Method for removing slag from remelting of nickel-based high-temperature alloy
By adding Ca, Ba, and Sr during the remelting process of nickel-based superalloys and combining it with electromagnetic stirring, the problem of removing slag from the remelting of nickel-based superalloys was solved, achieving efficient and rapid purification and improving alloy purity and production efficiency.
Patent Information
- Application Number
- CN202411161969.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-08-23
AI Technical Summary
Existing technologies are insufficient to efficiently and quickly remove slag generated during the remelting of nickel-based superalloys, leading to an increased risk of alloy melt contamination and affecting alloy purity and production efficiency.
In the vacuum induction melting process, elemental metals Ca, Ba, and Sr are added to the nickel-based superalloy melt and combined with electromagnetic stirring. The low vapor pressure and strong oxygen absorption capacity of these metals are used to cause the slag to react with the crucible wall to form oxides, thus quickly removing the slag.
It effectively reduces slag formation, improves alloy purity, lowers production costs, meets the requirements for service in special environments, and is suitable for DD series and DZ series nickel-based high-temperature alloys.
Smart Images

Figure CN118685657B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of nickel-based high-temperature alloy smelting and purification, and in particular relates to a method for removing remelting slag of a nickel-based high-temperature alloy. Background Art
[0002] As we all know, the application of nickel-based superalloys is of great importance and significance, and it provides a key material foundation for modern engineering technology. Nickel-based superalloys have shown excellent performance in high temperature, high pressure and corrosive environments, and can be widely used in aero engines, gas turbines, chemical reactors and nuclear reactors. The high temperature resistance, oxidation resistance, mechanical properties and corrosion resistance of nickel-based superalloys enable them to promote the advancement of high-temperature processes and technologies, extend the service life of equipment, improve work efficiency, reduce energy consumption and environmental impact, and thus promote the sustainable development of modern society.
[0003] The purity level of nickel-based superalloys is one of the important parameters for evaluating their excellent performance, and is also one of the important indicators for measuring the manufacturing level of nickel-based superalloys. The presence and distribution of inclusions in nickel-based superalloys directly damage the high-temperature application and structural stability of the material. Therefore, studying the purification technology of nickel-based superalloys is of great significance for improving the stability and performance of the alloy.
[0004] The purification of nickel-based high-temperature alloys is achieved during the smelting stage. To prepare nickel-based high-temperature alloys, first prepare nickel-based high-temperature alloy master alloy ingots, and then remelt the nickel-based high-temperature alloy master alloy ingots to obtain nickel-based high-temperature alloys. For the preparation of nickel-based high-temperature alloy master alloy ingots, alloy purification is mainly achieved by deoxidation and desulfurization; for the remelting of nickel-based high-temperature alloy master alloy ingots, alloy purification is mainly achieved by removing the scum generated during the remelting process. Regarding the remelting of nickel-based high-temperature alloy master alloy ingots (that is, the remelting of nickel-based high-temperature alloys), during the vacuum induction melting process, the nickel-based high-temperature alloy melt directly contacts the refractory crucible. Due to the scouring of the crucible refractory by the alloy melt, the refractory material will be melted into the alloy melt. The oxygen decomposed by the refractory material forms oxides with the active elements in the alloy melt. During the melting process, due to electromagnetic stirring, the oxide floats up and mixes with the metal to form a metal film of a certain thickness, which is the scum.
[0005] At present, in order to remove the scum generated in the remelting process, the scum is generally destroyed by rapidly stirring the alloy melt by increasing the melting temperature and accelerating the electromagnetic stirring, and then the scum is melted into the alloy melt. This undoubtedly intensifies the reaction between the alloy melt and the refractory material of the crucible, prolongs the processing time of alloy smelting, and increases the risk of inclusion contamination in the alloy melt. Therefore, it is necessary to develop a method for removing the remelting scum of nickel-based high-temperature alloys, so that the nickel-based high-temperature alloys can be purified efficiently and quickly during the remelting process.
[0006] The invention patent with application publication number CN117385214A discloses a method for deoxidation and desulfurization of a nickel-based high-temperature alloy based on a non-calcium refractory crucible. The method adopts a non-calcium refractory crucible, melts the nickel-based high-temperature alloy in a vacuum induction melting furnace, and adds metal elements to achieve deoxidation and desulfurization. The method comprises the following steps: placing the non-calcium refractory crucible in a vacuum induction melting furnace, and placing the nickel-based high-temperature alloy in the non-calcium refractory crucible; evacuating the furnace chamber to a certain vacuum degree, heating the furnace chamber to a smelting temperature, and then smelting and refining; adding metal element Y to the nickel-based high-temperature alloy during the evacuation, smelting or refining process; adding metal elements Ba and Ca to the nickel-based high-temperature alloy during the refining process; and completing the deoxidation and desulfurization of the nickel-based high-temperature alloy after the refining is completed. This technical solution achieves deoxidation and desulfurization of nickel-based high-temperature alloys by adding metal element Y during the smelting process and adding metal element Ba and Ca during the refining process. This technical solution is suitable for deoxidation and desulfurization of nickel-based high-temperature alloy master alloy ingots, but is not suitable for removing remelting slag of nickel-based high-temperature alloys.
[0007] The invention patent with application publication number CN117383950A discloses a non-calcium refractory crucible for desulfurization of nickel-based high-temperature alloy and a preparation method thereof. The non-calcium refractory crucible is made of a non-calcium refractory material, which is generated by the reaction of BaO, SrO and ZrO2 at high temperature. The compound generated by the reaction is Ba x Sr 1-x ZrO3; using the prepared non-calcium refractory crucible, smelting the nickel-based high-temperature alloy in a vacuum induction melting furnace to achieve desulfurization, comprising the following steps: placing the non-calcium refractory crucible in a vacuum induction melting furnace, and placing the nickel-based high-temperature alloy in the non-calcium refractory crucible; closing the vacuum induction melting furnace, evacuating the furnace chamber to 1×10 -3 -10Pa vacuum; while maintaining the vacuum, heat the furnace chamber to the melting temperature, and then melt and refine the nickel-based high-temperature alloy. After the refining is completed, the nickel-based high-temperature alloy can be desulfurized. This technical solution realizes the desulfurization of nickel-based high-temperature alloys through non-calcium refractory crucibles. Ba, Ca and Sr are added when preparing non-calcium refractory crucibles, instead of adding Ba, Ca and Sr during the smelting process. Therefore, this technical solution is not suitable for the efficient and rapid removal of remelting slag of nickel-based high-temperature alloys. Summary of the invention
[0008] In order to solve the problems existing in the prior art, the present invention provides a method for removing remelting slag of a nickel-based high-temperature alloy, and the removal method comprises the following steps in order:
[0009] Step 1: placing a nickel-based high-temperature alloy master alloy ingot in a crucible in a vacuum induction melting furnace, closing the vacuum induction melting furnace, and evacuating the furnace chamber to a certain vacuum degree;
[0010] Step 2: heating the furnace chamber while maintaining a certain vacuum degree to melt the nickel-based high-temperature alloy master alloy ingot. During the melting process, a feeder is used to feed metal element Ca into the alloy melt and electromagnetic stirring is performed. When the temperature in the furnace chamber rises to a certain temperature, the nickel-based high-temperature alloy master alloy ingot is completely melted, and a layer of slag is generated on the surface of the alloy melt.
[0011] Step 3: After the nickel-based high-temperature alloy master alloy ingot is completely melted, the smelting stage is entered. In the smelting stage, a feeder is used to sequentially feed metal elements Ca, Ba, and Sr into the alloy melt and electromagnetic stirring is performed. During the electromagnetic stirring process, the scum on the surface of the alloy melt can be quickly removed. At this time, the scum on the surface of the alloy melt quickly gathers at the circumferential position where the surface of the alloy melt contacts the crucible wall;
[0012] Step 4: Casting products using nickel-based high-temperature alloy after removing slag.
[0013] Preferably, in step one, the oxygen content in the nickel-based high-temperature alloy master alloy ingot does not exceed 10ppm, and the sulfur content does not exceed 5ppm; the material of the crucible is an oxide refractory material, and the oxide is any one of magnesium oxide, aluminum oxide, silicon oxide, a mixture of magnesium oxide and aluminum oxide, a mixture of aluminum oxide and silicon oxide, zirconium oxide, and barium zirconate; and the vacuum degree in the furnace chamber does not exceed 20Pa.
[0014] In any of the above schemes, it is preferred that in step 2, the vacuum degree in the furnace chamber is maintained at no more than 20Pa, and the temperature is increased from room temperature to 850°C at a heating rate of 80-100°C / min, and kept warm for 30-60s; after the insulation is completed, argon gas is introduced into the furnace chamber with an argon gas flow rate of 0.1-0.15 MPa / min, and then the metal element Ca is added to the alloy melt within 10s; the temperature is continued to be increased from 850°C to 1430-1550°C at a heating rate of 100-150°C / min, and kept warm for 30-60s, at which time the nickel-based high-temperature alloy master alloy ingot is completely melted.
[0015] In any of the above schemes, it is preferred that in step three, during the smelting stage, argon gas is kept flowing into the furnace chamber with an argon gas flow rate of 0.15-0.25 MPa / min, and metal elements Ca, Ba, and Sr are added to the alloy melt in sequence, with the time interval between the addition of the three metal elements not exceeding 10s; after the addition of the three metal elements is completed, electromagnetic stirring is performed for 1-2 minutes, and then the furnace chamber is evacuated to a vacuum degree of no more than 20Pa.
[0016] In any of the above schemes, preferably, in step 2 and step 3, the total mass of the metal elements Ca, Ba, and Sr added to the alloy melt is 1-4wt% of the mass of the nickel-based high-temperature alloy master alloy ingot.
[0017] In any of the above schemes, it is preferred that in step 2 and step 3, the mass of the metal elements Ca, Ba, and Sr added to the alloy melt accounts for 20-30wt%, 10-20wt%, and 50-70wt% of the total mass of the metal elements Ca, Ba, and Sr, respectively.
[0018] In any of the above schemes, preferably, in step 2, the mass of the metal element Ca added to the alloy melt is 30-50% of the total mass of the metal element Ca.
[0019] In any of the above schemes, preferably, in step three, the mass of the metal element Ca added to the alloy melt is 50-70% of the total mass of the metal element Ca.
[0020] In any of the above schemes, it is preferred that in step 2 and step 3, the metal elements Ca, Ba, and Sr added to the alloy melt are in block or filament form.
[0021] The vacuum induction melting furnace, vacuum pump, crucible, etc. used in the present invention can select existing equipment according to actual use conditions, and no special requirements are made on the equipment model. The pouring equipment and pouring process used for subsequent pouring can adopt traditional technologies. In the present invention, the timing, amount, and order of adding the metal elements Ca, Ba, and Sr are very critical, and combined with the synergistic effect of other process parameters, the nickel-based high-temperature alloy can finally achieve efficient and rapid removal of slag during the remelting process.
[0022] In step 2, when the temperature in the furnace chamber reaches 850°C, a portion of metal element Ca needs to be added. Since the melting point of Ca is 842°C, a portion of metal element Ca is added in advance at 850°C, and the molten Ca can be used to form a liquid to cover the contact part between the alloy and the crucible, so as to effectively control the contact between the alloy and the crucible substrate at the moment of melting in advance, wherein Ca will instantly participate in the reaction between the melt and the crucible, thereby inhibiting the reaction between the two.
[0023] In addition, before adding metallic element Ca, argon gas needs to be introduced into the furnace chamber. This is because metallic element Ca is highly volatile under vacuum. The introduction of argon gas is beneficial to inhibit the volatilization of the Ca element and promote the participation of the Ca element in the interface reaction between the alloy melt and the crucible.
[0024] In step three, during the smelting stage, metal elements Ca, Ba, and Sr need to be added to the alloy melt. For the reaction between the alloy melt and the crucible, the physical dissolution of the crucible is the main one, and the dissolved O will quickly react with Ca, Ba, and Sr to form oxides, which in turn react with the impurity phase Al2O3 in the alloy to generate a low-melting-point slag phase, which in turn causes the impurities to float to the liquid surface quickly, and at the same time, they adhere to the inner wall of the crucible under the action of electromagnetic stirring, playing a role in quickly removing slag.
[0025] The method for removing remelting slag of nickel-based high-temperature alloy of the present invention has the following beneficial effects:
[0026] (1) The present invention adds three alkaline earth metals, Ca, Ba and Sr, to the high-temperature alloy melt. The three alkaline earth metals have a relatively low vapor pressure and evaporate rapidly on the surface of the liquid, thereby destroying the metal slag film on the surface. At the same time, the three alkaline earth metals have a relatively strong oxygen absorption capacity. When the melt is stirred, they form composite oxides with inclusions in the melt and are adsorbed on the inner wall of the high-temperature alloy melting crucible. Alternatively, the formed composite oxides are adsorbed on the edge of the crucible in contact with the melt through stirring to form a slag line, thereby reducing the amount of slag generated in the alloy melt and the inclusions in the alloy melt.
[0027] (2) The present invention does not introduce new slag removal equipment and means, reducing the introduction of solid and gas phase impurities. Compared with the slag removal method of refining the alloy melt, the present invention can quickly remove slag, reduce the possibility of slag entering the alloy melt and causing pollution, has the advantages of short time consumption and reduced slag pollution, reduces the production cost of nickel-based high-temperature alloys, and improves the production quality and efficiency of nickel-based high-temperature alloys.
[0028] (3) In order to solve the technical problem that the scum produced in the prior art is involved in the alloy melt due to the interface effect between the crucible refractory material and the alloy melt during the smelting of nickel-based high-temperature alloys, the present invention adopts the addition of metal elements Ca, Ba, and Sr to improve the amount of scum in the smelting process of nickel-based high-temperature alloys, improve the purity of the smelted alloy, and enable the produced high-temperature alloy to meet the service requirements of special environments. (4) The present invention solves the technical problems that hinder the smelting of nickel-based high-temperature alloys, and lays a foundation for the efficient preparation of high-quality nickel-based high-temperature alloys. The scum removal method is particularly suitable for DD series and DZ series nickel-based high-temperature alloys. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 A flow chart of a preferred embodiment of a method for removing remelting slag of a nickel-based high-temperature alloy according to the present invention;
[0030] Figure 2 for Figure 1 A photograph of scum film formation during scum removal in the illustrated embodiment;
[0031] Figure 3 for Figure 1 A photograph showing the gradual removal of scum during the scum removal process of the illustrated embodiment;
[0032] Figure 4 for Figure 1 Photos of scum film removal during scum removal in the illustrated embodiment;
[0033] Figure 5 A photograph of scum filming during scum removal according to another preferred embodiment of the method for removing scum from nickel-based high-temperature alloy remelting according to the present invention;
[0034] Figure 6 for Figure 5 A photograph showing the gradual removal of scum during the scum removal process of the illustrated embodiment;
[0035] Figure 7 for Figure 5 Photos of scum film removal during scum removal in the illustrated embodiment;
[0036] Figure 8 A photograph of scum filming during scum removal according to another preferred embodiment of the method for removing scum from nickel-based high-temperature alloy remelting according to the present invention;
[0037] Fig. 9 for Figure 8 A photograph showing the gradual removal of scum during the scum removal process of the illustrated embodiment;
[0038] Fig.10 for Figure 8 A photograph of scum film cleaning during the scum removal process of the illustrated embodiment. DETAILED DESCRIPTION
[0039] In order to further understand the content of the present invention, the present invention will be described in detail below in conjunction with specific embodiments.
[0040] Embodiment 1:
[0041] like Figure 1 As shown, according to a preferred embodiment of the method for removing remelting slag of nickel-based high-temperature alloy of the present invention, the removal method comprises the following steps in chronological order:
[0042] Step 1: placing a nickel-based high-temperature alloy master alloy ingot in a crucible in a vacuum induction melting furnace, closing the vacuum induction melting furnace, and evacuating the furnace chamber to a certain vacuum degree;
[0043] Step 2: heating the furnace chamber while maintaining a certain vacuum degree to melt the nickel-based high-temperature alloy master alloy ingot. During the melting process, a feeder is used to feed metal element Ca into the alloy melt and electromagnetic stirring is performed. When the temperature in the furnace chamber rises to a certain temperature, the nickel-based high-temperature alloy master alloy ingot is completely melted, and a layer of slag is generated on the surface of the alloy melt.
[0044] Step 3: After the nickel-based high-temperature alloy master alloy ingot is completely melted, the smelting stage is entered. In the smelting stage, a feeder is used to sequentially feed metal elements Ca, Ba, and Sr into the alloy melt and electromagnetic stirring is performed. During the electromagnetic stirring process, the scum on the surface of the alloy melt can be quickly removed. At this time, the scum on the surface of the alloy melt quickly gathers at the circumferential position where the surface of the alloy melt contacts the crucible wall;
[0045] Step 4: Casting products using nickel-based high-temperature alloy after removing slag.
[0046] In step one, the grade of the nickel-based high-temperature alloy is DD419, the oxygen content in the nickel-based high-temperature alloy master alloy ingot does not exceed 10ppm, and the sulfur content does not exceed 5ppm; the material of the crucible is an oxide refractory material, and the oxide is a mixture of magnesium oxide and aluminum oxide; the vacuum degree in the furnace chamber is 20Pa.
[0047] In step 2, the vacuum degree in the furnace chamber is maintained at 20 Pa, and the temperature is increased from room temperature to 850°C at a heating rate of 90°C / min, and kept warm for 45 seconds; after the insulation is completed, argon gas is introduced into the furnace chamber with an argon gas flow rate of 0.12 MPa / min, and then metal element Ca is added to the alloy melt within 10 seconds; the temperature is continued to be increased from 850°C to 1490°C at a heating rate of 125°C / min, and kept warm for 45 seconds, at which time the nickel-based high-temperature alloy master alloy ingot is completely melted.
[0048] In step three, during the smelting stage, argon gas is kept flowing into the furnace chamber with an argon flow rate of 0.2 MPa / min, and metal elements Ca, Ba, and Sr are added to the alloy melt in turn. The time interval between the addition of the three metal elements is 10 s. After the addition of the three metal elements is completed, electromagnetic stirring is performed for 1.5 minutes, and then the vacuum degree in the furnace chamber is evacuated to 20 Pa.
[0049] In step 2 and step 3, the total mass of the metal elements Ca, Ba, and Sr added to the alloy melt is 2.5wt% of the mass of the nickel-based high-temperature alloy master alloy ingot. The mass of the metal elements Ca, Ba, and Sr added to the alloy melt accounts for 25wt%, 15wt%, and 60wt% of the total mass of the metal elements Ca, Ba, and Sr, respectively. The metal elements Ca, Ba, and Sr added to the alloy melt are all in block form.
[0050] In step 2, the mass of the metallic element Ca added to the alloy melt is 40% of the total mass of the metallic element Ca.
[0051] In step 3, the mass of the metallic element Ca added to the alloy melt is 60% of the total mass of the metallic element Ca.
[0052] The vacuum induction melting furnace, vacuum pump, crucible, etc. used in this embodiment can select existing equipment according to actual use conditions, and no special requirements are made on the equipment model. The pouring equipment and pouring process used in subsequent pouring can adopt traditional technologies. In this embodiment, the timing, amount, and order of adding the metal elements Ca, Ba, and Sr are very critical, and combined with the synergistic effect of other process parameters, the nickel-based high-temperature alloy can finally achieve efficient and rapid removal of slag during the remelting process.
[0053] In step 2, when the temperature in the furnace chamber reaches 850°C, a portion of metal element Ca needs to be added, because the melting point of Ca is 842°C. By adding a portion of metal element Ca in advance at 850°C, the molten Ca can be used to form a liquid to cover the contact part between the alloy and the crucible, which can effectively control the contact between the alloy and the crucible matrix at the moment of melting in advance, wherein Ca will instantly participate in the reaction between the melt and the crucible, thereby inhibiting the reaction between the two. In addition, before adding metal element Ca, argon gas needs to be introduced into the furnace chamber first. This is because metal element Ca has strong volatility under vacuum, and the introduction of argon gas is conducive to inhibiting the volatilization of the Ca element and promoting the participation of the Ca element in the interface reaction between the alloy melt and the crucible.
[0054] In step three, during the smelting stage, metal elements Ca, Ba, and Sr need to be added to the alloy melt. For the reaction between the alloy melt and the crucible, the physical dissolution of the crucible is the main one, and the dissolved O will quickly react with Ca, Ba, and Sr to form oxides, which in turn react with the impurity phase Al2O3 in the alloy to generate a low-melting-point slag phase, which in turn causes the impurities to float to the liquid surface quickly, and at the same time, they adhere to the inner wall of the crucible under the action of electromagnetic stirring, playing a role in quickly removing slag.
[0055] The process of removing scum in this embodiment is as follows: Figure 2 As shown, (a) is a photo of scum filming, (b) is a photo of scum gradually being removed, and (c) is a photo of scum filming. Figure 2 It can be clearly seen that a layer of slag is initially formed on the surface of the melt. After the metal elements Ca, Ba, and Sr are added, the slag gradually moves toward the crucible wall and eventually gathers at the circumferential position where the melt surface contacts the crucible wall, and the melt surface becomes clear.
[0056] The method for removing slag from remelting nickel-based high-temperature alloys in this embodiment has the following beneficial effects: (1) Three alkaline earth metals, Ca, Ba, and Sr, are added to the high-temperature alloy melt. These three alkaline earth metals have a low vapor pressure and evaporate rapidly on the surface of the liquid, thereby destroying the metal slag film on the surface. At the same time, these three alkaline earth metals have a strong oxygen absorption capacity. Under the stirring of the melt, they form composite oxides with the inclusions in the melt, which are adsorbed on the inner wall of the high-temperature alloy melting crucible or adsorbed on the edge of the crucible in contact with the melt through stirring to form a slag line, thereby reducing the amount of slag generated in the alloy melt and the inclusions in the alloy melt. (2) No new slag removal equipment and means are introduced, which reduces the introduction of solid and gas phase impurities. At the same time, the slag can be removed quickly, reducing the possibility of slag entering the alloy melt and causing pollution, and has the advantages of short time consumption and reduced slag pollution. (3) The addition of metal elements Ca, Ba, and Sr is used to improve the amount of slag during the smelting process of nickel-based high-temperature alloys, improve the purity of the molten alloy, and enable the produced high-temperature alloys to meet the service requirements of special environments.
[0057] Embodiment 2:
[0058] According to another preferred embodiment of the method for removing remelting slag of nickel-based high-temperature alloy of the present invention, the process steps, the equipment used, the technical principle and the beneficial effects are basically the same as those of the first embodiment, except that:
[0059] In step one, the grade of the nickel-based high-temperature alloy is DD419, the oxygen content in the nickel-based high-temperature alloy master alloy ingot does not exceed 10ppm, and the sulfur content does not exceed 5ppm; the material of the crucible is an oxide refractory material, and the oxide is a mixture of aluminum oxide and silicon oxide; the vacuum degree in the furnace chamber is 20Pa.
[0060] In step 2, the vacuum degree in the furnace chamber is maintained at 20 Pa, and the temperature is increased from room temperature to 850°C at a heating rate of 80°C / min, and kept warm for 60 seconds; after the insulation is completed, argon gas is introduced into the furnace chamber with an argon gas flow rate of 0.1 MPa / min, and then metal element Ca is added to the alloy melt within 10 seconds; the temperature is continued to be increased from 850°C to 1550°C at a heating rate of 100°C / min, and kept warm for 30 seconds, at which time the nickel-based high-temperature alloy master alloy ingot is completely melted.
[0061] In step three, during the smelting stage, argon gas is kept flowing into the furnace chamber with an argon flow rate of 0.15 MPa / min, and metal elements Ca, Ba, and Sr are added to the alloy melt in turn. The time interval between the addition of the three metal elements is 10 s. After the addition of the three metal elements, electromagnetic stirring is performed for 1 minute, and then the vacuum degree in the furnace chamber is evacuated to 20 Pa.
[0062] In step 2 and step 3, the total mass of the metal elements Ca, Ba, and Sr added to the alloy melt is 1wt% of the mass of the nickel-based high-temperature alloy master alloy ingot. The mass of the metal elements Ca, Ba, and Sr added to the alloy melt accounts for 20wt%, 10wt%, and 70wt% of the total mass of the metal elements Ca, Ba, and Sr, respectively. The metal elements Ca, Ba, and Sr added to the alloy melt are all in block form.
[0063] In step 2, the mass of the metallic element Ca added to the alloy melt is 30% of the total mass of the metallic element Ca.
[0064] In step 3, the mass of the metallic element Ca added to the alloy melt is 70% of the total mass of the metallic element Ca.
[0065] The process of removing scum in this embodiment is as follows: Figure 3 As shown, (a) is a photo of scum filming, (b) is a photo of scum gradually being removed, and (c) is a photo of scum filming. Figure 3 It can be clearly seen that a layer of slag is initially formed on the surface of the melt. After the metal elements Ca, Ba, and Sr are added, the slag gradually moves toward the crucible wall and eventually gathers at the circumferential position where the melt surface contacts the crucible wall, and the melt surface becomes clear.
[0066] Embodiment three:
[0067] According to another preferred embodiment of the method for removing remelting slag of nickel-based high-temperature alloy of the present invention, the process steps, the equipment used, the technical principle and the beneficial effects are basically the same as those of the first embodiment, except that:
[0068] In step one, the grade of the nickel-based high-temperature alloy is DD419, the oxygen content in the nickel-based high-temperature alloy master alloy ingot does not exceed 10ppm, and the sulfur content does not exceed 5ppm; the material of the crucible is an oxide refractory material, and the oxide is a mixture of aluminum oxide and silicon oxide; the vacuum degree in the furnace chamber is 20Pa.
[0069] In step 2, the vacuum degree in the furnace chamber is maintained at 20 Pa, and the temperature is increased from room temperature to 850°C at a heating rate of 100°C / min, and kept warm for 30 seconds; after the insulation is completed, argon gas is introduced into the furnace chamber with an argon gas flow rate of 0.15 MPa / min, and then metal element Ca is added to the alloy melt within 10 seconds; the temperature is continued to be increased from 850°C to 1430°C at a heating rate of 150°C / min, and kept warm for 60 seconds, at which time the nickel-based high-temperature alloy master alloy ingot is completely melted.
[0070] In step three, during the smelting stage, argon gas is kept flowing into the furnace chamber with an argon flow rate of 0.25 MPa / min, and metal elements Ca, Ba, and Sr are added to the alloy melt in turn. The time interval between the addition of the three metal elements is 10 s. After the addition of the three metal elements is completed, electromagnetic stirring is performed for 2 minutes, and then the vacuum degree in the furnace chamber is evacuated to 20 Pa.
[0071] In step 2 and step 3, the total mass of the metal elements Ca, Ba, and Sr added to the alloy melt is 4wt% of the mass of the nickel-based high-temperature alloy master alloy ingot. The mass of the metal elements Ca, Ba, and Sr added to the alloy melt accounts for 30wt%, 20wt%, and 50wt% of the total mass of the metal elements Ca, Ba, and Sr, respectively. The metal elements Ca, Ba, and Sr added to the alloy melt are all in block form.
[0072] In step 2, the mass of the metallic element Ca added to the alloy melt is 50% of the total mass of the metallic element Ca.
[0073] In step 3, the mass of the metallic element Ca added to the alloy melt is 50% of the total mass of the metallic element Ca.
[0074] The process of removing scum in this embodiment is as follows: Figure 4 As shown, (a) is a photo of scum filming, (b) is a photo of scum gradually being removed, and (c) is a photo of scum filming. Figure 4 It can be clearly seen that a layer of slag is initially formed on the surface of the melt. After the metal elements Ca, Ba, and Sr are added, the slag gradually moves toward the crucible wall and eventually gathers at the circumferential position where the melt surface contacts the crucible wall, and the melt surface becomes clear.
[0075] Comparative Example:
[0076] The nickel-based high-temperature alloy master alloy ingot is placed in a crucible in a vacuum induction melting furnace for melting. The alloy grade is DD419. The oxygen content in the master alloy ingot does not exceed 10ppm, and the sulfur content does not exceed 5ppm. The crucible material is a mixture of aluminum oxide and silicon oxide. The vacuum degree in the furnace chamber is 20Pa, and the melting temperature is 1490°C. Since no metal elements Ca, Ba, and Sr are added during the melting process, a layer of slag is generated on the surface of the melt. After electromagnetic stirring, the slag enters the alloy melt again, causing serious contamination of the alloy melt. The OTS fully automatic non-metallic inclusion analysis system in steel is used to perform inclusion tests (mainly testing oxides) on the metal samples of the above three embodiments and comparative examples. The test environment and test conditions are the same, and the test results are shown in Tables 1-4.
[0077]
[0078]
[0079]
[0080]
[0081] It can be seen from Tables 1 to 4 that after adding metal elements Ca, Ba, and Sr during the smelting process, the number of oxide particles in the melt is significantly reduced, because a part of the inclusions gather with the slag to the circumferential position where the melt surface contacts the crucible wall, and only a small amount of inclusions enters the melt; for the alloy melt without adding metal elements Ca, Ba, and Sr, all the oxide particles enter the alloy melt, causing serious pollution to the alloy melt.
[0082] Special note: The technical solution of the present invention involves many parameters, and the synergistic effects between the various parameters need to be comprehensively considered to obtain the beneficial effects and significant progress of the present invention. Moreover, the value ranges of the various parameters in the technical solution are obtained after a large number of experiments. For each parameter and the combination of each parameter, the inventor has recorded a large amount of experimental data. Due to space limitations, the specific experimental data will not be disclosed here.
[0083] It is not difficult for those skilled in the art to understand that the method for removing remelting slag of nickel-based high-temperature alloy of the present invention includes any combination of the invention content and specific implementation methods of the above-mentioned invention specification and the various parts shown in the drawings. Due to the limited space and to make the specification concise, the various schemes composed of these combinations are not described one by one. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for removing remelting slag of nickel-based high-temperature alloy, Features: The removal method comprises the following steps in chronological order: Step 1: placing a nickel-based high-temperature alloy master alloy ingot in a crucible in a vacuum induction melting furnace, closing the vacuum induction melting furnace, and evacuating the furnace chamber to a certain vacuum degree; Step 2: heating the furnace chamber while maintaining a certain vacuum degree to melt the nickel-based high-temperature alloy master alloy ingot. During the melting process, a feeder is used to feed metal element Ca into the alloy melt and electromagnetic stirring is performed. When the temperature in the furnace chamber rises to a certain temperature, the nickel-based high-temperature alloy master alloy ingot is completely melted, and a layer of slag is generated on the surface of the alloy melt. Step 3: After the nickel-based high-temperature alloy master alloy ingot is completely melted, the smelting stage is entered. In the smelting stage, a feeder is used to sequentially feed metal elements Ca, Ba, and Sr into the alloy melt and electromagnetic stirring is performed. During the electromagnetic stirring process, the scum on the surface of the alloy melt can be quickly removed. At this time, the scum on the surface of the alloy melt quickly gathers at the circumferential position where the surface of the alloy melt contacts the crucible wall; Step 4: Casting products using nickel-based high-temperature alloy after removing slag; In step 1, the vacuum degree in the furnace chamber does not exceed 20Pa; In step 2, the vacuum degree in the furnace chamber is maintained at no more than 20 Pa, and the temperature is increased from room temperature to 850°C at a heating rate of 80-100°C / min, and kept at this temperature for 30-60s; After the insulation is completed, argon gas is introduced into the furnace chamber with an argon gas flow rate of 0.1-0.15 MPa / min, and then metal element Ca is added to the alloy melt within 10 seconds; the temperature is continued to be raised from 850°C to 1430-1550°C at a heating rate of 100-150°C / min, and the temperature is kept for 30-60 seconds, at which time the nickel-based high-temperature alloy master alloy ingot is completely melted; In step 3, during the smelting stage, argon gas is kept flowing into the furnace chamber, and the argon gas flow rate is 0.15-0.25 MPa / min, and metal elements Ca, Ba, and Sr are added to the alloy melt in sequence, and the time interval between the addition of the three metal elements is no more than 10s; after the addition of the three metal elements is completed, electromagnetic stirring is performed for 1-2 minutes, and then the vacuum in the furnace chamber is evacuated to a vacuum degree of no more than 20Pa; In step 2 and step 3, the total mass of the metal elements Ca, Ba, and Sr added to the alloy melt is 1-4wt% of the mass of the nickel-based high-temperature alloy master alloy ingot; the mass of the metal elements Ca, Ba, and Sr added to the alloy melt accounts for 20-30wt%, 10-20wt%, and 50-70wt% of the total mass of the metal elements Ca, Ba, and Sr, respectively; In step 2, the mass of the metallic element Ca added to the alloy melt is 30-50% of the total mass of the metallic element Ca; in step 3, the mass of the metallic element Ca added to the alloy melt is 50-70% of the total mass of the metallic element Ca.
2. The method for removing remelting slag of nickel-based high-temperature alloy according to claim 1, Features: In step one, the oxygen content in the nickel-based high-temperature alloy master alloy ingot does not exceed 10ppm, and the sulfur content does not exceed 5ppm; the material of the crucible is an oxide refractory material, and the oxide is any one of magnesium oxide, aluminum oxide, silicon oxide, a mixture of magnesium oxide and aluminum oxide, a mixture of aluminum oxide and silicon oxide, zirconium oxide, and barium zirconate.
3. The method for removing remelting slag of nickel-based high-temperature alloy according to claim 2, Features: In step 2 and step 3, the metal elements Ca, Ba and Sr added to the alloy melt are all in block or wire form.
Citation Information