A lithium metal negative electrode and its preparation method and application

By constructing a Ti electronic conductive network on the surface of the lithium metal negative electrode and suppressing the silicon sulfide solid electrolyte layer of lithium dendrites, the short circuit problem caused by the growth of lithium dendrites is solved, and the ratio and cycling performance of lithium batteries are improved.

CN118676374BActive Publication Date: 2024-11-19JIANGSU ZENIO NEW ENERGY BATTERY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411155004.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-19
Estimated Expiration
2044-08-21

AI Technical Summary

Technical Problem

Lithium metal negative electrodes are prone to lithium dendrites growth in solid-state batteries, resulting in short-circuit problems. The existing surface modification methods sacrifice current density and affect rate performance.

Method used

The first modification layer with Ti electronic conductive network and buffering effect is constructed on the surface of metal lithium, and a second modification layer with the inhibition of lithium dendrites and rapid lithium conduction effect is constructed on it to form a three-layer ion-electron-buffer mechanism protection. .

Benefits of technology

Effectively avoid the deposition of lithium at the interface between the solid electrolyte and the negative electrode, reduce the local stress value of the lithium metal negative electrode, improve the current density, and have high rate performance and excellent cycling performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118676374B_ABST
    Figure CN118676374B_ABST
Patent Text Reader

Abstract

The present invention relates to a lithium metal negative electrode and a preparation method and application thereof, wherein the lithium metal negative electrode comprises a substrate, a first modification layer and a second modification layer; at least one of the two sides of the substrate along the thickness direction comprises metallic lithium; the first modification layer is arranged on the surface of the metallic lithium, and the first modification layer comprises titanium and a Li-Ti-O compound; the second modification layer is arranged on a side of the first modification layer away from the substrate, and the second modification layer comprises silicon and a sulfide solid electrolyte. The above-mentioned lithium metal negative electrode can be prepared by steps such as coating, transfer printing, and in-situ reaction. The lithium metal negative electrode is used in a secondary battery, which can effectively inhibit the growth of lithium dendrites, promote the rapid migration of electrons and ions at the negative terminal, and buffer the expansion of lithium metal, so that the secondary battery has both high rate performance and long cycle life.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of batteries, and in particular to a lithium metal negative electrode and a preparation method and application thereof. Background Art

[0002] Solid-state batteries are one of the main ways for lithium-ion batteries to achieve an energy density of more than 500 Wh / kg, but they need to be used in conjunction with lithium metal negative electrodes. At present, sulfide solid-state batteries with lithium metal negative electrodes are very prone to short circuits. Lithium metal without any protective layer can only last for a few cycles before short circuits occur. The reason is that lithium metal will undergo severe expansion and contraction during the charge and discharge cycle, resulting in unstable interface contact. Those point contacts cause concentrated lithium deposition due to high overpotential, so lithium dendrites are very likely to grow.

[0003] At present, the solutions to the growth of lithium dendrites on lithium metal negative electrodes include the use of lithium alloy negative electrodes, three-dimensional current collectors, surface modification and other methods. Surface modification refers to covering the surface of lithium metal with a coating that inhibits the growth of lithium dendrites, eliminating the factors that cause the growth of lithium dendrites, and reducing the concentration of local lithium ion sites. Commonly used surface modification methods use polymer coatings or inorganic coatings, relying on mechanical strength to inhibit lithium dendrites from piercing the protective layer, but this method sacrifices current density and reduces the rate performance of the battery. Therefore, there is an urgent need for a method that can effectively eliminate the growth of lithium dendrites without affecting the rate performance of the battery. Summary of the invention

[0004] In order to solve the above problems, the present invention provides a lithium metal negative electrode, which constructs a first modified layer with a Ti electronic conductive network and a buffering effect on the surface of the metal lithium, and constructs a second modified layer with a lithium dendrite inhibition and a rapid lithium conduction effect on the first modified layer, thereby forming a metal lithium surface protected by an ion-electron-buffer three-layer mechanism. Under the synergistic effect of the first modified layer and the second modified layer, the deposition of lithium at the interface between the solid electrolyte and the negative electrode can be effectively avoided, and the deposition of lithium ions on the lithium metal side can be promoted, thereby reducing the local stress value of the lithium metal negative electrode and increasing the current density, so that the solid-state battery based on the lithium metal negative electrode has both high rate performance and excellent cycle performance.

[0005] Specifically, the following technical solutions are provided:

[0006] A first aspect of the present invention provides a lithium metal negative electrode, which comprises a substrate, a first modified layer and a second modified layer; at least one of the two sides of the substrate along the thickness direction comprises metallic lithium; the first modified layer is arranged on the surface of the metallic lithium, and the first modified layer comprises titanium and a Li-Ti-O compound; the second modified layer is arranged on a side of the first modified layer away from the substrate, and the second modified layer comprises silicon and a sulfide solid electrolyte.

[0007] Furthermore, the substrate is a metal strip, such as a lithium metal strip, a copper-lithium composite metal strip or a lithium alloy composite strip, wherein the lithium alloy composite strip includes but is not limited to a lithium aluminum alloy composite strip, a lithium magnesium alloy composite strip, a lithium tin alloy composite strip, etc.

[0008] Further, the thickness of the first modified layer is preferably 0.48-3 μm, for example, 0.5 μm, 1 μm, 1.5 μm, 2 μm, 2.5 μm, 3 μm, etc., including but not limited to the thickness values ​​listed above; the thickness of the second modified layer is preferably 1-5 μm, for example, 1 μm, 1.5 μm, 2 μm, 2.5 μm, 3 μm, 3.5 μm, 4 μm, 4.5 μm, 5 μm, etc., including but not limited to the thickness values ​​listed above.

[0009] Furthermore, the Li-Ti-O compound comprises lithium titanate Li4Ti5O 12 .

[0010] Furthermore, the first modification layer further comprises a first binder; preferably, the first binder is polyethylene oxide; more preferably, the molecular weight of the first binder is 100,000-800,000, and the mass percentage of the first binder in the first modification layer is 3%-10%.

[0011] Further, the particle size D50 of silicon in the second modified layer is preferably 500-5000 nm, for example, 500 nm, 1000 nm, 1500 nm, 2000 nm, 2500 nm, 3000 nm, 3500 nm, 4000 nm, 4500 nm, 5000 nm, etc., including but not limited to the particle size values ​​listed above; the particle size D50 of the sulfide solid electrolyte in the second modified layer is 500-8000 nm, for example, 500 nm, 1000 nm, 2000 nm, 3000 nm, 4000 nm, 5000 nm, 6000 nm, 7000 nm, 8000 nm, etc., including but not limited to the particle size values ​​listed above.

[0012] Furthermore, the sulfide solid electrolyte is preferably Li6PS5Cl and / or Li3PS4.

[0013] Furthermore, the mass ratio of silicon to sulfide solid electrolyte in the second modified layer is (0.2-2):1, such as 0.2:1, 0.5:1, 1:1, 1.5:1, 2:1, etc., including but not limited to the ratios listed above.

[0014] Furthermore, the second modified layer also contains a second binder; preferably, the second binder can be selected from one or more of nitrile rubber, styrene-butadiene rubber, SEBS, or other binders that do not react with lithium metal; more preferably, the molecular weight of the second binder is 3000-50000, and the mass percentage of the second binder in the second modified layer is 0.5%-4%.

[0015] A second aspect of the present invention provides a method for preparing a lithium metal negative electrode, comprising the following steps:

[0016] S1, coating a first slurry comprising titanium dioxide, a first binder and a first solvent on one surface of a first release film, and drying the slurry to form a first coating on the first release film;

[0017] coating a second slurry comprising silicon powder, a sulfide solid electrolyte, a second binder and a second solvent on one surface of the second release film, and drying the slurry to form a second coating on the second release film;

[0018] S2, transferring the first coating to the side of the substrate containing metallic lithium to form a first modified layer, and then transferring the second coating to the side of the first modified layer away from the substrate to form a second modified layer, thereby obtaining the lithium metal negative electrode.

[0019] Further, in S1, the particle size D50 of the titanium dioxide is preferably 100-3000 nm, for example, 100 nm, 500 nm, 1000 nm, 1500 nm, 2000 nm, 2500 nm, 3000 nm, etc., including but not limited to the particle size values ​​listed above.

[0020] Furthermore, in S1, the mass ratio of titanium dioxide to the first binder in the first slurry is preferably (10-30):1, including but not limited to 10:1, 15:1, 20:1, 25:1, 30:1, etc.

[0021] Furthermore, in S1, the first solvent is preferably one or more of acetonitrile, N-methylpyrrolidone, and N,N-dimethylformamide.

[0022] Furthermore, in S1, the second solvent is a non-polar solvent; preferably, the second solvent is toluene and / or xylene.

[0023] Furthermore, in S1, the drying temperature is preferably 60-80°C.

[0024] Further, in S2, the transfer method includes rolling, specifically: the first coating is transferred to the side of the substrate containing metallic lithium by a first rolling, to form a first modified layer, and then the second coating is transferred to the side of the first modified layer away from the substrate by a second rolling, to form a second modified layer, to obtain the lithium metal negative electrode; the pressure of the first rolling is preferably 5-50 MPa; the pressure of the second rolling is preferably 10-50 MPa.

[0025] A third aspect of the present invention provides a secondary battery, comprising a negative electrode plate, wherein the negative electrode plate is the lithium metal negative electrode described in the first aspect or the lithium metal negative electrode prepared by the preparation method described in the second aspect.

[0026] Compared with the prior art, the present invention has the following beneficial effects:

[0027] The present invention provides a lithium metal negative electrode. A first modification layer comprising Ti and a Li-Ti-O compound is constructed on the surface of a base metal lithium, and a second modification layer comprising silicon and a sulfide solid electrolyte is constructed on the first modification layer, so as to form a metal lithium surface protected by an ion-electron-buffer mechanism. The growth of lithium dendrites of the lithium battery negative electrode during the charge and discharge cycle can be effectively suppressed, and a lithium battery comprising the lithium metal negative electrode can obtain a higher rate performance, with an average coulombic efficiency of not less than 98.5% after 100 cycles at 0.2 C, and a capacity retention rate of not less than 92.0% after 100 cycles.

[0028] The present invention also provides a method for preparing a lithium metal negative electrode, wherein a coating containing titanium dioxide and a coating containing silicon and a sulfide solid electrolyte are transferred to form a first modification layer and a second modification layer on the surface of a base metal lithium. The above-mentioned preparation method is simple to operate and easy to realize industrial production. In the above-mentioned preparation method, titanium dioxide and lithium can be used to contact and react with each other to prepare uniformly distributed titanium and Li-Ti-O compounds in situ on the surface of metal lithium. The substances in the first modification layer formed by this method are tightly bound, so that titanium can form an electronic conductive network in the first modification layer, promote the deposition of lithium ions on the lithium metal side, and at the same time, the formed Li-Ti-O compound (such as lithium titanate Li4Ti5O 12 ) Since the volume of embedded lithium hardly expands, the local stress value of the lithium metal negative electrode can be reduced by depositing the first modified layer with lithium ions to avoid the rupture of the SEI film, so that the first modified layer can serve as an electronic conductive layer and a buffer layer at the same time. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 Schematic diagram of the partial structure of the lithium metal negative electrode and the solid electrolyte layer, wherein 11 is the metal lithium surface, 12 is the first modified layer, 13 is the second modified layer, and 2 is the solid electrolyte layer. DETAILED DESCRIPTION

[0030] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which the present invention belongs. The terms used herein in the specification of the present invention are for the purpose of describing specific embodiments only and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items. The "include" or "comprising" described in the present invention means that in addition to the components described, other components may also be included or contained. The "include" or "comprising" described in the present invention may also be replaced by the closed "for" or "consisting of...".

[0031] As described in the background art, lithium metal batteries have a serious problem of lithium dendrite growth, and the existing method of suppressing lithium dendrites by surface modification of lithium metal negative electrodes has a significant impact on the battery rate.

[0032] To solve the above problems, an embodiment of the present invention provides a lithium metal negative electrode, comprising a substrate, a first modified layer and a second modified layer; wherein at least one of the two sides of the substrate along the thickness direction comprises metallic lithium; the first modified layer is arranged on the surface of the metallic lithium (the surface of the substrate where the metallic lithium is located), and the first modified layer comprises titanium and a Li-Ti-O compound; the second modified layer is arranged on a side of the first modified layer away from the substrate, and the second modified layer comprises silicon and a sulfide solid electrolyte.

[0033] In order to solve the problem that it is difficult to effectively suppress lithium dendrites without affecting the rate performance, the present invention proposes a new type of lithium metal negative electrode, which constructs a first modification layer including a Ti electronic conductive network and a Li-Ti-O buffer structure on the surface of the substrate lithium metal, and constructs a second modification layer including silicon that can suppress lithium dendrites and a sulfide solid electrolyte that is conducive to rapid lithium conduction on the first modification layer, thereby forming a lithium metal negative electrode with an ion-electron-buffer three-layer mechanism to protect the surface of the metal lithium. Among them: the electronic conductive network formed by titanium in the first modification layer can promote the deposition of lithium ions on the lithium metal side and reduce the growth of lithium dendrites at the interface; in addition, the first modification layer contains a Li-Ti-O compound (such as lithium titanate Li4Ti5O) that hardly expands in volume when lithium is inserted. 12 ), thereby forming a buffer structure, which can effectively reduce the local stress value of lithium metal and avoid SEI film rupture. At the same time, the second modified layer containing silicon and sulfide solid electrolyte constitutes a fast ion transmission channel, which can not only promote ion transmission and improve rate performance, but also the silicon in the second modified layer can dissolve the tiny lithium seeds grown on the surface of the second modified layer, further inhibiting the growth of lithium dendrites at the interface. Under the synergistic effect of the first modified layer and the second modified layer, the solid-state battery containing the lithium metal negative electrode can effectively inhibit the growth of lithium dendrites, and has both high rate performance and excellent cycle performance.

[0034] In the present invention, the substrate is a metal strip containing metallic lithium, such as a lithium metal strip, a copper-lithium composite metal strip, a lithium alloy composite strip, a lithium-aluminum alloy composite strip, a lithium-magnesium alloy composite strip, a lithium-tin alloy composite strip, etc. It may also be other metal strips containing metallic lithium or metal / non-metal composite strips.

[0035] In the present invention, the first modified layer mainly plays the role of conductivity and buffering, but the ion conductivity is relatively poor. If the layer is too thick, it will have a greater impact on the rate performance, but it should not be too thin. If the first modified layer is too thin, it will not be able to effectively inhibit the growth of interfacial lithium dendrites and buffer the expansion of lithium metal. Preferably, the thickness of the first modified layer is controlled in the range of 0.48-3 μm, for example, 0.5 μm, 1 μm, 1.5 μm, 2 μm, 2.5 μm, 3 μm, etc., including but not limited to the thickness values ​​listed above.

[0036] In the present invention, the second modified layer can inhibit the formation of interfacial lithium dendrites while serving as a fast lithium conducting layer, but the second modified layer cannot be too thick, as excessive thickness will affect the energy density of the battery. Preferably, the thickness of the second modified layer is controlled in the range of 1-5 μm, for example, 1 μm, 1.5 μm, 2 μm, 2.5 μm, 3 μm, 3.5 μm, 4 μm, 4.5 μm, 5 μm, etc., including but not limited to the thickness values ​​listed above.

[0037] In the present invention, the Li-Ti-O compound in the second modified layer comprises lithium titanate Li4Ti5O 12 , lithium titanate Li4Ti5O 12 The volume of embedded lithium hardly expands, and the second modified layer containing this substance has a buffering effect on lithium metal, which is beneficial to improving the cycle life of the battery.

[0038] In the present invention, the first modified layer also includes a first binder. In some preferred embodiments of the present invention, the first binder used in the first modified layer is polyethylene oxide. Since the molecular weight of the binder will affect the solubility and adhesion of the binder, and the content of the binder in the first modified layer will affect the film-forming property and conductivity of the first modified layer, it is more preferred that the molecular weight of the first binder is controlled within the range of 100,000-800,000, and the mass percentage of the first binder in the first modified layer is controlled within the range of 3%-10%.

[0039] In the present invention, the second modified layer contains silicon and sulfide solid electrolyte particles. In order to effectively dissolve lithium dendrites and form a lithium ion fast channel that can promote efficient lithium ion transmission, the content of silicon and sulfide solid electrolyte particles in the second modified layer needs to be controlled. If the silicon content in the second modified layer is too high, although it is beneficial to dissolve lithium dendrites, the negative electrode has poor ionic conductivity (relatively low content of sulfide solid electrolyte), which affects the rate performance of the battery; if the silicon content is too low, the lithium dendrites on the negative electrode surface cannot be effectively dissolved. Preferably, the mass ratio of silicon to sulfide solid electrolyte in the second modified layer is controlled in the range of (0.2-2): 1, such as 0.2: 1, 0.5: 1, 1: 1, 1.5: 1, 2: 1, etc., including but not limited to the ratios listed above.

[0040] In addition, the particle size of silicon in the second modified layer cannot be too large or too small. If the particle size is too large, the number of silicon particles at a certain content will be small, and it will be easy to distribute unevenly in the second modified layer, and lithium dendrites cannot be effectively dissolved. If the particle size is too small, small silicon particles will be coated on the surface of the sulfide solid electrolyte particles, blocking the rapid transmission channel of lithium ions and affecting the rate performance. Therefore, it is necessary to control the particle size of silicon and sulfide solid electrolyte particles in the second modified layer within a suitable range. Preferably, the particle size D50 of silicon in the second modified layer is controlled within a range of 500-5000 nm, for example, 500 nm, 1000 nm, 1500 nm, 2000 nm, 2500 nm, 3000 nm, 3500 nm, 4000 nm, 4500 nm, 5000 nm, etc., including but not limited to the particle size values ​​listed above; the particle size D50 of the sulfide solid electrolyte in the second modified layer is controlled within a range of 500-8000 nm, for example, 500 nm, 1000 nm, 2000 nm, 3000 nm, 4000 nm, 5000 nm, 6000 nm, 7000 nm, 8000 nm, etc., including but not limited to the particle size values ​​listed above.

[0041] In the present invention, the second modified layer preferably contains a sulfide solid electrolyte with high ionic conductivity and good stability to avoid reaction with other substances, such as Li6PS5Cl and / or Li3PS4.

[0042] In the present invention, the second modified layer further comprises a second binder, which may be selected from one or more of nitrile rubber, styrene-butadiene rubber, and SEBS, or other binders that do not react with lithium metal; more preferably, the molecular weight of the second binder is 3000-50000, and the mass percentage of the second binder in the second modified layer is 0.5%-4%. The molecular weight of the second binder and the mass percentage in the second modified layer are controlled within the above range to ensure the bonding force while improving the processability, and to enable the second modified layer to have good film-forming properties while maintaining a relatively high ionic conductivity.

[0043] The embodiment of the present invention also provides a method for preparing the above-mentioned lithium metal negative electrode. In addition to the following preparation method provided by the present invention, other methods can also be used to prepare the above-mentioned lithium metal negative electrode; the preparation method provided by the present invention comprises the following steps:

[0044] S1, coating a first slurry comprising titanium dioxide, a first binder and a first solvent on one surface of a first release film, and drying the slurry to form a first coating on the first release film;

[0045] coating a second slurry comprising silicon powder, a sulfide solid electrolyte, a second binder and a second solvent on one surface of the second release film, and drying the slurry to form a second coating on the second release film;

[0046] S2. Transfer the first coating on the first release film to the side of the substrate containing metallic lithium to form a first modified layer, and then transfer the second coating on the second release film to the side of the first modified layer away from the substrate to form a second modified layer to obtain the above-mentioned lithium metal negative electrode.

[0047] The present invention forms a first modification layer and a second modification layer on the surface of a base metal lithium by transfer printing of a coating containing titanium dioxide and a coating containing silicon and a sulfide solid electrolyte, and prepares uniformly distributed titanium and Li-Ti-O compounds in situ on the surface of the metal lithium by contact reaction between titanium dioxide and lithium. The substances in the first modification layer formed by the above method are tightly combined, so that titanium can form an electronic conductive network in the first modification layer, promotes the deposition of lithium ions on the lithium metal side, and reduces the growth of lithium dendrites at the negative electrode interface. At the same time, the formed Li-Ti-O compound has the characteristic of non-expansion when storing lithium, can effectively buffer the expansion of lithium metal, and reduce the local stress value of the lithium metal negative electrode, thereby effectively improving the cycle life of a lithium battery containing the lithium metal negative electrode.

[0048] In the present invention, the particle size of titanium dioxide will affect its reaction with lithium metal. Too large a particle size will lead to insufficient reaction between titanium dioxide and metallic lithium, and failure to form a connected titanium electron conductive network, affecting the conductivity of the first modified layer, and the product lithium titanate content is relatively small, which cannot effectively buffer the expansion of lithium metal. Preferably, the particle size D50 of titanium dioxide in S1 is controlled within the range of 100-3000 nm, for example, 100 nm, 500 nm, 1000 nm, 1500 nm, 2000 nm, 2500 nm, 3000 nm, etc., including but not limited to the particle size values ​​listed above.

[0049] In some preferred embodiments, the mass ratio of titanium dioxide to the first binder in the first slurry is preferably (10-30):1, including but not limited to 10:1, 15:1, 20:1, 25:1, 30:1, etc.

[0050] In the present invention, the first solvent is preferably one or more of acetonitrile, N-methylpyrrolidone, and N,N-dimethylformamide; the second solvent is preferably a non-polar solvent, such as toluene, xylene, a toluene / xylene mixed solvent, and the like.

[0051] In the present invention, the drying temperature in S1 is preferably 60-80° C. to form a uniform and complete coating, and to avoid excessively high temperatures during the drying process, which may cause the binder to melt and flow, and the uniformity and integrity of the formed coating may be affected by the surface tension.

[0052] In the present invention, in S2, the transfer can be performed by rolling, specifically: the first coating on the first release film is transferred to the side of the substrate containing metallic lithium by a first rolling press to form a first modified layer, and then the second coating on the second release film is transferred to the side of the first modified layer away from the substrate by a second rolling press to form a second modified layer, thereby obtaining a lithium metal negative electrode; preferably, the pressure of the first rolling press is preferably 5-50 MPa, and the pressure of the second rolling press is preferably 10-50 MPa.

[0053] The present invention further provides a lithium secondary battery in the embodiment part, comprising a lithium metal negative electrode prepared by the above preparation method, and the lithium secondary battery exhibits excellent rate performance and cycle stability.

[0054] The present invention is further described below in conjunction with specific embodiments so that those skilled in the art can better understand the present invention and implement it, but the embodiments are not intended to limit the present invention. Example 1

[0055] This embodiment relates to the preparation of a Li-30Ti-0.2Si-S composite film and a lithium ion battery used as a lithium metal negative electrode, and the specific operations are as follows:

[0056] (1) TiO2 powder (particle size D50 is 100 nm) and PEO (molecular weight is 100,000) are placed in a stirring tank at a weight ratio of 30:1. The total weight of TiO2 and PEO is 10 g. 30 mL of anhydrous acetonitrile is added as a solvent and stirred into a uniform slurry by mechanical stirring. The prepared slurry is coated on a PET release film with a 50 μm coating gap width using a doctor coater and dried at 60 °C to form a TiO2 dry film. The dry film thickness is measured by a spiral micrometer and is 0.48 μm;

[0057] Silicon powder (particle size of 500 nm) and lithium phosphorus sulfur chlorine solid electrolyte powder (LPSC powder, particle size of 500 nm) were mixed in a weight ratio of 0.2:1, and then nitrile rubber (molecular weight of 3000) was added. The total weight of silicon powder, LPSC and nitrile rubber was 3 g, and the content of nitrile rubber was 0.5%. Then 10 mL of xylene was added as a solvent and stirred into a uniform slurry by mechanical stirring. The prepared slurry was coated on a PET release film with a coating gap width of 50 μm using a doctor coater, and the Si-SE dry film was dried at 60 °C. The dry film thickness was measured with a spiral micrometer to be 1.03 μm.

[0058] (2) The coating surface of the TiO2 dry film prepared in step (1) is laminated to the lithium surface of the copper-lithium composite tape and rolled at a pressure of 5 MPa and a speed of 0.3 m / min to transfer the TiO2 dry film to the lithium foil side of the copper-lithium composite tape. The PET release film is peeled off to obtain a Li-TiO2 composite film.

[0059] The coating surface of the Si-SE dry film prepared in step (1) was laminated with the TiO2 dry film surface of the Li-TiO2 composite film and rolled at a pressure of 10 MPa to transfer the Si-SE composite film to the surface of the Li-TiO2 composite film. The PET release film was peeled off to obtain a Li-30Ti-0.2Si-S composite film.

[0060] Preparation of lithium-ion batteries:

[0061] Negative electrode sheet: The Li-30Ti-0.2Si-S composite film is cut into 4×6 cm electrodes with tabs by a die cutter as the negative electrode sheet;

[0062] Positive electrode: Vapor-grown conductive carbon fiber (VGCF) was used as the conductive agent, hydrogenated nitrile rubber (HNBR) was used as the binder, and the mixture was placed in a covered glass bottle with a mass ratio of NCM811:LPSC:VGCF:HNBR=80:17:1:2. Xylene was added to a solid content of 70%. The mixture was stirred at 500 rpm for 12 h at room temperature to form a uniform slurry. The slurry was then coated on aluminum foil with a coating machine. The coating slit width was adjusted to 200 μm. After drying, the active material loading was 16 mg / cm 2 The positive electrode.

[0063] Electrolyte layer: LPSC and HNBR were mixed in a mass ratio of 99:1 and placed in a covered glass bottle. Xylene was added until the solid content was 60%. The mixture was stirred at 500 rpm for 12 h at room temperature to form a uniform slurry. The slurry was then coated on a PET release film using a coater and dried in a vacuum oven at 80 °C for 10 h to obtain a sulfide electrolyte membrane. The dry film thickness was measured by a spiral micrometer to be 35 μm.

[0064] They are assembled into solid-state batteries by laminating the positive electrode sheet with the material area and the electrolyte layer on the PET release film to form a laminated film. The roller gap width of the roller press is adjusted to 70% of the thickness of the laminated film. The laminated film is then rolled and the electrolyte layer is transferred to the positive electrode sheet. The PET release film is then peeled off to obtain a positive-electrolyte composite film. The composite film is then cut into films of the same size and shape as the negative electrode sheet using a die-cutting machine. The composite film is then laminated with the negative electrode sheet loading material surface. The tabs are then welded and the battery is vacuum-sealed with an aluminum-plastic film in the conventional manner in the industry, but there is no need to leave an air bag. The assembled battery is tested under conventional pressure fixtures in the industry. Example 2

[0065] This embodiment relates to the preparation of a Li-30Ti-2Si-S composite film and a lithium ion battery used as a lithium metal negative electrode, and the specific operations are as follows:

[0066] (1) TiO2 powder (particle size D50 is 3000 nm) and PEO (molecular weight is 800,000) are placed in a stirring tank at a weight ratio of 30:1. The total weight of TiO2 and PEO is 10 g. 30 mL of anhydrous acetonitrile is added as solvent and stirred into a uniform slurry by mechanical stirring. The prepared slurry is coated on a PET release film with a 50 μm coating gap width using a doctor coater and dried at 80 °C to form a TiO2 dry film. The dry film thickness is measured by a spiral micrometer and is 2.95 μm;

[0067] Silica powder (particle size of 5000 nm) and LPSC powder (particle size of 8000 nm) were mixed in a weight ratio of 2:1, and then nitrile rubber (molecular weight of 25000) was added. The total weight of silica powder, LPSC and nitrile rubber was 3 g, and the content of nitrile rubber was 1%. Then 10 mL of xylene was added as a solvent and stirred into a uniform slurry by mechanical stirring. The prepared slurry was coated on a PET release film with a 50 μm coating gap width using a doctor coater, and the Si-SE dry film was dried at 80 °C. The dry film thickness was measured with a spiral micrometer to be 4.90 μm.

[0068] (2) The coating surface of the TiO2 dry film prepared in step (1) is laminated to the lithium surface of the copper-lithium composite tape and rolled at a pressure of 50 MPa and a speed of 0.3 m / min to transfer the TiO2 dry film to the lithium foil side of the copper-lithium composite tape, and the PET release film is peeled off to obtain a Li-TiO2 composite film.

[0069] The coating surface of the Si-SE dry film prepared in step (1) was laminated with the TiO2 dry film surface of the Li-TiO2 composite film and rolled at a pressure of 50 MPa to transfer the Si-SE composite film to the surface of the Li-TiO2 composite film. The PET release film was peeled off to obtain a Li-30Ti-2Si-S composite film.

[0070] Preparation of lithium-ion batteries:

[0071] Negative electrode sheet: The Li-30Ti-2Si-S composite film is cut into 4×6 cm electrodes with tabs by a die-cutting machine as the negative electrode sheet;

[0072] Positive electrode: Vapor-grown conductive carbon fiber (VGCF) was used as the conductive agent, hydrogenated nitrile rubber (HNBR) was used as the binder, and the mixture was placed in a covered glass bottle with a mass ratio of NCM811:LPSC:VGCF:HNBR=80:17:1:2. Xylene was added to a solid content of 70%. The mixture was stirred at 500 rpm for 12 h at room temperature to form a uniform slurry. The slurry was then coated on aluminum foil with a coating machine, and the coating slit width was adjusted to 200 μm. After drying, the active material loading was 16 mg / cm 2 The positive electrode.

[0073] Electrolyte layer: LPSC and HNBR were mixed in a mass ratio of 99:1 and placed in a covered glass bottle. Xylene was added to a solid content of 60%. The mixture was stirred at 500 rpm for 12 h at room temperature to form a uniform slurry. The slurry was then coated on a PET release film with a coater and dried in a vacuum oven at 80 °C for 10 h to obtain a sulfide electrolyte membrane. The dry film thickness was measured to be 33 μm with a spiral micrometer.

[0074] They are assembled into solid-state batteries by laminating the positive electrode sheet with the material area and the electrolyte layer on the PET release film to form a laminated film. The roller gap width of the roller press is adjusted to 70% of the thickness of the laminated film. The laminated film is then rolled and the electrolyte layer is transferred to the positive electrode sheet. The PET release film is then peeled off to obtain a positive-electrolyte composite film. The composite film is then cut into films of the same size and shape as the negative electrode sheet using a die-cutting machine. The composite film is then laminated with the negative electrode sheet loading material surface. The tabs are then welded and the battery is vacuum-sealed with an aluminum-plastic film in the conventional manner in the industry, but there is no need to leave an air bag. The assembled battery is tested under conventional pressure fixtures in the industry. Example 3

[0075] This embodiment relates to the preparation of a Li-10Ti-1Si-S composite film and a lithium ion battery used as a lithium metal negative electrode, and the specific operations are as follows:

[0076] (1) TiO2 powder (particle size D50 is 1500 nm) and PEO (molecular weight is 400,000) are placed in a stirring tank at a weight ratio of 10:1. The total weight of TiO2 and PEO is 10 g. 30 mL of anhydrous acetonitrile is added as a solvent and stirred into a uniform slurry by mechanical stirring. The prepared slurry is coated on a PET release film with a 50 μm coating gap width using a doctor coater and dried at 70 °C to form a TiO2 dry film. The dry film thickness is measured by a spiral micrometer and is 1.29 μm;

[0077] Silica powder (particle size of 2500 nm) and LPSC powder (particle size of 4000 nm) were mixed in a weight ratio of 1:1, and then nitrile rubber (molecular weight of 5000) was added. The total weight of silica powder, LPSC and nitrile rubber was 3 g, and the content of nitrile rubber was 1.5%. Then 10 mL of xylene was added as a solvent and stirred into a uniform slurry by mechanical stirring. The prepared slurry was coated on a PET release film with a doctor coater with a slit width of 50 μm, and the Si-SE dry film was dried at 70 °C. The dry film thickness was measured with a spiral micrometer and was 3.15 μm.

[0078] (2) The coating surface of the TiO2 dry film prepared in step (1) is laminated to the lithium surface of the copper-lithium composite tape and rolled at a pressure of 25 MPa and a speed of 0.3 m / min to transfer the TiO2 dry film to the lithium foil side of the copper-lithium composite tape. The PET release film is peeled off to obtain a Li-TiO2 composite film.

[0079] The coating surface of the Si-SE dry film prepared in step (1) was laminated with the TiO2 dry film surface of the Li-TiO2 composite film and rolled at a pressure of 30 MPa to transfer the Si-SE composite film to the surface of the Li-TiO2 composite film. The PET release film was peeled off to obtain a Li-10Ti-1Si-S composite film.

[0080] Preparation of lithium-ion batteries:

[0081] Negative electrode sheet: The Li-10Ti-1Si-S composite film is cut into 4×6 cm electrodes with tabs using a die-cutting machine as the negative electrode sheet;

[0082] Positive electrode: Vapor-grown conductive carbon fiber (VGCF) was used as the conductive agent, hydrogenated nitrile rubber (HNBR) was used as the binder, and the mixture was placed in a covered glass bottle with a mass ratio of NCM811:LPSC:VGCF:HNBR=80:17:1:2. Xylene was added to a solid content of 70%. The mixture was stirred at 500 rpm for 12 h at room temperature to form a uniform slurry. The slurry was then coated on aluminum foil with a coating machine, and the coating slit width was adjusted to 200 μm. After drying, the active material loading was 16 mg / cm 2 The positive electrode.

[0083] Electrolyte layer: LPSC and HNBR were mixed in a mass ratio of 99:1 and placed in a covered glass bottle. Xylene was added to a solid content of 60%. The mixture was stirred at 500 rpm for 12 h at room temperature to form a uniform slurry. The slurry was then coated on a PET release film with a coater and dried in a vacuum oven at 80 °C for 10 h to obtain a sulfide electrolyte membrane. The dry film thickness was measured to be 34 μm with a spiral micrometer.

[0084] They are assembled into solid-state batteries by laminating the positive electrode sheet with the material area and the electrolyte layer on the PET release film to form a laminated film. The roller gap width of the roller press is adjusted to 70% of the thickness of the laminated film. The laminated film is then rolled and the electrolyte layer is transferred to the positive electrode sheet. The PET release film is then peeled off to obtain a positive-electrolyte composite film. The composite film is then cut into films of the same size and shape as the negative electrode sheet using a die-cutting machine. The composite film is then laminated with the negative electrode sheet loading material surface. The tabs are then welded and the battery is vacuum-sealed with an aluminum-plastic film in the conventional manner in the industry, but there is no need to leave an air bag. The assembled battery is tested under conventional pressure fixtures in the industry. Example 4

[0085] This embodiment relates to the preparation of a Li-15Ti-0.5Si-S composite film and a lithium ion battery used as a lithium metal negative electrode, and the specific operations are as follows:

[0086] (1) TiO2 powder (particle size D50 is 500 nm) and PEO (molecular weight is 200,000) are placed in a stirring tank at a weight ratio of 15:1. The total weight of TiO2 and PEO is 10 g. 30 mL of anhydrous acetonitrile is added as a solvent and stirred into a uniform slurry by mechanical stirring. The prepared slurry is coated on a PET release film with a 50 μm coating gap width using a doctor coater and dried at 70 °C to form a TiO2 dry film. The dry film thickness is measured by a spiral micrometer to be 0.55 μm.

[0087] Silica powder (particle size of 1000 nm) and LPSC powder (particle size of 1000 nm) were mixed in a weight ratio of 0.5:1, and then nitrile rubber (molecular weight of 10000) was added. The total weight of silica powder, LPSC and nitrile rubber was 3 g, and the content of nitrile rubber was 2%. Then 10 mL of xylene was added as a solvent and stirred into a uniform slurry by mechanical stirring. The prepared slurry was coated on a PET release film with a coating device with a slit width of 50 μm, and the Si-SE dry film was dried at 70 °C. The dry film thickness was measured with a spiral micrometer and was 1.43 μm.

[0088] (2) The coating surface of the TiO2 dry film prepared in step (1) is laminated to the lithium surface of the copper-lithium composite tape and rolled at a pressure of 10 MPa and a speed of 0.3 m / min to transfer the TiO2 dry film to the lithium foil side of the copper-lithium composite tape. The PET release film is peeled off to obtain a Li-TiO2 composite film.

[0089] The coating surface of the Si-SE dry film prepared in step (1) was laminated with the TiO2 dry film surface of the Li-TiO2 composite film and rolled at a pressure of 20 MPa to transfer the Si-SE composite film to the surface of the Li-TiO2 composite film. The PET release film was peeled off to obtain a Li-15Ti-0.5Si-S composite film.

[0090] Preparation of lithium-ion batteries:

[0091] Negative electrode sheet: The Li-15Ti-0.5Si-S composite film is cut into 4×6 cm electrodes with tabs using a die-cutting machine as the negative electrode sheet;

[0092] Positive electrode: Vapor-grown conductive carbon fiber (VGCF) was used as the conductive agent, hydrogenated nitrile rubber (HNBR) was used as the binder, and the mixture was placed in a covered glass bottle with a mass ratio of NCM811:LPSC:VGCF:HNBR=80:17:1:2. Xylene was added to a solid content of 70%. The mixture was stirred at 500 rpm for 12 h at room temperature to form a uniform slurry. The slurry was then coated on aluminum foil with a coating machine, and the coating slit width was adjusted to 200 μm. After drying, the active material loading was 16 mg / cm 2 The positive electrode.

[0093] Electrolyte layer: LPSC and HNBR were mixed in a mass ratio of 99:1 and placed in a covered glass bottle. Xylene was added to a solid content of 60%. The mixture was stirred at 500 rpm for 12 h at room temperature to form a uniform slurry. The slurry was then coated on a PET release film using a coater and dried in a vacuum oven at 80 °C for 10 h to obtain a sulfide electrolyte membrane. The dry film thickness was measured to be 35 μm using a spiral micrometer.

[0094] They are assembled into solid-state batteries by laminating the positive electrode sheet with the material area and the electrolyte layer on the PET release film to form a laminated film. The roller gap width of the roller press is adjusted to 70% of the thickness of the laminated film. The laminated film is then rolled and the electrolyte layer is transferred to the positive electrode sheet. The PET release film is then peeled off to obtain a positive-electrolyte composite film. The composite film is then cut into films of the same size and shape as the negative electrode sheet using a die-cutting machine. The composite film is then laminated with the negative electrode sheet loading material surface. The tabs are then welded and the battery is vacuum-sealed with an aluminum-plastic film in the conventional manner in the industry, but there is no need to leave an air bag. The assembled battery is tested under conventional pressure fixtures in the industry. Example 5

[0095] This embodiment relates to the preparation of a Li-20Ti-1.5Si-S composite film and a lithium ion battery used as a lithium metal negative electrode, and the specific operations are as follows:

[0096] (1) TiO2 powder (particle size D50 is 1000 nm) and PEO (molecular weight is 600,000) are placed in a stirring tank at a weight ratio of 20:1. The total weight of TiO2 and PEO is 10 g. 30 mL of anhydrous acetonitrile is added as a solvent and stirred into a uniform slurry by mechanical stirring. The prepared slurry is coated on a PET release film with a 50 μm coating gap width using a doctor coater and dried at 70 °C to form a TiO2 dry film. The dry film thickness is measured by a spiral micrometer and is 0.85 μm;

[0097] Silica powder (particle size of 1500 nm) and LPSC powder (particle size of 2000 nm) were mixed in a weight ratio of 1.5:1, and then nitrile rubber (molecular weight of 15000) was added. The total weight of silica powder, LPSC and nitrile rubber was 3 g, and the content of nitrile rubber was 2.5%. Then 10 mL of xylene was added as a solvent and stirred into a uniform slurry by mechanical stirring. The prepared slurry was coated on a PET release film with a doctor coater with a slit width of 50 μm, and the Si-SE dry film was dried at 70 °C. The dry film thickness was measured with a spiral micrometer and was 1.88 μm.

[0098] (2) The coating surface of the TiO2 dry film prepared in step (1) is laminated to the lithium surface of the copper-lithium composite tape and rolled at a pressure of 15 MPa and a speed of 0.3 m / min to transfer the TiO2 dry film to the lithium foil side of the copper-lithium composite tape, and the PET release film is peeled off to obtain a Li-TiO2 composite film.

[0099] The coating surface of the Si-SE dry film prepared in step (1) was laminated with the TiO2 dry film surface of the Li-TiO2 composite film and rolled at a pressure of 40 MPa to transfer the Si-SE composite film to the surface of the Li-TiO2 composite film. The PET release film was peeled off to obtain a Li-20Ti-1.5Si-S composite film.

[0100] Preparation of lithium-ion batteries:

[0101] Negative electrode sheet: The Li-20Ti-1.5Si-S composite film is cut into 4×6 cm electrodes with tabs using a die-cutting machine as the negative electrode sheet;

[0102] Positive electrode: Vapor-grown conductive carbon fiber (VGCF) was used as the conductive agent, hydrogenated nitrile rubber (HNBR) was used as the binder, and the mixture was placed in a covered glass bottle with a mass ratio of NCM811:LPSC:VGCF:HNBR=80:17:1:2. Xylene was added to a solid content of 70%. The mixture was stirred at 500 rpm for 12 h at room temperature to form a uniform slurry. The slurry was then coated on aluminum foil with a coating machine, and the coating slit width was adjusted to 200 μm. After drying, the active material loading was 16 mg / cm 2 The positive electrode.

[0103] Electrolyte layer: LPSC and HNBR were mixed in a mass ratio of 99:1 and placed in a covered glass bottle. Xylene was added to a solid content of 60%. The mixture was stirred at 500 rpm for 12 h at room temperature to form a uniform slurry. The slurry was then coated on a PET release film with a coater and dried in a vacuum oven at 80 °C for 10 h to obtain a sulfide electrolyte membrane. The dry film thickness was measured to be 36 μm with a spiral micrometer.

[0104] They are assembled into solid-state batteries by laminating the positive electrode sheet with the material area and the electrolyte layer on the PET release film to form a laminated film. The roller gap width of the roller press is adjusted to 70% of the thickness of the laminated film. The laminated film is then rolled and the electrolyte layer is transferred to the positive electrode sheet. The PET release film is then peeled off to obtain a positive-electrolyte composite film. The composite film is then cut into films of the same size and shape as the negative electrode sheet using a die-cutting machine. The composite film is then laminated with the negative electrode sheet loading material surface. The tabs are then welded and the battery is vacuum-sealed with an aluminum-plastic film in the conventional manner in the industry, but there is no need to leave an air bag. The assembled battery is tested under conventional pressure fixtures in the industry. Example 6

[0105] This embodiment relates to the preparation of a Li-25Ti-1Si-S composite film and a lithium ion battery used as a lithium metal negative electrode, and the specific operations are as follows:

[0106] (1) TiO2 powder (particle size D50 is 2000 nm) and PEO (molecular weight is 500,000) are placed in a stirring tank at a weight ratio of 25:1. The total weight of TiO2 and PEO is 10 g. 30 mL of anhydrous acetonitrile is added as solvent and stirred into a uniform slurry by mechanical stirring. The prepared slurry is coated on a PET release film with a 50 μm coating gap width using a doctor coater and dried at 70 °C to form a TiO2 dry film. The dry film thickness is measured by a spiral micrometer and is 2.01 μm;

[0107] Silica powder (particle size of 2000 nm) and LPSC powder (particle size of 3000 nm) were mixed in a weight ratio of 1:1, and then nitrile rubber (molecular weight of 20000) was added. The total weight of silica powder, LPSC and nitrile rubber was 3 g, and the content of nitrile rubber was 3%. Then 10 mL of xylene was added as a solvent and stirred into a uniform slurry by mechanical stirring. The prepared slurry was coated on a PET release film with a doctor coater with a coating gap width of 50 μm, and the Si-SE dry film was dried at 70 °C. The dry film thickness was measured with a spiral micrometer to be 2.45 μm.

[0108] (2) The coating surface of the TiO2 dry film prepared in step (1) is laminated with the lithium surface of the copper-lithium composite tape and rolled at a pressure of 20 MPa and a speed of 0.3 m / min to transfer the TiO2 dry film to the lithium foil side of the copper-lithium composite tape, and the PET release film is peeled off to obtain a Li-TiO2 composite film.

[0109] The coating surface of the Si-SE dry film prepared in step (1) was laminated with the TiO2 dry film surface of the Li-TiO2 composite film and rolled at a pressure of 20 MPa to transfer the Si-SE composite film to the surface of the Li-TiO2 composite film. The PET release film was peeled off to obtain a Li-25Ti-1Si-S composite film.

[0110] Preparation of lithium-ion batteries:

[0111] Negative electrode sheet: The Li-25Ti-1Si-S composite film is cut into 4×6 cm electrodes with tabs by a die-cutting machine as the negative electrode sheet;

[0112] Positive electrode: Vapor-grown conductive carbon fiber (VGCF) was used as the conductive agent, hydrogenated nitrile rubber (HNBR) was used as the binder, and the mixture was placed in a covered glass bottle with a mass ratio of NCM811:LPSC:VGCF:HNBR=80:17:1:2. Xylene was added to a solid content of 70%. The mixture was stirred at 500 rpm for 12 h at room temperature to form a uniform slurry. The slurry was then coated on aluminum foil with a coating machine, and the coating slit width was adjusted to 200 μm. After drying, the active material loading was 16 mg / cm 2 The positive electrode.

[0113] Electrolyte layer: LPSC and HNBR were mixed in a mass ratio of 99:1 and placed in a covered glass bottle. Xylene was added to a solid content of 60%. The mixture was stirred at 500 rpm for 12 h at room temperature to form a uniform slurry. The slurry was then coated on a PET release film with a coater and dried in a vacuum oven at 80 °C for 10 h to obtain a sulfide electrolyte membrane. The dry film thickness was measured to be 34 μm with a spiral micrometer.

[0114] They are assembled into solid-state batteries by laminating the positive electrode sheet with the material area and the electrolyte layer on the PET release film to form a laminated film. The roller gap width of the roller press is adjusted to 70% of the thickness of the laminated film. The laminated film is then rolled and the electrolyte layer is transferred to the positive electrode sheet. The PET release film is then peeled off to obtain a positive-electrolyte composite film. The composite film is then cut into films of the same size and shape as the negative electrode sheet using a die-cutting machine. The composite film is then laminated with the negative electrode sheet loading material surface. The tabs are then welded and the battery is vacuum-sealed with an aluminum-plastic film in the conventional manner in the industry, but there is no need to leave an air bag. The assembled battery is tested under conventional pressure fixtures in the industry. Example 7

[0115] This embodiment relates to the preparation of a Li-20Ti-1Si-S composite film and a lithium ion battery used as a lithium metal negative electrode, and the specific operations are as follows:

[0116] (1) TiO2 powder (particle size D50 is 1500 nm) and PEO (molecular weight is 500,000) are placed in a stirring tank at a weight ratio of 20:1. The total weight of TiO2 and PEO is 10 g. 30 mL of anhydrous acetonitrile is added as solvent and stirred into a uniform slurry by mechanical stirring. The prepared slurry is coated on a PET release film with a 50 μm coating gap width using a doctor coater and dried at 70 °C to form a TiO2 dry film. The dry film thickness is measured by a spiral micrometer and is 1.27 μm;

[0117] Silica powder (particle size of 3000 nm) and LPSC powder (particle size of 5000 nm) were mixed in a weight ratio of 1:1, and then nitrile rubber (molecular weight of 30000) was added. The total weight of silica powder, LPSC and nitrile rubber was 3 g, and the content of nitrile rubber was 3.5%. Then 10 mL of xylene was added as a solvent and stirred into a uniform slurry by mechanical stirring. The prepared slurry was coated on a PET release film with a doctor coater with a coating gap width of 50 μm, and the Si-SE dry film was dried at 70 ℃. The dry film thickness was measured by a spiral micrometer and was 3.81 μm.

[0118] (2) The coating surface of the TiO2 dry film prepared in step (1) is laminated to the lithium surface of the copper-lithium composite tape and rolled at a pressure of 30 MPa and a speed of 0.3 m / min to transfer the TiO2 dry film to the lithium foil side of the copper-lithium composite tape. The PET release film is peeled off to obtain a Li-TiO2 composite film.

[0119] The coating surface of the Si-SE dry film prepared in step (1) was laminated with the TiO2 dry film surface of the Li-TiO2 composite film and rolled at a pressure of 30 MPa to transfer the Si-SE composite film to the surface of the Li-TiO2 composite film. The PET release film was peeled off to obtain a Li-20Ti-1Si-S composite film.

[0120] Preparation of lithium-ion batteries:

[0121] Negative electrode sheet: The Li-20Ti-1Si-S composite film is cut into 4×6 cm electrodes with tabs using a die-cutting machine as the negative electrode sheet;

[0122] Positive electrode: Vapor-grown conductive carbon fiber (VGCF) was used as the conductive agent, hydrogenated nitrile rubber (HNBR) was used as the binder, and the mixture was placed in a covered glass bottle with a mass ratio of NCM811:LPSC:VGCF:HNBR=80:17:1:2. Xylene was added to a solid content of 70%. The mixture was stirred at 500 rpm for 12 h at room temperature to form a uniform slurry. The slurry was then coated on aluminum foil with a coating machine, and the coating slit width was adjusted to 200 μm. After drying, the active material loading was 16 mg / cm 2 The positive electrode.

[0123] Electrolyte layer: LPSC and HNBR were mixed in a mass ratio of 99:1 and placed in a covered glass bottle. Xylene was added to a solid content of 60%. The mixture was stirred at 500 rpm for 12 h at room temperature to form a uniform slurry. The slurry was then coated on a PET release film using a coater and dried in a vacuum oven at 80 °C for 10 h to obtain a sulfide electrolyte membrane. The dry film thickness was measured to be 35 μm using a spiral micrometer.

[0124] They are assembled into solid-state batteries by laminating the positive electrode sheet with the material area and the electrolyte layer on the PET release film to form a laminated film. The roller gap width of the roller press is adjusted to 70% of the thickness of the laminated film. The laminated film is then rolled and the electrolyte layer is transferred to the positive electrode sheet. The PET release film is then peeled off to obtain a positive-electrolyte composite film. The composite film is then cut into films of the same size and shape as the negative electrode sheet using a die-cutting machine. The composite film is then laminated with the negative electrode sheet loading material surface. The tabs are then welded and the battery is vacuum-sealed with an aluminum-plastic film in the conventional manner in the industry, but there is no need to leave an air bag. The assembled battery is tested under conventional pressure fixtures in the industry. Example 8

[0125] This embodiment relates to the preparation of a Li-20Ti-1Si-S composite film and a lithium ion battery used as a lithium metal negative electrode, and the specific operations are as follows:

[0126] (1) TiO2 powder (particle size D50 is 1500 nm) and PEO (molecular weight is 500,000) are placed in a stirring tank at a weight ratio of 20:1. The total weight of TiO2 and PEO is 10 g. 30 mL of anhydrous acetonitrile is added as a solvent and stirred into a uniform slurry by mechanical stirring. The prepared slurry is coated on a PET release film with a 50 μm coating gap width using a doctor coater and dried at 70 °C to form a TiO2 dry film. The dry film thickness is measured by a spiral micrometer and is 1.33 μm;

[0127] Silica powder (particle size of 4000 nm) and LPSC powder (particle size of 6000 nm) were mixed in a weight ratio of 1:1, and then nitrile rubber (molecular weight of 35000) was added. The total weight of silica powder, LPSC and nitrile rubber was 3 g, and the content of nitrile rubber was 4%. Then 10 mL of xylene was added as a solvent and stirred into a uniform slurry by mechanical stirring. The prepared slurry was coated on a PET release film with a doctor coater with a coating gap width of 50 μm, and the Si-SE dry film was dried at 70 °C. The dry film thickness was measured with a spiral micrometer to be 4.14 μm.

[0128] (2) The coating surface of the TiO2 dry film prepared in step (1) is laminated to the lithium surface of the copper-lithium composite tape and rolled at a pressure of 40 MPa and a speed of 0.3 m / min to transfer the TiO2 dry film to the lithium foil side of the copper-lithium composite tape, and the PET release film is peeled off to obtain a Li-TiO2 composite film.

[0129] The coating surface of the Si-SE dry film prepared in step (1) was laminated with the TiO2 dry film surface of the Li-TiO2 composite film and rolled at a pressure of 20 MPa to transfer the Si-SE composite film to the surface of the Li-TiO2 composite film. The PET release film was peeled off to obtain a Li-20Ti-1Si-S composite film.

[0130] Preparation of lithium-ion batteries:

[0131] Negative electrode sheet: The Li-20Ti-1Si-S composite film is cut into 4×6 cm electrodes with tabs using a die-cutting machine as the negative electrode sheet;

[0132] Positive electrode: Vapor-grown conductive carbon fiber (VGCF) was used as the conductive agent, hydrogenated nitrile rubber (HNBR) was used as the binder, and the mixture was placed in a covered glass bottle with a mass ratio of NCM811:LPSC:VGCF:HNBR=80:17:1:2. Xylene was added to a solid content of 70%. The mixture was stirred at 500 rpm for 12 h at room temperature to form a uniform slurry. The slurry was then coated on aluminum foil with a coating machine, and the coating slit width was adjusted to 200 μm. After drying, the active material loading was 16 mg / cm 2 The positive electrode.

[0133] Electrolyte layer: LPSC and HNBR were mixed in a mass ratio of 99:1 and placed in a covered glass bottle. Xylene was added to a solid content of 60%. The mixture was stirred at 500 rpm for 12 h at room temperature to form a uniform slurry. The slurry was then coated on a PET release film with a coater and dried in a vacuum oven at 80 °C for 10 h to obtain a sulfide electrolyte membrane. The dry film thickness was measured to be 37 μm with a spiral micrometer.

[0134] They are assembled into solid-state batteries by laminating the positive electrode sheet with the material area and the electrolyte layer on the PET release film to form a laminated film. The roller gap width of the roller press is adjusted to 70% of the thickness of the laminated film. The laminated film is then rolled and the electrolyte layer is transferred to the positive electrode sheet. The PET release film is then peeled off to obtain a positive-electrolyte composite film. The composite film is then cut into films of the same size and shape as the negative electrode sheet using a die-cutting machine. The composite film is then laminated with the negative electrode sheet loading material surface. The tabs are then welded and the battery is vacuum-sealed with an aluminum-plastic film in the conventional manner in the industry, but there is no need to leave an air bag. The assembled battery is tested under conventional pressure fixtures in the industry. Example 9

[0135] This embodiment relates to the preparation of a Li-20Ti-1Si-S composite film and a lithium ion battery used as a lithium metal negative electrode, and the specific operations are as follows:

[0136] (1) TiO2 powder (particle size D50 is 1500 nm) and PEO (molecular weight is 500,000) are placed in a stirring tank at a weight ratio of 20:1. The total weight of TiO2 and PEO is 10 g. 30 mL of anhydrous acetonitrile is added as solvent and stirred into a uniform slurry by mechanical stirring. The prepared slurry is coated on a PET release film with a 50 μm coating gap width using a doctor coater and dried at 70 °C to form a TiO2 dry film. The dry film thickness is measured by a spiral micrometer and is 1.28 μm;

[0137] Silica powder (particle size of 2000 nm) and LPSC powder (particle size of 7000 nm) were mixed in a weight ratio of 1:1, and then nitrile rubber (molecular weight of 40000) was added. The total weight of silica powder, LPSC and nitrile rubber was 3 g, and the content of nitrile rubber was 2%. Then 10 mL of xylene was added as a solvent and stirred into a uniform slurry by mechanical stirring. The prepared slurry was coated on a PET release film with a coating device with a slit width of 50 μm, and the Si-SE dry film was dried at 70 ℃. The dry film thickness was measured by a spiral micrometer and was 4.69 μm.

[0138] (2) The coating surface of the TiO2 dry film prepared in step (1) is laminated to the lithium surface of the copper-lithium composite tape and rolled at a pressure of 10 MPa and a speed of 0.3 m / min to transfer the TiO2 dry film to the lithium foil side of the copper-lithium composite tape. The PET release film is peeled off to obtain a Li-TiO2 composite film.

[0139] The coating surface of the Si-SE dry film prepared in step (1) was laminated with the TiO2 dry film surface of the Li-TiO2 composite film and rolled at a pressure of 20 MPa to transfer the Si-SE composite film to the surface of the Li-TiO2 composite film. The PET release film was peeled off to obtain a Li-20Ti-1Si-S composite film.

[0140] Preparation of lithium-ion batteries:

[0141] Negative electrode sheet: The Li-20Ti-1Si-S composite film is cut into 4×6 cm electrodes with tabs using a die-cutting machine as the negative electrode sheet;

[0142] Positive electrode: Vapor-grown conductive carbon fiber (VGCF) was used as the conductive agent, hydrogenated nitrile rubber (HNBR) was used as the binder, and the mixture was placed in a covered glass bottle with a mass ratio of NCM811:LPSC:VGCF:HNBR=80:17:1:2. Xylene was added to a solid content of 70%. The mixture was stirred at 500 rpm for 12 h at room temperature to form a uniform slurry. The slurry was then coated on aluminum foil with a coating machine, and the coating slit width was adjusted to 200 μm. After drying, the active material loading was 16 mg / cm 2 The positive electrode.

[0143] Electrolyte layer: LPSC and HNBR were mixed in a mass ratio of 99:1 and placed in a covered glass bottle. Xylene was added to a solid content of 60%. The mixture was stirred at 500 rpm for 12 h at room temperature to form a uniform slurry. The slurry was then coated on a PET release film with a coater and dried in a vacuum oven at 80 °C for 10 h to obtain a sulfide electrolyte membrane. The dry film thickness was measured to be 34 μm with a spiral micrometer.

[0144] They are assembled into solid-state batteries by laminating the positive electrode sheet with the material area and the electrolyte layer on the PET release film to form a laminated film. The roller gap width of the roller press is adjusted to 70% of the thickness of the laminated film. The laminated film is then rolled and the electrolyte layer is transferred to the positive electrode sheet. The PET release film is then peeled off to obtain a positive-electrolyte composite film. The composite film is then cut into films of the same size and shape as the negative electrode sheet using a die-cutting machine. The composite film is then laminated with the negative electrode sheet loading material surface. The tabs are then welded and the battery is vacuum-sealed with an aluminum-plastic film in the conventional manner in the industry, but there is no need to leave an air bag. The assembled battery is tested under conventional pressure fixtures in the industry. Example 10

[0145] This embodiment relates to the preparation of a Li-20Ti-1Si-S composite film and a lithium ion battery used as a lithium metal negative electrode, and the specific operations are as follows:

[0146] (1) TiO2 powder (particle size D50 is 1500 nm) and PEO (molecular weight is 500,000) are placed in a stirring tank at a weight ratio of 20:1. The total weight of TiO2 and PEO is 10 g. 30 mL of anhydrous acetonitrile is added as a solvent and stirred into a uniform slurry by mechanical stirring. The prepared slurry is coated on a PET release film with a 50 μm coating gap width using a doctor coater and dried at 70 °C to form a TiO2 dry film. The dry film thickness is measured by a spiral micrometer and is 1.35 μm;

[0147] Silica powder (particle size of 2000 nm) and LPSC powder (particle size of 4000 nm) were mixed in a weight ratio of 1:1, and then nitrile rubber (molecular weight of 45000) was added. The total weight of silica powder, LPSC and nitrile rubber was 3 g, and the content of nitrile rubber was 2%. Then 10 mL of xylene was added as a solvent and stirred into a uniform slurry by mechanical stirring. The prepared slurry was coated on a PET release film with a coating device with a slit width of 50 μm, and the Si-SE dry film was dried at 70 °C. The dry film thickness was measured with a spiral micrometer to be 3.07 μm.

[0148] (2) The coating surface of the TiO2 dry film prepared in step (1) is laminated to the lithium surface of the copper-lithium composite tape and rolled at a pressure of 10 MPa and a speed of 0.3 m / min to transfer the TiO2 dry film to the lithium foil side of the copper-lithium composite tape. The PET release film is peeled off to obtain a Li-TiO2 composite film.

[0149] The coating surface of the Si-SE dry film prepared in step (1) was laminated with the TiO2 dry film surface of the Li-TiO2 composite film and rolled at a pressure of 20 MPa to transfer the Si-SE composite film to the surface of the Li-TiO2 composite film. The PET release film was peeled off to obtain a Li-20Ti-1Si-S composite film.

[0150] Preparation of lithium-ion batteries:

[0151] Negative electrode sheet: The Li-20Ti-1Si-S composite film is cut into 4×6 cm electrodes with tabs using a die-cutting machine as the negative electrode sheet;

[0152] Positive electrode: Vapor-grown conductive carbon fiber (VGCF) was used as the conductive agent, hydrogenated nitrile rubber (HNBR) was used as the binder, and the mixture was placed in a covered glass bottle with a mass ratio of NCM811:LPSC:VGCF:HNBR=80:17:1:2. Xylene was added to a solid content of 70%. The mixture was stirred at 500 rpm for 12 h at room temperature to form a uniform slurry. The slurry was then coated on aluminum foil with a coating machine, and the coating slit width was adjusted to 200 μm. After drying, the active material loading was 16 mg / cm 2 The positive electrode sheet of the same size as the ternary eight series positive electrode sheet;

[0153] Electrolyte layer: LPSC and HNBR were mixed in a mass ratio of 99:1, placed in a covered glass bottle, and xylene was added to a solid content of 60%. The mixture was stirred at 500 rpm for 12 hours at room temperature to form a uniform slurry, which was then coated on a PET release film with a coater and dried in a vacuum oven at 80 °C for 10 hours to obtain a sulfide electrolyte membrane. The dry film thickness was measured by a spiral micrometer to be 35 μm. Sulfide solid electrolyte layer;

[0154] They are assembled into solid-state batteries by laminating the positive electrode sheet with the material area and the electrolyte layer on the PET release film to form a laminated film. The roller gap width of the roller press is adjusted to 70% of the thickness of the laminated film. The laminated film is then rolled and the electrolyte layer is transferred to the positive electrode sheet. The PET release film is then peeled off to obtain a positive-electrolyte composite film. The composite film is then cut into films of the same size and shape as the negative electrode sheet using a die-cutting machine. The composite film is then laminated with the negative electrode sheet loading material surface. The tabs are then welded and the battery is vacuum-sealed with an aluminum-plastic film in the conventional manner in the industry, but there is no need to leave an air bag. The assembled battery is tested under conventional pressure fixtures in the industry. Comparative Example 1

[0155] This comparative example relates to the preparation of a lithium ion battery, which is specifically as follows:

[0156] (1) Sulfide solid electrolyte LPSC powder and nitrile rubber powder were mixed in a mass ratio of 99:1, and xylene was added as a solvent to a solid content of 60%. The mixture was stirred at 500 rpm for 10 h to form a uniform slurry, which was then coated on a PET release film using a coater. The sulfide solid electrolyte membrane was obtained by vacuum drying at 80 °C for 10 h. The dry film thickness was measured by a spiral micrometer and was 35 μm.

[0157] (2) According to the method of Example 1, the coated film is rolled together with the ternary octane positive electrode to combine the positive electrode and the electrolyte layer together, and then the substrate of the electrolyte layer is peeled off to obtain a positive electrode-electrolyte layer composite film.

[0158] (3) According to the method of Example 1, the positive electrode-electrolyte layer composite film prepared in step (2) is rolled together with the copper-lithium composite tape into a sandwich structure; the nickel electrode tab is welded on the negative electrode side, and the aluminum electrode tab is welded on the positive electrode side. The battery cell with the electrode tabs welded is top-sealed, side-sealed and vacuum-sealed in an aluminum-plastic film to obtain a laminated battery. Comparative Example 2

[0159] This comparative example involves the preparation of a Li-TiO2 composite film and a lithium-ion battery for use as a lithium metal negative electrode. The difference from Example 10 is that the composite film used as a lithium metal negative electrode does not contain a Si-SE layer, and the Li-TiO2 composite film is directly used as a lithium metal negative electrode. The other operations are the same, and the corresponding lithium-ion battery is prepared. Comparative Example 3

[0160] This comparative example relates to the preparation of a Li-Si-S composite film and a lithium ion battery for use as a lithium metal negative electrode. The difference from Example 10 is that the composite film used as a lithium metal negative electrode does not contain a TiO2 layer, and the coating surface of the Si-SE composite film is directly bonded to the lithium surface of the copper-lithium composite belt, and roller pressing is performed at a rolling pressure of 20 MPa to transfer the Si-SE composite film to the surface of the copper-lithium composite belt to obtain a Li-Si-S composite film. The remaining operations are the same to prepare the corresponding lithium ion battery. Comparative Example 4

[0161] This comparative example relates to the preparation of a Li-19Ti-Si composite film and a lithium ion battery used as a lithium metal negative electrode, and the specific operation is as follows:

[0162] (1) TiO2 powder (particle size D50 is 1500 nm), silicon powder (particle size D50 = 2000 nm) and PEO (molecular weight is 500,000) are placed in a stirring tank at a weight ratio of 19:1:1. The total weight of TiO2, silicon powder and PEO is 10 g. 30 mL of anhydrous acetonitrile is added as solvent and stirred into a uniform slurry by mechanical stirring. The prepared slurry is coated on a PET release film with a 50 μm coating gap width using a doctor coater and dried at 70 °C to form a TiO2-Si dry film. The dry film thickness is measured by a spiral micrometer to be 2.75 μm.

[0163] (2) The coating surface of the TiO2-Si dry film prepared in step (1) is laminated to the lithium surface of the copper-lithium composite tape and rolled at a pressure of 10 MPa and a speed of 0.3 m / min to transfer the TiO2-Si dry film to the lithium foil side of the copper-lithium composite tape. The PET release film is peeled off to obtain a Li-19Ti-Si composite film.

[0164] Preparation of lithium-ion batteries:

[0165] Negative electrode sheet: The Li-19Ti-Si composite film is cut into 4×6 cm electrodes with tabs using a die-cutting machine as the negative electrode sheet;

[0166] Positive electrode: Vapor-grown conductive carbon fiber (VGCF) was used as the conductive agent, hydrogenated nitrile rubber (HNBR) was used as the binder, and the mixture was placed in a covered glass bottle with a mass ratio of NCM811:LPSC:VGCF:HNBR=80:17:1:2. Xylene was added to a solid content of 70%. The mixture was stirred at 500 rpm for 12 h at room temperature to form a uniform slurry. The slurry was then coated on aluminum foil with a coating machine, and the coating slit width was adjusted to 200 μm. After drying, the active material loading was 16 mg / cm 2 The positive electrode sheet of the same size as the ternary eight series positive electrode sheet;

[0167] Electrolyte layer: LPSC and HNBR were mixed in a mass ratio of 99:1, placed in a covered glass bottle, and xylene was added to a solid content of 60%. The mixture was stirred at 500 rpm for 12 h at room temperature to form a uniform slurry, which was then coated on a PET release film using a coater and dried in a vacuum oven at 80 °C for 10 h to obtain a sulfide electrolyte membrane. The dry film thickness was measured by a spiral micrometer to be 35 μm. Sulfide solid electrolyte layer;

[0168] They are assembled into solid-state batteries by laminating the positive electrode sheet with the material area and the electrolyte layer on the PET release film to form a laminated film. The roller gap width of the roller press is adjusted to 70% of the thickness of the laminated film. The laminated film is then rolled and the electrolyte layer is transferred to the positive electrode sheet. The PET release film is then peeled off to obtain a positive-electrolyte composite film. The composite film is then cut into films of the same size and shape as the negative electrode sheet using a die-cutting machine. The composite film is then laminated with the negative electrode sheet loading material surface. The tabs are then welded and the battery is vacuum-sealed with an aluminum-plastic film in the conventional manner in the industry, but there is no need to leave an air bag. The assembled battery is tested under conventional pressure fixtures in the industry.

[0169] Performance Testing

[0170] The lithium ion batteries prepared in the above examples and comparative examples were subjected to electrochemical tests, and the test methods were as follows:

[0171] 1 C rate capacity: In a 25 ℃ constant temperature room, charge to 4.3 V at 1 C constant current, let stand for 10 min, then discharge to 2.8 V at 1 C constant current, let stand for 10 min, and then perform the second cycle charge and discharge operation. The discharge capacity of the second cycle is the 1 C rate capacity;

[0172] 2 C rate capacity: In a 25 ℃ constant temperature room, charge to 4.3 V at 2 C constant current, let stand for 10 min, then discharge to 2.8 V at 2 C constant current, let stand for 10 min, and then perform the second cycle charge and discharge operation. The discharge capacity of the second cycle is the 2 C rate capacity;

[0173] 0.1 C first efficiency: In a 25 ℃ constant temperature room, charge to 4.3 V at 0.1 C constant current, record the first 0.1 C charging capacity, let stand for 10 min, then discharge to 2.8 V at 0.1 C constant current, record the first 0.1 C discharge capacity, calculate 0.1 C first efficiency = (first 0.1 C discharge capacity / first 0.1 C charging capacity) × 100%;

[0174] 0.2 C cycle average coulombic efficiency: in a 25 ℃ constant temperature room, charge to 4.3 V at 0.2 C constant current, let stand for 10 min, then discharge to 2.8 V at 0.2 C constant current, let stand for 10 min, and then perform cyclic charge and discharge operations. Calculate the average coulombic efficiency from the 2nd to the 100th cycle, which is the 0.2 C cycle average coulombic efficiency;

[0175] 0.2 C cycle 100 times capacity retention rate: in a 25 ℃ constant temperature room, charge to 4.3 V at 0.2 C constant current, let stand for 10 min, then discharge to 2.8 V at 0.2 C constant current, record the first discharge capacity, let stand for 10 min, then cycle charge and discharge 100 times, record the discharge capacity of the 100th cycle, calculate 0.2 C cycle 100 times capacity retention rate = (discharge capacity of the 100th cycle / first discharge capacity) × 100%.

[0176] The above performance test results are shown in Table 1 below:

[0177] Table 1

[0178]

[0179] It can be seen from Table 1 that compared with the lithium ion battery prepared by directly using the copper-lithium composite belt without a modification layer as the negative electrode in Comparative Example 1, the lithium metal negative electrode is obtained by setting the first modification layer and the second modification layer on the lithium metal surface of the copper-lithium composite belt in Examples 1 to 10. The lithium ion battery prepared by this type of lithium metal negative electrode has high gram capacity, high initial efficiency, excellent rate performance and long cycle life, and the ratio of the discharge capacity at a current density of 2 C to the discharge capacity at a current density of 1 C is more than 83%, the first efficiency at a current density of 0.1 C is not less than 85%, the cycle average coulomb efficiency at 0.2 C (the average coulomb efficiency from the second cycle to the 100th cycle) is not less than 98.5%, and the capacity retention rate after 100 cycles at 0.2 C is not less than 92%.

[0180] It can be seen from Example 10 and Comparative Examples 2 and 3 that only setting the first modification layer or the second modification layer on the lithium metal surface of the lithium-copper composite belt cannot effectively improve the cycle life of the lithium-ion battery. In addition, in Comparative Example 4, silicon particles are directly added to the first modification layer to prepare a lithium metal negative electrode co-modified with Ti, Si, and lithium titanate. Compared with Comparative Example 1, the gram capacity and cycle life are improved, but the first efficiency, average coulomb efficiency and cycle life of the battery are lower than those of Comparative Example 2. It can be seen that directly adding silicon powder that inhibits lithium dendrites to the first modification layer will reduce the conductivity and buffering effect of the first modification layer, which is not conducive to improving the battery cycle performance.

[0181] The above-described embodiments are only preferred embodiments for fully illustrating the present invention, and the protection scope of the present invention is not limited thereto. Equivalent substitutions or changes made by those skilled in the art based on the present invention are within the protection scope of the present invention. The protection scope of the present invention shall be subject to the claims.

Claims

1. A lithium metal negative electrode, characterized in that The lithium metal negative electrode comprises a substrate, a first modified layer and a second modified layer; At least one of the two sides of the substrate along the thickness direction contains metallic lithium; The first modified layer is disposed on the surface of the metallic lithium, and the first modified layer comprises titanium and a Li-Ti-O compound; The second modified layer is disposed on a side of the first modified layer away from the substrate, and the second modified layer comprises silicon and a sulfide solid electrolyte.

2. The lithium metal negative electrode according to claim 1, characterized in that The substrate is a lithium metal strip or a copper-lithium composite metal strip or a lithium alloy composite strip; the lithium alloy composite strip is a lithium-aluminum alloy composite strip or a lithium-magnesium alloy composite strip or a lithium-tin alloy composite strip.

3. The lithium metal negative electrode according to claim 1, characterized in that The thickness of the first modified layer is 0.48-3 μm; The second modification layer has a thickness of 1-5 μm.

4. The lithium metal negative electrode according to claim 1, characterized in that The Li-Ti-O compound comprises lithium titanate Li4Ti5O 12 ; The first modification layer further comprises a first binder; the first binder is polyethylene oxide; the molecular weight of the first binder is 100,000-800,000; the mass percentage of the first binder in the first modification layer is 3%-10%.

5. The lithium metal negative electrode according to claim 1, characterized in that Contain at least one of the following characteristics: (1) The particle size D50 of the silicon is 500-5000 nm; (2) The particle size D50 of the sulfide solid electrolyte is 500-8000 nm; (3) The sulfide solid electrolyte is Li6PS5Cl and / or Li3PS4; (4) The mass ratio of silicon to sulfide solid electrolyte in the second modified layer is (0.2-2):1; (5) The second modification layer further comprises a second binder; the second binder is selected from one or more of nitrile rubber, styrene-butadiene rubber, and SEBS; the molecular weight of the second binder is 3000-50000; and the mass percentage of the second binder in the second modification layer is 0.5%-4%.

6. A method for preparing a lithium metal negative electrode according to any one of claims 1 to 5, characterized in that: The following steps are involved: S1, coating a first slurry comprising titanium dioxide, a first binder and a first solvent on one surface of a first release film, and drying the slurry to form a first coating on the first release film; coating a second slurry comprising silicon powder, a sulfide solid electrolyte, a second binder and a second solvent on one surface of the second release film, and drying the slurry to form a second coating on the second release film; S2, transferring the first coating to the side of the substrate containing metallic lithium to form a first modified layer, and then transferring the second coating to the side of the first modified layer away from the substrate to form a second modified layer, thereby obtaining the lithium metal negative electrode.

7. The preparation method according to claim 6, characterized in that: Contain at least one of the following characteristics: (1) The particle size D50 of the titanium dioxide is 100-3000 nm; (2) The mass ratio of titanium dioxide to the first binder in the first slurry is (10-30):1; (3) The first solvent is selected from one or more of acetonitrile, N-methylpyrrolidone, and N,N-dimethylformamide.

8. The preparation method according to claim 6, characterized in that: The second solvent is toluene and / or xylene.

9. The preparation method according to claim 6, characterized in that: In S2, the transfer method includes rolling, specifically: the first coating is transferred to the side of the substrate containing metallic lithium by a first rolling, to form a first modified layer, and then the second coating is transferred to the side of the first modified layer away from the substrate by a second rolling, to form a second modified layer, to obtain the lithium metal negative electrode; the pressure of the first rolling is 5-50 MPa; the pressure of the second rolling is 10-50 MPa.

10. A secondary battery comprising a negative electrode plate, characterized in that: The negative electrode plate is a lithium metal negative electrode as described in any one of claims 1-5, or a lithium metal negative electrode prepared by the preparation method as described in any one of claims 6-9.