepared in the embodiment and the comparative example were respectively taken and first cycle capacity test was carried out under the test conditions of 25°C, 0.2 C rate, 3.0 V charge cut-off voltage, and 0 V discharge cut-off voltage.
[0110] The specific measurement method of the first-cycle charge capacity and the first-cycle discharge capacity is as follows: after the battery is charged to 3.0V at a rate of 0.2C, the charge capacity is divided by the amount of active material, which is the first-cycle charge capacity; then the battery is discharged to 0V at a rate of 0.2C, and the discharged capacity is divided by the amount of active material, which is the first-cycle discharge capacity.
[0111] The specific measurement method of the first-cycle coulomb efficiency is: first-cycle discharge specific capacity / first-cycle charge specific capacity.
[0112] 1C / 1C cycle life test: The sodium ion button half-cells prepared in the embodiment and the comparative example were respectively subjected to a 1C / 1C cycle test at 25°C (charge cut-off voltage 3.0V, discharge cut-off voltage 0V).
[0113] The specific measurement method of the discharge capacity after 200 cycles of 1C / 1C is as follows: after the battery has been cycled to 199 cycles, it is charged to 3.0V again and then discharged to 0V at a rate of 0.2C. The discharged capacity divided by the amount of active material is the discharge capacity at the 200th cycle.
[0114] The specific measurement method of the capacity retention rate of 1C / 1C cycle 200 cycles is: 200th cycle discharge specific capacity / first cycle discharge specific capacity.
[0115] The measurement method of the charge transfer resistance of the new battery is: use the Autolab electrochemical workstation to test the charge transfer resistance of the half-cell, and the test frequency is 0.01Hz~100kHz.
[0116] The specific measurement method of the rate discharge capacity of a half-cell is as follows: after the battery is charged to 3.0V, it is discharged to 0V at rates of 0.5C, 1C, 2C, and 5C respectively. The discharged capacity divided by the amount of active material is the discharge capacity at different rates.
[0117] Among them, the first charge and discharge capacity, coulomb efficiency, discharge capacity after 200 cycles of 1C / 1C and charge transfer resistance of the new battery of the half-cell are shown in Table 1. The rate discharge capacity of the half-cell is shown in Table 2.
[0118] Table 1
[0119]
[0120] Table 2
[0121]
[0122] It can be seen from the data in Table 1 and Table 2 that the negative electrode composite material prepared by the present invention is used for the negative electrode of a sodium ion battery, and the conductivity, electron transfer rate and ion diffusion rate are significantly improved, and it has lower charging internal resistance and discharge internal resistance, and exhibits better rate performance and cycle performance.
[0123] also, Figure 1 This is a scanning electron microscope image of the negative electrode composite material prepared in Example 1. Figure 1 It can be seen that the negative electrode composite material prepared in Example 1 has a flower ball-like structure formed by stacking a number of sheet structures.
[0124] Specifically, it can be seen from Table 1 and Table 2 that the negative electrode composite materials prepared in Examples 1 to 5 are applied to sodium ion button half-cells, and the first charge and discharge capacity, the first cycle coulomb efficiency, the discharge specific capacity at different rates, and the discharge specific capacity after 200 cycles of 1C / 1C are significantly improved, and the charge transfer resistance of the new battery is significantly reduced. By comparing Example 3, Example 4 and Example 5, it can be seen that the appropriate addition amount of galactose and sodium tetraborate pentahydrate helps to improve the first charge and discharge capacity, coulomb efficiency, the discharge specific capacity at different rates, and the discharge specific capacity after 200 cycles of 1C / 1C. During the preparation process of the negative electrode composite material of Comparative Example 1, no hexose and boron source were added, and carbonization was not performed, and the initial charge and discharge capacity, coulomb efficiency, discharge specific capacity at different rates, and discharge specific capacity after 200 cycles of 1C / 1C were significantly reduced, and the charge transfer resistance of the new battery was significantly improved; during the preparation process of the negative electrode composite material of Comparative Example 2, no boron source was added, and the initial charge and discharge capacity, coulomb efficiency, discharge specific capacity at different rates, and discharge specific capacity after 200 cycles of 1C / 1C were significantly reduced, and the charge transfer resistance of the new battery was improved to a certain extent.
[0125] Test Example 2
[0126] The negative electrode composite materials prepared in the examples and comparative examples were measured, wherein the specific surface area of the negative electrode composite material, the pore size of the flaky porous skeleton, and the porosity of the flaky porous skeleton were measured by nitrogen adsorption and desorption isothermal test, the average particle size of the negative electrode composite material, the sheet diameter of the flaky porous skeleton, and the sheet thickness of the flaky porous skeleton were calibrated by SEM images, and the molar ratio of boron element to carbon element in the flaky porous skeleton and the content of NiS particles (based on the total mass of the negative electrode composite material) were measured by energy dispersive X-ray spectrometer EDS. The test results are shown in Table 3.
[0127] Table 3
[0128]
[0129] It can be seen from the data in Table 3 that the lateral size of the negative electrode composite materials prepared in Examples 1 to 5 is 3.5 to 5 μm, and the specific surface area is 600 to 700 m 2 / g, the sheet diameter of the flaky porous skeleton is 1-1.5 μm, the thickness is 30-35 nm, the pore diameter is 10-20 nm, and the porosity is 20-30%. The negative electrode composite material prepared in this embodiment has a uniform nanoparticle distribution and a porous structure. Comparative Example 1 does not have an obvious flower ball structure due to the absence of hexose and boron source, and the specific surface area is significantly reduced.
[0130] Based on the data in Tables 1 to 3, the negative electrode materials prepared in the examples have lower charge transfer resistance, higher sodium ion diffusion capacity, and higher electrical performance. At the same time, due to the presence of an additional sodium source, the first-cycle coulomb efficiency is higher. Compared with Comparative Examples 1 and 2, the presence of boron-doped carbon materials in Examples 1 to 5 significantly reduces the charge transfer resistance and significantly increases the sodium ion diffusion coefficient, indicating that the electrochemical reaction kinetics is significantly improved, which is beneficial to the performance of electrical performance. Compared with Examples 1 to 4, the cycle performance and rate performance of Example 5 are significantly reduced, indicating that the amount of boron doping is too small, and the improvement of the electrical performance of the battery is limited.
[0131] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a negative electrode composite material, characterized in that: The method comprises the following steps: S1, adding nickel salt, complexing agent, hexose and boron source into a solvent for mixing to obtain a first material; performing hydrothermal treatment on the first material to obtain a second material; S2, centrifuging the second material, collecting the precipitate, washing it, and drying it to obtain a precursor; S3, carbonizing the precursor to obtain a carbonized precursor; mixing the carbonized precursor with sulfur powder and performing a sulfurization treatment; The molar ratio of the nickel salt, the complexing agent, the hexose and the boron source is 1:3-7:1-4:0.1-1.
5.
2. The preparation method according to claim 1, characterized in that: The nickel salt is selected from at least one of nickel nitrate, nickel sulfate, nickel chloride and nickel acetate; and / or, the complexing agent is at least one selected from nitrilotriacetic acid, ethylenediaminetetraacetic acid, hexamethylenetetramine, diisopropyltetramine and tetrahydroxypropylethylenediamine; And / or, the hexose is selected from at least one of glucose, maltose, sucrose and galactose; And / or, the boron source is selected from at least one of sodium tetraborate decahydrate, sodium tetraborate pentahydrate and anhydrous sodium tetraborate; And / or, the solvent is water.
3. The preparation method according to claim 1 or 2, characterized in that: The mass ratio of the nickel salt to the solvent is 1:150-250; And / or, the carbonized precursor and the sulfur powder are mixed in a molar ratio of 1:1-5.
4. The preparation method according to claim 1, characterized in that: In step S1, the mixing process is magnetic stirring; the conditions of the magnetic stirring include: stirring time is 20-40 min, stirring speed is 200-400 r / min; and / or, the hydrothermal treatment is carried out in a polytetrafluoroethylene reactor; and / or, the conditions of the hydrothermal treatment include: a temperature of 160-200° C. and a time of 6-12 h; And / or, in step S2, the washing liquid used for washing is selected from anhydrous ethanol and / or water; And / or, the drying conditions include: temperature of 50-70°C and time of 18-36h; And / or, in step S3, the carbonization treatment and the sulfurization treatment are performed in a protective atmosphere; And / or, the carbonization treatment conditions include: carbonization temperature of 500-650° C., carbonization time of 1-3 h; And / or, the vulcanization treatment conditions include: the vulcanization temperature is 280-350° C., and the vulcanization time is 1-3 hours.
5. A negative electrode composite material, characterized in that: Prepared according to the preparation method according to any one of claims 1 to 4.
6. The negative electrode composite material according to claim 5, characterized in that: The negative electrode composite material has a flower ball-like structure formed by stacking a number of sheets; The sheet layer includes a sheet-like porous skeleton and NiS particles embedded in the sheet-like porous skeleton, wherein the sheet-like porous skeleton is a carbon material doped with boron atoms.
7. The negative electrode composite material according to claim 6, characterized in that: The average lateral size of the negative electrode composite material is 3-5 μm; And / or, the specific surface area of the negative electrode composite material is 400-800m 2 / g.
8. The negative electrode composite material according to claim 6, characterized in that: The sheet diameter of the sheet-like porous skeleton is 1-2 μm; And / or, the thickness of the lamellar porous skeleton is 30-40 nm; And / or, the pore size of the sheet-like porous skeleton is 10-30 nm; And / or, the porosity of the lamellar porous skeleton is 15-30%; And / or, in the flaky porous skeleton, the molar ratio of boron element to carbon element is 1:7-9.
9. The negative electrode composite material according to claim 6, characterized in that: The average particle size of the NiS particles is 10-30 nm; And / or, based on the total mass of the negative electrode composite material, the content of the NiS particles is 60-80wt%.
10. A negative electrode plate, characterized in that: The negative electrode plate comprises a current collector and a negative electrode composite material arranged on a surface of the current collector, wherein the negative electrode composite material comprises the negative electrode composite material according to any one of claims 5 to 9.
11. A battery, characterized in that: The battery comprises the negative electrode sheet according to claim 10.