A CABS alloy material of extruded board and plastic-forming grade for refrigerator liner and preparation method thereof

By using extruded blister grade CABS alloy material in the refrigerator liner, silicon nitride, diatomaceous earth and fluorocarbon chains are introduced through the preparation method of modified PS resin, the corrosion of traditional materials in hydrofluoroolefin foaming agents is solved. The risk of cracking significantly improves the mechanical properties and corrosion resistance of the material.

CN118684993BActive Publication Date: 2024-11-05HEFEI COBEL ADVANCED PLASTICS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411194775.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-11-05
Estimated Expiration
2044-08-29

AI Technical Summary

Technical Problem

Traditional refrigerator inner liner materials are susceptible to corrosion by new hydrofluoroolefin foaming agents during long-term use, resulting in an increased risk of cracking.

Method used

Using extruded blister grade CABS alloy material, the interface interaction force between ABS resin and PP resin is enhanced by the preparation method of modified PS resin, silicon nitride, diatomaceous earth and fluorocarbon chain are introduced to improve the mechanical properties of the material and Reduce the erosion of foaming agents.

Benefits of technology

It significantly improves the mechanical properties of the alloy material, reduces the corrosion impact of the foaming agent, and improves the corrosion resistance of the refrigerator inner liner.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118684993B_ABST
    Figure CN118684993B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of polymer materials, and discloses an extruded plate blister-grade CABS alloy material for refrigerator liner and a preparation method thereof, which is composed of 50-85 parts of ABS resin, 5-30 parts of modified PS resin, 5-30 parts of PP resin, 5-15 parts of compatibilizer, and 0.1-5 parts of processing aid, calculated by mass. Compared with the prior art, the present invention has the beneficial effects that: under the action of the modified PS resin, the interaction force between the interfaces of the ABS resin, the modified PS resin, and the PP resin is enhanced, the crystallinity is improved, the mechanical properties of the alloy material are improved, and the erosion of the foaming agent is slowed down.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of polymer materials, and in particular to an extruded board blister-grade CABS alloy material for a refrigerator liner and a preparation method thereof. Background Art

[0002] At present, the refrigerator liner materials in the home appliance industry are mainly traditional HIPS (high-impact polystyrene) and ABS (acrylonitrile-butadiene-styrene copolymer). Foaming material is usually used as an insulation layer between the refrigerator liner and the external metal shell. During long-term use, the residual foaming agent will corrode the refrigerator liner. The new hydrofluoroolefin foaming agent has great application potential due to its excellent environmental performance and thermal conductivity. However, if it is used on traditional HIPS and ABS liners, the liner will face a greater risk of cracking after being corroded. Summary of the invention

[0003] In order to solve the problems mentioned in the above background technology, the present invention provides an extruded board blister grade CABS alloy material for a refrigerator liner and a preparation method thereof.

[0004] In order to achieve the above object, the present invention adopts the following technical solutions:

[0005] The first aspect of the present invention provides an extruded board blister grade CABS alloy material for refrigerator liner, which is composed of 50-85 parts of ABS resin, 5-30 parts of modified PS resin, 5-30 parts of PP resin, 5-15 parts of compatibilizer, and 0.1-5 parts of processing aid, calculated by weight.

[0006] The modified PS resin preparation method is as follows:

[0007] 1-allyloxy-2,3-propylene oxide was dispersed in THF, the pH was adjusted to 9-10 with sodium hydroxide solution, perfluorohexylethyl alcohol was dispersed in THF, added dropwise to the above reaction system, refluxed, and dried to obtain intermediate A;

[0008] The silicon nitride, diatomaceous earth was added to an aqueous ethanol solution, heated with stirring, vinyl triethoxysilane was added, the reaction was stirred, and dried to obtain intermediate B;

[0009] Under a nitrogen atmosphere, Tween 80 and deionized water were added into the reactor, stirred and dispersed evenly, intermediate B and Span 80 were ultrasonically dispersed in cyclohexane, and then added into the above reactor, stirred and dispersed evenly, finally styrene, intermediate A and tert-butyl hydroperoxide were added into the reactor, emulsified, ferrous chloride was added, polymerization reaction was carried out, ethanol was added to break the emulsion, filtered, washed and dried to obtain modified PS resin.

[0010] Preferably, the molar ratio of the 1-allyloxy-2,3-propylene oxide to perfluorohexylethyl alcohol is (1-1.1):1.

[0011] Preferably, the concentration of the sodium hydroxide solution is 0.1-1 mol / L.

[0012] Preferably, the mass ratio of silicon nitride, diatomaceous earth and vinyltriethoxysilane is 1:(0.5-2):(0.05-0.15).

[0013] Preferably, the mass concentration of the ethanol aqueous solution is 60%-80%.

[0014] Preferably, the mass ratio of Tween 80, intermediate B, Span 80, styrene, intermediate A, tert-butyl hydroperoxide and ferrous chloride is (10-30): (80-120): (5-15): (400-600): (30-50): (5-15): (10-20).

[0015] Preferably, the processing aid is selected from any one or more of antioxidants, dispersants, lubricants, and toners.

[0016] A second aspect of the present invention provides a method for preparing the above alloy material, comprising the following steps:

[0017] ABS resin, modified PS resin, PP resin, compatibilizer and processing aid are premixed, and the premixed materials are sent to a twin-screw extruder for extrusion granulation to obtain the alloy material.

[0018] Preferably, the parameters of the twin-screw extruder are:

[0019] Temperature settings: Zone 1 80±10℃, Zone 2 210±10℃, Zone 3 215±10℃, Zone 4 215±10℃, Zone 5 210±10℃, Zone 6 210±10℃, Zone 7 210±10℃, Zone 8 210±10℃, Zone 9 210±10℃, Die head 215±10℃; Main machine speed: 30±3hz; Main machine current: 75±20A; Feeding speed: 13±3hz; Vacuum: -0.07±0.03MPa.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] 1. The present invention uses the hydroxyl group on perfluorohexylethyl alcohol to perform a ring-opening reaction on 1-allyloxy-2,3-propylene oxide to obtain an intermediate A containing a double bond and a fluorocarbon chain; both silicon nitride and diatomaceous earth have a certain number of active hydroxyl groups on their surfaces, and the two are compounded for use, and their surfaces are modified by a silane coupling agent containing double bonds, and double bonds are introduced to obtain an intermediate B containing double bonds; due to the large difference in activity between the polymerization monomer intermediate A, intermediate B, and styrene, the present invention places the intermediate B at the interface of the two phases, uses an oxidation-reduction initiator to initiate emulsion polymerization at the interface, and finally successfully introduces the silicon nitride, diatomaceous earth, and fluorocarbon chains into the polymer to obtain a modified PS resin.

[0022] 2. Under the action of modified PS resin, the interaction force between the interfaces of ABS resin, modified PS resin and PP resin is enhanced, the crystallinity is improved, the mechanical properties of the alloy material are improved, and the erosion of the foaming agent is slowed down. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 This is a rendering of the alloy material obtained in Example 1 being prepared into a specimen and fixed on an ESCR fixture (before the corrosion experiment begins).

[0024] Figure 2 This is a diagram showing the effect of the alloy material obtained in Example 1 being prepared into a specimen for corrosion experiment. DETAILED DESCRIPTION

[0025] Unless otherwise specified, the raw materials and reagents used in the present invention are commercially available or can be prepared by known methods.

[0026] ABS resin: INEOS Styrolution GP22;

[0027] PP resin: Dushanzi Petrochemical T30S;

[0028] Compatibilizer: Sinopec SEBS;

[0029] Antioxidant 1076, 168: BASF;

[0030] Dispersant: Indonesia EBS B50;

[0031] The lubricant is: Italian calcium stearate;

[0032] Color powder: BASF;

[0033] Diatomaceous earth: Aladdin K592278;

[0034] Silicon nitride: Tianjin Hi-Tech New Materials, particle size 500nm.

[0035] In the present application, the blister-grade CABS alloy material means a blister-grade composite ABS alloy material, that is, an alloy material composed of ABS resin, modified PS resin, and PP resin.

[0036] Preparation Example 1

[0037] 119g of 1-allyloxy-2,3-propylene oxide was dispersed in 1L THF (tetrahydrofuran), the pH was adjusted to 9-10 with 0.5mol / L sodium hydroxide solution, 364g of perfluorohexylethyl alcohol was dispersed in 1L THF, and added dropwise to the above reaction system, refluxed for 5h, and dried to obtain intermediate A;

[0038] 100g of silicon nitride and 100g of diatomaceous earth were added to 1L of 70% ethanol aqueous solution, heated to 50°C with stirring, 10g of vinyl triethoxysilane was added, the reaction was stirred at 55°C for 2h, and dried to obtain intermediate B;

[0039] Under a nitrogen atmosphere, 20 g of Tween 80 and 5 L of deionized water were added to the reactor, and the mixture was stirred and dispersed evenly. 100 g of intermediate B and 10 g of Span 80 were ultrasonically dispersed in 2 L of cyclohexane, and then added to the above reactor, and the mixture was stirred and dispersed evenly. Finally, 500 g of styrene, 40 g of intermediate A, and 10 g of tert-butyl hydroperoxide were added to the reactor, emulsified at 40 ° C for 1 h, 15 g of ferrous chloride was added, and the polymerization reaction was carried out at 50 ° C for 6 h. Ethanol was added to break the emulsification, filtered, washed, and dried to obtain a modified PS resin.

[0040] Preparation Example 2

[0041] The difference between this preparation example and preparation example 1 is that:

[0042] Add 100 g of silicon nitride and 50 g of diatomaceous earth to 1 L of 70% by mass ethanol aqueous solution;

[0043] The rest is exactly the same as Preparation Example 1.

[0044] Preparation Example 3

[0045] The difference between this preparation example and preparation example 1 is that:

[0046] Add 50g of silicon nitride and 100g of diatomaceous earth to 1L of 70% by mass ethanol aqueous solution;

[0047] The rest is exactly the same as Preparation Example 1.

[0048] Preparation Example 4

[0049] The difference between this preparation example and preparation example 1 is that:

[0050] Add 100 g of silicon nitride and 0 g of diatomaceous earth to 1 L of 70% by mass ethanol aqueous solution;

[0051] The rest is exactly the same as Preparation Example 1.

[0052] Preparation Example 5

[0053] The difference between this preparation example and preparation example 1 is that:

[0054] Add 0g of silicon nitride and 100g of diatomaceous earth to 1L of 70% by mass ethanol aqueous solution;

[0055] The rest is exactly the same as Preparation Example 1.

[0056] Preparation Example 6

[0057] The difference between this preparation example and preparation example 1 is that:

[0058] Finally, 500 g of styrene, 0 g of intermediate A, and 10 g of tert-butyl hydroperoxide were added to the reactor and emulsified at 40 °C for 1 h;

[0059] The rest is exactly the same as Preparation Example 1. Example 1

[0060] A CABS alloy material for an extruded plate blister for a refrigerator liner, which is composed of 60 parts of ABS resin, 20 parts of modified PS resin (obtained in Preparation Example 1), 10 parts of PP resin, 10 parts of a compatibilizer, 0.2 parts of an antioxidant 1076, 0.3 parts of an antioxidant 168, 0.3 parts of a dispersant, 0.5 parts of a lubricant, and 1 part of a color powder, calculated by weight.

[0061] Premixing the materials in the above proportions, and feeding the premixed materials into a twin-screw extruder for extrusion and granulation to obtain the alloy material;

[0062] The parameters of the twin-screw extruder are: temperature setting: zone 1 80℃, zone 2 210℃, zone 3 215℃, zone 4 215℃, zone 5 210℃, zone 6 210℃, zone 7 210℃, zone 8 210℃, zone 9 210℃, die head 215℃; main engine speed: 32hz; main engine current: 80-90; feeding speed: 15hz; vacuum: -0.08MPa. Example 2

[0063] The difference between this example and Example 1 is that: 10 parts of modified PS resin (obtained in Preparation Example 1);

[0064] The rest is exactly the same as in Example 1. Example 3

[0065] The difference between this example and Example 1 is that: 30 parts of modified PS resin (obtained in Preparation Example 1);

[0066] The rest is exactly the same as in Example 1. Example 4

[0067] The difference between this example and Example 1 is that: 20 parts of modified PS resin (obtained in Preparation Example 2);

[0068] The rest is exactly the same as in Example 1. Example 5

[0069] The difference between this example and Example 1 is that: 20 parts of modified PS resin (obtained in Preparation Example 3);

[0070] The rest is exactly the same as in Example 1.

[0071] Comparative Example 1

[0072] The difference between this comparative example and Example 1 is that: 20 parts of modified PS resin (obtained in Preparation Example 4);

[0073] The rest is exactly the same as in Example 1.

[0074] Comparative Example 2

[0075] The difference between this comparative example and Example 1 is that: 20 parts of modified PS resin (obtained in Preparation Example 5);

[0076] The rest is exactly the same as in Example 1.

[0077] Comparative Example 3

[0078] The difference between this comparative example and Example 1 is that: 20 parts of modified PS resin (obtained in Preparation Example 6);

[0079] The rest is exactly the same as in Example 1.

[0080] Results and Testing

[0081] Foaming agent resistance test: The alloy material obtained in Example 1 was prepared into a spline and fixed to the ESCR mold. The ESCR bending strain was 2%. After fixing for 1 hour, it was placed in a pressure corrosion tank containing a foaming agent liquid (the foaming agent composition was: cyclopentane CP + isopentane IP + LBA). The temperature in the tank was 40±1°C and maintained for 3 hours (adjusted according to the corrosion of the spline). Note that the foaming agent liquid cannot contact the plastic spline; after the corrosion is completed, the pressure is released and the spline is taken out, straightened, and placed for 48 hours before the tensile strength test. The experimental process is shown in Figures 1 and 2.

[0082] Mechanical properties testing:

[0083] Tensile strength, elongation at break: GB / T1040.1-2018, test conditions: 50mm / min;

[0084] Impact strength: GB / T 1843-2008, test conditions: 5.5J; the results are shown in Table 1.

[0085] Table 1

[0086]

[0087] From Table 1 and Examples 1-5, it can be seen that the alloy material prepared by the present invention has excellent performance in tensile strength, impact strength, elongation at break, and tensile strength after foaming agent detection, and the performance is greatly improved compared with traditional ABS materials.

[0088] By comparing Example 1, Comparative Examples 1 and 2, it can be seen that diatomaceous earth and silicon nitride play a very important role in the performance of the alloy material. Regardless of the lack of diatomaceous earth (Comparative Example 1) or the lack of silicon nitride (Comparative Example 2), the performance of the alloy material is significantly reduced. However, when the two are used at the same time, the performance of the alloy material is significantly improved, with a synergistic enhancement effect.

[0089] By comparing Example 1 and Comparative Example 3, it can be seen that the introduction of fluorocarbon chains also has an important influence on the properties of the alloy material.

[0090] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A CABS alloy material for refrigerator liner, characterized in that: The composition is composed of 50-85 parts of ABS resin, 5-30 parts of modified PS resin, 5-30 parts of PP resin, 5-15 parts of compatibilizer and 0.1-5 parts of processing aid according to the weight ratio; The modified PS resin preparation method is as follows: 1-allyloxy-2,3-propylene oxide was dispersed in THF, the pH was adjusted to 9-10 with sodium hydroxide solution, perfluorohexylethyl alcohol was dispersed in THF, added dropwise to the above reaction system, refluxed, and dried to obtain intermediate A; The silicon nitride, diatomaceous earth was added to an aqueous ethanol solution, heated with stirring, vinyl triethoxysilane was added, the reaction was stirred, and dried to obtain intermediate B; Under nitrogen atmosphere, Tween 80 and deionized water were added into the reaction kettle, stirred and dispersed evenly, intermediate B and Span 80 were ultrasonically dispersed in cyclohexane, and then added into the above reaction kettle, stirred and dispersed evenly, finally styrene, intermediate A and tert-butyl hydroperoxide were added into the reaction kettle, emulsified, ferrous chloride was added, polymerization reaction was carried out, ethanol was added to break the emulsion, filtered, washed and dried to obtain modified PS resin; The molar ratio of 1-allyloxy-2,3-propylene oxide and perfluorohexylethyl alcohol is (1-1.1): 1; The mass ratio of silicon nitride, diatomaceous earth and vinyl triethoxysilane is 1: (0.5-2): (0.05-0.15); The mass ratio of Tween 80, intermediate B, Span 80, styrene, intermediate A, tert-butyl hydroperoxide and ferrous chloride is (10-30): (80-120): (5-15): (400-600): (30-50): (5-15): (10-20).

2. The CABS alloy material for refrigerator liner according to claim 1, characterized in that: The concentration of the sodium hydroxide solution is 0.1-1 mol / L.

3. The CABS alloy material for refrigerator liner according to claim 1, characterized in that: The mass concentration of the ethanol aqueous solution is 60%-80%.

4. The CABS alloy material for refrigerator liner according to claim 1, characterized in that: The processing aid is selected from any one or more of antioxidants, dispersants, lubricants and toners.

5. The method for preparing the alloy material according to any one of claims 1 to 4, characterized in that: The steps include: ABS resin, modified PS resin, PP resin, compatibilizer and processing aid are premixed, and the premixed materials are sent to a twin-screw extruder for extrusion granulation to obtain the alloy material.

6. The method for preparing the alloy material according to claim 5, characterized in that: The parameters of the twin-screw extruder are: temperature setting: zone 1 80±10℃, zone 2 210±10℃, zone 3 215±10℃, zone 4 215±10℃, zone 5 210±10℃, zone 6 210±10℃, zone 7 210±10℃, zone 8 210±10℃, zone 9 210±10℃, die head 215±10℃; main engine speed: 30±3hz; main engine current: 75±20A; feeding speed: 13±3hz; vacuum: -0.07±0.03MPa.