A perfluoropolyether block copolymer and its preparation method and application
Through the preparation of perfluoropolyether block copolymer, the wear resistance and environmentally friendly problems of screen coatings of electronic products are solved, and high water resistance, antifouling performance and wear resistance are achieved, which is suitable for surface protection of electronic products.
Patent Information
- Application Number
- CN202410893616.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-04
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-07-04
AI Technical Summary
The wear resistance, light transmission and chemical stability of the screen coatings of existing electronic products are poor, and traditional organic fluoride is harmful to the environment and the human body. It is necessary to develop a green, pollution-free fluoropolymer material to replace traditional fluorine. Polymers improve the protective performance of electronic products.
Perfluoropolyether block copolymer is prepared by atom transfer radical polymerization method, and polymerization is carried out using perfluoropolyether bisol and methacryloyloxypropyl tris(trimethylsiloxane)silane to control the polymerization degree To improve adhesion and durability, a perfluoropolyether block copolymer has excellent antifouling properties and wear resistance.
It has achieved a green and environmentally friendly perfluoropolyether block copolymer, with high water resistance, antifouling properties and wear resistance, and is suitable for surface protection of electronic products, significantly improving the comprehensive performance of electronic products.
Smart Images

Figure QLYQS_1 
Figure QLYQS_2 
Figure BDA0004928305360000021
Abstract
Description
Technical Field
[0001] The invention belongs to the field of polymer fluorine materials, and specifically relates to a perfluoropolyether block copolymer and a preparation method and application thereof. Background Art
[0002] In modern people's lives, smart electronic devices, such as tablets, smart phones, laptops and smart watches, are gradually entering ordinary people's homes. As their prices become more and more affordable, they are widely welcomed by consumers. At present, most of these electronic products are equipped with touch panels, so today's consumers and manufacturers not only pay attention to the appearance and performance configuration of the products, but also pay more attention to the touch, waterproof performance and durability of the screen protective film of electronic products. However, with the development of technology to the present, there are still many difficult to solve problems in the screen coating of electronic products, such as the unsatisfactory wear resistance of the screen coating, poor light transmittance, heat resistance and chemical stability, so solving these problems in actual production and life has become a hot topic for researchers.
[0003] Fluoropolymers can impart a protective effect to substrates at a relatively thin film thickness (less than 1 μm). By applying a solution containing a fluoropolymer on the surface of an electronic component, a protective coating can be formed after drying. Patent CN116769375A discloses a self-curing protective agent composition, which is composed of a self-curing fluoropolymer and a fluorinated solvent, and the self-curing fluoropolymer is obtained by free radical copolymerization of at least a fluoroacrylate monomer, a non-fluoroacrylate monomer containing a cyclic group or a tertiary butyl group, and an acrylate monomer containing an isocyanate group. Although the self-curing protective agent composition can form a protective coating with excellent and durable waterproof and antifouling properties and excellent anti-rust properties on the surface of electronic devices, its wear resistance still needs to be improved. In addition, traditional organic fluorides are more harmful to the environment. Therefore, when applying new fluoropolymers to the field of surface protection of electronic components, while improving the comprehensive performance, it should also be noted that the use of fluoropolymers that are harmful to the environment and human body should be avoided.
[0004] Based on the problems existing in the existing technology, a green and pollution-free fluoropolymer material is developed to replace the traditional organic fluoride for application in the protection of electronic products. While having a good protective effect on electronic products, it will not pose a threat or harm to the natural environment and human body. This is a very challenging and practical research. Summary of the invention
[0005] In view of the deficiencies in the prior art, the present invention provides a perfluoropolyether block copolymer and a preparation method and application thereof. The perfluoropolyether block copolymer is green and non-toxic, has a high synthesis rate, and the coating formed by using it in a surface treatment agent has good water resistance, wear resistance and excellent anti-fouling performance.
[0006] The first aspect of the present invention provides a method for preparing a perfluoropolyether block copolymer, comprising the following preparation steps:
[0007] (1) perfluoropolyether diol, triethylamine and 1,1,2-trifluorotrichloroethane are mixed in sequence, stirred in an ice water bath, a brominating agent solution is added dropwise thereto, reacted for 20-24 hours, and then spin-dried to obtain a mixture 1;
[0008] (2) adding 1,1,2-trifluorotrichloroethane and distilled water to the mixture 1 obtained in step (1) in sequence, stirring thoroughly, standing to separate and removing distilled water, repeating the process of adding distilled water, stirring, standing, and removing distilled water 2-3 times, adding anhydrous sodium sulfate, standing, centrifuging to remove anhydrous sodium sulfate, and spinning to dryness to obtain a perfluoropolyether diol initiator;
[0009] (3) mixing the perfluoropolyether diol initiator, methacryloxypropyl tris(trimethylsiloxy)silane, cuprous chloride and mixed solvent obtained in step (2), freezing, evacuating, introducing inert gas, thawing, and repeating the freezing, evacuating, introducing inert gas and thawing process 2-3 times to obtain mixture 2;
[0010] (4) dissolving 2,2-bipyridine in a mixed solvent, adding the mixture 2 obtained in step (3), repeating the freezing, vacuuming, introducing inert gas, and thawing process in step (3) 2-3 times, reacting at 70-80° C. for 3-4 hours, passing through a neutral alumina column, and performing rotary evaporation concentration, precipitation, and separation to obtain a mixture 3;
[0011] (5) The mixture 3 of step (4) is dissolved in acetonitrile, ethanolamine, potassium carbonate and potassium iodide are added thereto, and refluxed under a nitrogen environment to obtain a perfluoropolyether block copolymer.
[0012] In some embodiments, the structural formula of the perfluoropolyether diol is:
[0013]
[0014] The number average molecular weight is 2000-4000, wherein m and n are both integers greater than 0.
[0015] The present invention adopts the method of atom transfer radical polymerization to prepare the perfluoropolyether block copolymer. Firstly, the perfluoropolyether diol is used as the raw material, triethylamine is used as the acid binding agent, 1,1,2-trifluorotrichloroethane is used as the solvent, the perfluoropolyether diol macromolecular initiator is synthesized by a brominating agent, and then methacryloxypropyl tris(trimethylsiloxy)silane and the perfluoropolyether diol macromolecular initiator are used to initiate the polymerization reaction to obtain the perfluoropolyether block copolymer, and the polymerization degree of the monomer is controlled within a certain range by controlling the synthesis process, which is beneficial to improve the comprehensive performance of the perfluoropolyether block copolymer.
[0016] At present, many studies at home and abroad use perfluoropolyether alcohol as raw material for research, but the comprehensive performance of the obtained perfluoropolyether polymer is still not ideal. The perfluoropolyether diol used in the present invention contains a perfluoropolyether main chain and is connected to a functional double-terminal hydroxyl group, which has the advantages of better waterproof and oil release, anti-sticking, low surface energy, chemical resistance and stability. It is used in the field of surface treatment agents to obtain better protective performance than the polymer synthesized from perfluoropolyether alcohol (PFPE-Si(OR)3), which further expands the application range of perfluoropolyether diol. In addition, in this study, methacryloxypropyl tris(trimethylsiloxy)silane was selected as a monomer and connected to both ends of perfluoropolyether diol, which can significantly improve the adhesion, durability and wear resistance of perfluoropolyether block copolymers.
[0017] The structure of the perfluoropolyether block copolymer synthesized in the present invention is (RO)3Si-PFPE-Si(OR)3, which has better performance than the perfluoropolyether copolymer having only one -Si(OR)3 functional group at one end, and has better antifouling performance and wear resistance.
[0018] The applicant has found that by strictly controlling the ratio of the substances used in each step, it is advantageous to control the polymerization degree of methacryloxypropyltris(trimethylsiloxy)silane and improve the synthesis rate of the perfluoropolyether block copolymer.
[0019] In some embodiments, the ratio of the amount of perfluoropolyether diol, triethylamine and 1,1,2-trifluorotrichloroethane used in step (1) is 1 mmol: (2.1-2.5) mmol: (28-33) mL.
[0020] Preferably, in step (1), the usage ratio of perfluoropolyether diol, triethylamine and 1,1,2-trifluorotrichloroethane is 1 mmol:2.3 mmol:30 mL.
[0021] In some embodiments, the brominating agent solution is a 1,1,2-trifluorotrichloroethane solution containing 2-bromoisobutyryl bromide; the molar ratio of the 2-bromoisobutyryl bromide to the perfluoropolyether diol is (2-2.5):1.
[0022] Preferably, the brominating agent solution is a 1,1,2-trifluorotrichloroethane solution containing 2-bromoisobutyryl bromide; the molar ratio of the 2-bromoisobutyryl bromide to the perfluoropolyether diol is 2.3:1.
[0023] In some embodiments, the amount of 2,2-bipyridine is 10-20% of the molar amount of the perfluoropolyether diol initiator in the mixture 2.
[0024] Preferably, the amount of 2,2-bipyridine used is 16% of the molar amount of the perfluoropolyether diol initiator in mixture 2.
[0025] In some embodiments, the molar ratio of the perfluoropolyether diol initiator, methacryloxypropyl tris(trimethylsiloxy)silane and cuprous chloride in step (3) is 1:(5-10):(1.3-1.6).
[0026] Preferably, in step (3), the molar ratio of the perfluoropolyether diol initiator, methacryloxypropyl tris(trimethylsiloxane) and cuprous chloride is 1:8:1.5.
[0027] In some embodiments, the mixed solvent comprises trifluoroethanol and ethyl perfluorobutyl ether in a volume ratio of (2.5-3):1.
[0028] Preferably, the mixed solvent comprises trifluoroethanol and ethyl perfluorobutyl ether in a volume ratio of 2.8:1.
[0029] In some embodiments, in step (5), the molar ratio of mixture 3, ethanolamine and potassium carbonate is 1:(2-2.2):(2-2.3); the reflux temperature is 80-90° C., and the reflux time is 20-30 h.
[0030] The second aspect of the present invention provides a perfluoropolyether block copolymer prepared by the above-mentioned preparation method, and the structural formula of the perfluoropolyether block copolymer is:
[0031]
[0032] Among them, 2≤o+k≤15, o and k are both integers greater than 0.
[0033] In some embodiments, the route for the mixture 3 in step (5) to generate the perfluoropolyether block copolymer is as follows:
[0034]
[0035] The third aspect of the present invention provides an application of the perfluoropolyether block copolymer prepared by the above-mentioned preparation method in the field of surface treatment agents.
[0036] In some embodiments, the perfluoropolyether block copolymer is used in an amount of 0.1-10 wt % of the surface treatment agent.
[0037] In some embodiments, the preparation of the surface treatment agent includes: using trifluorotoluene as a diluent to prepare a perfluoropolyether block copolymer into a spray liquid, adding isobutanol and acetic acid, wherein the isobutanol is 0.4-0.6% of the mass of the spray liquid, and the concentration of acetic acid in the spray liquid is 0.4-0.5 mg / L.
[0038] Based on the problems existing in the prior art, the beneficial effects of the present invention are:
[0039] The invention strictly controls the preparation process, uses perfluoropolyether diol as raw material, triethylamine as acid binding agent, 1,1,2-trifluorotrichloroethane as solvent, synthesizes perfluoropolyether diol macromolecular initiator by brominating agent, and then initiates polymerization reaction with methacryloxypropyl tri(trimethylsiloxy)silane and perfluoropolyether diol macromolecular to obtain perfluoropolyether block copolymer. The perfluoropolyether block copolymer is green and environmentally friendly, has high synthesis rate, has excellent comprehensive performance, and has good water resistance, antifouling performance and wear resistance when applied to surface protective agent. DETAILED DESCRIPTION
[0040] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0041] In order to better illustrate the specific implementation mode of the present invention, further examples are given below.
[0042] The number average molecular weight of the perfluoropolyether diol used in Examples 1-6 and Comparative Example 1 of the present invention is 3000, purchased from Taipuda New Materials Co., Ltd., and the number average molecular weight of the perfluoropolyether alcohol used in Comparative Example 2 is 3000, purchased from Suzhou Cangmu New Materials Co., Ltd.
[0043] The number average molecular weight of the perfluoropolyether block copolymer in the present invention is obtained by gel permeation chromatography.
[0044] Preparation Example 1
[0045] Preparation of brominating agent solution: 5.3 g of 2-bromoisobutyryl bromide was dissolved in 100 mL of 1,1,2-trifluorotrichloroethane to obtain a brominating agent solution.
[0046] Preparation Example 2
[0047] Preparation of mixed solvent: 280 mL of trifluoroethanol and 100 mL of ethyl perfluorobutyl ether were mixed evenly to obtain a mixed solvent.
[0048] Example 1
[0049] A method for preparing a perfluoropolyether block copolymer comprises the following preparation steps:
[0050] (1) 10 mmol of perfluoropolyether diol, 23 mmol of triethylamine and 300 mL of 1,1,2-trifluorotrichloroethane were mixed in sequence, stirred in an ice-water bath at 0°C, 100 mL of brominating agent solution was added dropwise thereto, reacted for 22 hours, and then dried by spin drying to obtain a mixture 1;
[0051] (2) adding 100 mL of 1,1,2-trifluorotrichloroethane and 100 mL of distilled water to the mixture 1 obtained in step (1) in sequence, stirring thoroughly, standing to separate and removing the distilled water, repeating the process of adding distilled water, stirring, standing, and removing the distilled water twice, adding anhydrous sodium sulfate and standing for 10 h, centrifuging to remove the anhydrous sodium sulfate, and spinning to dryness to obtain a perfluoropolyether diol initiator;
[0052] (3) 5 mmol of the perfluoropolyether diol initiator obtained in step (2), 40 mmol of methacryloxypropyl tris(trimethylsiloxy)silane, 7.5 mmol of cuprous chloride and 200 mL of a mixed solvent were mixed, and the mixture was frozen at -25°C for 3 h, evacuated, introduced with argon for 30 min, and thawed. The freezing, evacuation, introduction of inert gas and thawing process were repeated three times to obtain a mixture 2;
[0053] (4) 0.8 mmol of 2,2-bipyridine was dissolved in 200 mL of a mixed solvent and added to the mixture 2 obtained in step (3). The freezing, vacuuming, introducing argon for 30 min, and thawing process in step (3) were repeated three times, and then reacted at 75° C. for 3.5 h. The mixture was passed through a neutral alumina column, concentrated by rotary evaporation, precipitated with acetonitrile, and separated to obtain a mixture 3.
[0054] (5) 1 mmol of the mixture 3 obtained in step (4) was dissolved in 500 mL of acetonitrile, and 2.1 mmol of ethanolamine, 2.2 mmol of potassium carbonate and 0.57 g of potassium iodide were added thereto. The mixture was refluxed at 85° C. under a nitrogen environment for 25 h to obtain a perfluoropolyether block copolymer.
[0055] The brominating agent solution used is obtained from Preparation Example 1; the mixed solvent used is obtained from Preparation Example 2.
[0056] The number average molecular weight of the obtained perfluoropolyether block copolymer was 5574.
[0057] Example 2
[0058] A method for preparing a perfluoropolyether block copolymer comprises the following preparation steps:
[0059] (1) 10 mmol of perfluoropolyether diol, 21 mmol of triethylamine and 280 mL of 1,1,2-trifluorotrichloroethane were mixed in sequence, stirred in an ice-water bath at 0°C, 87 mL of brominating agent solution was added dropwise thereto, reacted for 22 hours, and then dried by spin drying to obtain a mixture 1;
[0060] (2) adding 100 mL of 1,1,2-trifluorotrichloroethane and 100 mL of distilled water to the mixture 1 obtained in step (1) in sequence, stirring thoroughly, standing to separate and removing the distilled water, repeating the process of adding distilled water, stirring, standing, and removing the distilled water twice, adding anhydrous sodium sulfate and standing for 10 h, centrifuging to remove the anhydrous sodium sulfate, and spinning to dryness to obtain a perfluoropolyether diol initiator;
[0061] (3) 5 mmol of the perfluoropolyether diol initiator obtained in step (2), 25 mmol of methacryloxypropyl tris(trimethylsiloxy)silane, 6.5 mmol of cuprous chloride and 200 mL of a mixed solvent were mixed, and the mixture was frozen at -20°C for 4 h, evacuated, introduced with argon for 30 min, and thawed. The freezing, evacuation, introduction of inert gas and thawing process were repeated twice to obtain a mixture 2;
[0062] (4) 0.5 mmol of 2,2-bipyridine was dissolved in 200 mL of a mixed solvent and added to the mixture 2 obtained in step (3). The freezing, vacuuming, introducing argon for 30 min, and thawing process in step (3) were repeated twice, and then reacted at 70° C. for 4 h. The mixture was passed through a neutral alumina column, concentrated by rotary evaporation, precipitated with acetonitrile, and separated to obtain a mixture 3.
[0063] (5) 1 mmol of the mixture 3 obtained in step (4) was dissolved in 500 mL of acetonitrile, and 2.2 mmol of ethanolamine, 2.3 mmol of potassium carbonate and 0.45 g of potassium iodide were added thereto. The mixture was refluxed at 90° C. under a nitrogen atmosphere for 20 h to obtain a perfluoropolyether block copolymer.
[0064] The brominating agent solution used is obtained from Preparation Example 1; the mixed solvent used is obtained from Preparation Example 2.
[0065] The number average molecular weight of the obtained perfluoropolyether block copolymer was 4308.
[0066] Example 3
[0067] A method for preparing a perfluoropolyether block copolymer comprises the following preparation steps:
[0068] (1) 10 mmol of perfluoropolyether diol, 25 mmol of triethylamine and 330 mL of 1,1,2-trifluorotrichloroethane were mixed in sequence, stirred in an ice-water bath at 0°C, 105.5 mL of brominating agent solution was added dropwise thereto, reacted for 24 hours, and then dried by spin drying to obtain a mixture 1;
[0069] (2) adding 100 mL of 1,1,2-trifluorotrichloroethane and 100 mL of distilled water to the mixture 1 obtained in step (1) in sequence, stirring thoroughly, standing to separate and removing the distilled water, repeating the process of adding distilled water, stirring, standing, and removing the distilled water for 3 times, adding anhydrous sodium sulfate and standing for 10 h, centrifuging to remove the anhydrous sodium sulfate, and spinning to dryness to obtain a perfluoropolyether diol initiator;
[0070] (3) 5 mmol of the perfluoropolyether diol initiator obtained in step (2), 50 mmol of methacryloxypropyl tris(trimethylsiloxy)silane, 8 mmol of cuprous chloride and 200 mL of a mixed solvent were mixed, and the mixture was frozen at -30°C for 2 h, evacuated, introduced with argon for 30 min, and thawed. The freezing, evacuation, introduction of inert gas and thawing process were repeated three times to obtain a mixture 2;
[0071] (4) 1 mmol of 2,2-bipyridine was dissolved in 200 mL of a mixed solvent, and the mixture was added to the mixture 2 obtained in step (3). The freezing, vacuuming, introducing argon for 30 min, and thawing process in step (3) were repeated three times, and the mixture was reacted at 80° C. for 4 h. The mixture was passed through a neutral alumina column, concentrated by rotary evaporation, precipitated with acetonitrile, and separated to obtain a mixture 3.
[0072] (5) 1 mmol of the mixture 3 obtained in step (4) was dissolved in 500 mL of acetonitrile, and 2.2 mmol of ethanolamine, 2.3 mmol of potassium carbonate and 0.57 g of potassium iodide were added thereto. The mixture was refluxed at 85° C. under a nitrogen environment for 25 h to obtain a perfluoropolyether block copolymer.
[0073] The brominating agent solution used is obtained from Preparation Example 1; the mixed solvent used is obtained from Preparation Example 2.
[0074] The number average molecular weight of the obtained perfluoropolyether block copolymer was 6412.
[0075] Example 4
[0076] A method for preparing a perfluoropolyether block copolymer, the specific implementation method is the same as that of Example 1, except that the perfluoropolyether diol initiator used in step (3) is 6 mmol.
[0077] The number average molecular weight of the obtained perfluoropolyether block copolymer was 4720.
[0078] Example 5
[0079] A method for preparing a perfluoropolyether block copolymer, the specific implementation method is the same as that of Example 1, except that the amount of methacryloxypropyl tris(trimethylsiloxy)silane used in step (3) is 20 mmol.
[0080] The number average molecular weight of the obtained perfluoropolyether block copolymer was 3885.
[0081] Example 6
[0082] A method for preparing a perfluoropolyether block copolymer, the specific implementation method is the same as that of Example 1, except that the amount of methacryloxypropyl tris(trimethylsiloxy)silane used in step (3) is 60 mmol.
[0083] The number average molecular weight of the obtained perfluoropolyether block copolymer was 6836.
[0084] Comparative Example 1
[0085] A method for preparing a perfluoropolyether block copolymer comprises the following preparation steps:
[0086] (1) 10 mmol of perfluoropolyether alcohol, 23 mmol of triethylamine and 300 mL of 1,1,2-trifluorotrichloroethane were mixed in sequence, stirred in an ice-water bath at 0° C., 100 mL of brominating agent solution was added dropwise thereto, reacted for 22 hours, and then spin-dried to obtain a mixture 1;
[0087] (2) adding 100 mL of 1,1,2-trifluorotrichloroethane and 100 mL of distilled water to the mixture 1 obtained in step (1) in sequence, stirring thoroughly, standing to separate and removing the distilled water, repeating the process of adding distilled water, stirring, standing, and removing the distilled water twice, adding anhydrous sodium sulfate and standing for 10 h, centrifuging to remove the anhydrous sodium sulfate, and spinning to dryness to obtain a perfluoropolyether diol initiator;
[0088] (3) 5 mmol of the perfluoropolyether alcohol initiator obtained in step (2), 40 mmol of methacryloxypropyl tris(trimethylsiloxy)silane, 7.5 mmol of cuprous chloride and 200 mL of a mixed solvent were mixed, and then frozen at -25°C for 3 h, evacuated, introduced with argon for 30 min, and thawed. The freezing, evacuation, introduction of inert gas and thawing process were repeated three times to obtain a mixture 2;
[0089] (4) 0.8 mmol of 2,2-bipyridine was dissolved in 200 mL of a mixed solvent and added to the mixture 2 obtained in step (3). The freezing, vacuuming, introducing argon for 30 min, and thawing process in step (3) were repeated three times, and then reacted at 75° C. for 3.5 h. The mixture was passed through a neutral alumina column, concentrated by rotary evaporation, precipitated with acetonitrile, and separated to obtain a mixture 3.
[0090] (5) 1 mmol of the mixture 3 obtained in step (4) was dissolved in 500 mL of acetonitrile, and 2.1 mmol of ethanolamine, 2.2 mmol of potassium carbonate and 0.57 g of potassium iodide were added thereto. The mixture was refluxed at 85° C. under a nitrogen environment for 25 h to obtain a perfluoropolyether block copolymer.
[0091] The brominating agent solution used is obtained from Preparation Example 1; the mixed solvent used is obtained from Preparation Example 2.
[0092] The number average molecular weight of the obtained perfluoropolyether block copolymer was 5573.
[0093] Comparative Example 2
[0094] A method for preparing a perfluoropolyether block copolymer, the specific implementation method is the same as that of Example 1, except that an equal molar amount of 3-[tri(1-methylethoxy)silyl]propyl methacrylate is used in step (3) instead of methacryloyloxypropyl tris(trimethylsiloxy)silane.
[0095] The number average molecular weight of the obtained perfluoropolyether block copolymer was 5038.
[0096] Performance Testing
[0097] 1. Yield of perfluoropolyether block copolymer: The yield of the perfluoropolyether block copolymer obtained in each embodiment and comparative example is calculated according to the following formula: Yield (%) = M2 / M1×100%, wherein M1 represents the theoretical perfluoropolyether block copolymer (unit: g); M2 represents the actual yield of the perfluoropolyether block copolymer (unit: g). The specific results are shown in Table 1.
[0098] Table 1
[0099]
[0100] As can be seen from Table 1, the yield of the perfluoropolyether block copolymer in Examples 1-3 is relatively high, and Example 1 can reach 70.9%; while in Examples 4-6, due to the change in the preparation conditions (perfluoropolyether diol initiator, amount of methacryloxypropyl tris(trimethylsiloxane)silane), the yield of the perfluoropolyether block copolymer is reduced; in Comparative Example 1, perfluoropolyether alcohol is used instead of perfluoropolyether diol, and in Comparative Example 2, 3-[tris(1-methylethoxy)silyl]propyl methacrylate is used instead of methacryloxypropyl tris(trimethylsiloxane)silane, both of which reduce the yield of the perfluoropolyether block copolymer.
[0101] 2. The perfluoropolyether block copolymers prepared in Example 1, Comparative Example 1 and Comparative Example 2 were respectively prepared into perfluoropolyether block copolymer solutions with a concentration of 0.6 mg / mL using trifluorotoluene, and isobutanol (isobutanol is 0.5% of the mass of the perfluoropolyether block copolymer solution) and acetic acid (the concentration of acetic acid in the perfluoropolyether block copolymer solution is 0.45 mg / L) were added thereto.
[0102] The mobile phone glass was soaked in anhydrous ethanol, ultrasonically treated for 5 minutes, then taken out, washed with acetone three times, dried at 60°C for 10 minutes, and then irradiated with ultraviolet light for 30 minutes to obtain a hydroxylated mobile phone glass. The perfluoropolyether block copolymer solution of each experimental group was sprayed on the hydroxylated mobile phone glass, left at room temperature for 15 minutes, and then baked at 150°C for 1 hour. The coating on the obtained mobile phone glass was tested for the following properties:
[0103] (1) Hydrophobicity and oleophobicity: The hydrophobicity was tested by static contact angle. The static contact angle between water, n-hexadecane and the coating was measured using a JC2000C contact angle meter. The volume of each drop of the test liquid was 1 μL and the test temperature was 25°C.
[0104] (2) Wear resistance: The coating was subjected to friction test using a friction tester, with 0000# Rhino steel wool as the friction medium, a friction stroke of 20 mm, a frequency of 50 Hz, a load mass of 1035 g, and reciprocating friction. The test was stopped when the water contact angle was less than 100°.
[0105] The specific test results are shown in Table 2.
[0106] Table 2
[0107]
[0108]
[0109] As can be seen from Table 2, the coating formed by the solution prepared from the perfluoropolyether block copolymer prepared in Example 1 has significantly higher hydrophobicity, oleophobicity and wear resistance than those in Comparative Example 1 and Comparative Example 2. This is because perfluoropolyether alcohol is used instead of perfluoropolyether diol in Comparative Example 1, and 3-[tri(1-methylethoxy)silyl]propyl methacrylate is used instead of methacryloyloxypropyl tris(trimethylsiloxy)silane in Comparative Example 2, which not only reduces the yield of the perfluoropolyether block copolymer, but also changes the degree of polymerization of the silane substance, affecting the comprehensive performance of the perfluoropolyether block copolymer.
[0110] The above is only a preferred embodiment of the present invention and does not constitute any form of limitation to the present application. Although the present application is disclosed as above in the preferred embodiment, it is not intended to limit the present application. Any technician familiar with the profession, without departing from the scope of the technical solution of the present application, using the technical content disclosed above to make slight changes or modifications are equivalent to equivalent implementation cases. However, any simple modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the scope of the technical solution.
Claims
1. A method for preparing a perfluoropolyether block copolymer, characterized in that: The method comprises the following preparation steps: (1) perfluoropolyether diol, triethylamine and 1,1,2-trifluorotrichloroethane are mixed in sequence, stirred in an ice water bath, and a brominating agent solution is added dropwise thereto. After reacting for 20-24 hours, the mixture is spin-dried to obtain a mixture 1; (2) adding 1,1,2-trifluorotrichloroethane and distilled water to the mixture 1 obtained in step (1) in sequence, stirring thoroughly, standing to separate and removing distilled water, repeating the process of adding distilled water, stirring, standing, and removing distilled water 2-3 times, adding anhydrous sodium sulfate, standing, centrifuging to remove anhydrous sodium sulfate, and spinning to dryness to obtain a perfluoropolyether diol initiator; (3) mixing the perfluoropolyether diol initiator, methacryloxypropyl tris(trimethylsiloxy)silane, cuprous chloride and mixed solvent obtained in step (2), freezing, evacuating, introducing inert gas, thawing, and repeating the freezing, evacuating, introducing inert gas and thawing process 2-3 times to obtain mixture 2; (4) dissolving 2,2-bipyridine in a mixed solvent, adding the mixture 2 obtained in step (3), repeating the freezing, vacuuming, introducing inert gas, and thawing process in step (3) 2-3 times, reacting at 70-80° C. for 3-4 hours, passing through a neutral alumina column, and performing rotary evaporation concentration, precipitation, and separation to obtain a mixture 3; (5) The mixture 3 of step (4) is dissolved in acetonitrile, and ethanolamine, potassium carbonate and potassium iodide are added thereto, and refluxed under a nitrogen environment to obtain a perfluoropolyether block copolymer.
2. The method for preparing the perfluoropolyether block copolymer according to claim 1, characterized in that: The structural formula of the perfluoropolyether diol is: , The number average molecular weight is 2000-4000, wherein m and n are both integers greater than 0.
3. The method for preparing the perfluoropolyether block copolymer according to claim 1, characterized in that: In the step (1), the usage ratio of perfluoropolyether diol, triethylamine and 1,1,2-trifluorotrichloroethane is 1 mmol: (2.1-2.5) mmol: (28-33) mL.
4. The method for preparing the perfluoropolyether block copolymer according to claim 1, characterized in that: The brominating agent solution is a 1,1,2-trifluorotrichloroethane solution containing 2-bromoisobutyryl bromide; the molar ratio of the 2-bromoisobutyryl bromide to the perfluoropolyether diol is (2-2.5):
1.
5. The method for preparing the perfluoropolyether block copolymer according to claim 1, characterized in that: The amount of 2,2-bipyridine used is 10-20% of the molar amount of the perfluoropolyether diol initiator in mixture 2.
6. The method for preparing the perfluoropolyether block copolymer according to claim 1, characterized in that: In the step (3), the molar ratio of the perfluoropolyether diol initiator, methacryloxypropyl tris(trimethylsiloxy)silane and cuprous chloride is 1:(5-10):(1.3-1.6).
7. The method for preparing the perfluoropolyether block copolymer according to claim 1, characterized in that: The mixed solvent comprises trifluoroethanol and ethyl perfluorobutyl ether in a volume ratio of (2.5-3):
1.
8. A perfluoropolyether block copolymer prepared by the preparation method according to any one of claims 1 to 7, characterized in that: The structural formula of the perfluoropolyether block copolymer is: , Among them, 2≤o+k≤15, o and k are both integers greater than 0.
9. Use of the perfluoropolyether block copolymer prepared by the preparation method according to any one of claims 1 to 7 or the perfluoropolyether block copolymer according to claim 8 in the field of surface treatment agents.
10. Use of the perfluoropolyether block copolymer according to claim 9 in the field of surface treatment agents, characterized in that: The amount of the perfluoropolyether block copolymer used is 0.1-10 wt % of the surface treatment agent.