Highly sensitive and wide linear flexible strain sensor based on composite gradient structure
By adopting a composite gradient structure in a flexible strain sensor, combining the compatible modification of PEDOT:PSS and PDMS and triethylene glycol treatment to improve conductivity, ensuring stable connection of the electrode structure, solving the sensor sensitivity, linear range and stability between sensor sensitivity, linear range and stability The balance problem realizes high sensitivity, wide linearity and long life sensor design.
Patent Information
- Application Number
- CN202411170417.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-08-26
AI Technical Summary
Existing flexible strain sensors are difficult to combine high sensitivity, wide linear range and high stability, and the poor heterogeneous interface bonding between the conductive strain layer and the substrate leads to poor stability. Unstable electrode connections affect the reliability and service life of the sensor. .
Highly sensitive wide linear flexible strain sensor using composite gradient structure, including low-conductive inner core and high-conductive film layer. The low-conductive inner core is compatible with PEDOT:PSS and PDMS, and the high-conductive film layer is compatible with triethylene glycol and ZnCl2 The treatment improves conductivity, and the electrode structure ensures stable connections through carbon fiber fixing junctions and conductive adhesives.
The high sensitivity of the sensor and a wide linear sensing range are achieved, the stability and service life are improved, the conductive layer stripping and electrical separation are avoided, and the reliability and environmental adaptability of the sensor are enhanced.
Smart Images

Figure CN118687465B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of sensors, and in particular relates to a highly sensitive and widely linear flexible strain sensor based on a composite gradient structure. Background Art
[0002] Flexible strain sensors, with their excellent flexibility, portability, high efficiency and low cost, have shown great application potential in the fields of robot skin, wearable devices, etc. Among them, double-layer crack-type flexible strain sensors have been widely studied due to their advantages such as high sensitivity, low detection limit, wide sensing range and fast response. In practical application scenarios, not only high sensitivity for monitoring subtle strains is required, but also high linearity is required to simplify calibration and avoid errors caused by uncertain pre-strain introduced when installing the sensor. However, since this type of sensor only has a significantly faster resistance increase than other stages in the narrow stage from crack connection to complete fracture, it is difficult to achieve both high sensitivity and a wide linear sensing range.
[0003] In recent years, researchers have made a lot of efforts in the research field of high linearity flexible strain sensors:
[0004] The academic paper "High-Performance Strain Sensors Based on Au / Graphene Composite Films with Hierarchical Cracks for Wide Linear-Range Motion Monitoring" (Cheng X, Cai J, Xu JH, et al. High-Performance Strain SensorsBased on Au / Graphene Composite Films with Hierarchical Cracks for Wide Linear-Range Motion Monitoring[J].Applied Materials&Interfaces 2022, 14,39230–39239) proposed an Au / graphene composite film (AGCF) strain sensor with hierarchical cracks based on the concept of fractal pattern bionics. The unique wrinkle structure introduced by the self-assembled graphene film (SAGF) can induce extensive microcracks, but inhibit the catastrophic crack extension or fracture of the AGCF. The prepared sensor has a high GF (≈153) in a wide linear working range (R2≈0.9975, 0~20%).
[0005] The academic paper "From network to channel: Crack-based strain sensors with high sensitivity, stretchability, and linearity via strain engineering" (Wang W Y, Liu YX, Ding MK, et al. From network to channel: Crack-based strain sensors with high sensitivity, stretchability, and linearity via strain engineering [J]. Nano Energy 2023, 116, 108832) uses three methods to control the generation and extension behavior of cracks by introducing soft-rigid interface, elastic modulus mismatch and size matching. Through strain engineering optimization and network cracks, a flexible strain sensor with a GF value of up to 690.95 in the linear working range of 0 ~ 40% was prepared.
[0006] The academic paper "Enhancement of linearity range of stretchable ultrasensitive metal crack strain sensor via superaligned carbon nanotube-based strain engineering" (Kang-Hyun Kim, Soon Kyu Hong, Sung-Hun Ha, et al. Enhancement of linearity range of stretchable ultrasensitive metal crack strain sensor viasuperaligned carbon nanotube-based strain engineering[J]. Materials Horizons2020, 7, 2662-2672) is based on Pt / SACNT hybrid piezoresistive film. By redistributing the surface strain of the PDMS substrate during stretching, the SACNT film induces random high-density short cracks in the Pt film, thereby improving the stretchability and linearity of the sensor.
[0007] The academic paper "High Sensitivity, Wide Linear-Range Strain Sensor Based onMXene / AgNW Composite Film with Hierarchical Microcrack" (Wang T, Qiu ZG, Li HC, et al. High Sensitivity, Wide Linear-Range Strain Sensor Based on MXene / AgNW Composite Film with Hierarchical Microcrack[J]. Small 2023, 19, 2304033) developed a MXene / silver nanowire (AgNW) composite strain sensor with hierarchical microcracks (hmc), optimized the sensitivity, stretchability and linearity, and achieved a high GF of 244 and a wide linear working range (60%, R 2 ≈99.25%).
[0008] Patent application CN116447967A combines a wrinkle structure that can improve linearity and stretchability with a crack structure that can improve sensitivity to prepare a strain sensor with a sensitivity of 22.98 in the strain range of 0-30%. When the sensor is within the strain range of 10%, the linear fit can reach 0.9978, and when the sensor strain is within the range of 20% and 30%, the linear fit can be improved to 0.9985.
[0009] Patent application CN116147475A provides a strain sensor based on double-thread conductive yarn and its preparation method. The double-thread is bonded to the surface of spandex yarn by hot pressing low-melting point hot fuse wire, and forms a double-thread shape, forming a double-thread yarn integrating two heterogeneous materials, low-melting point hot fuse wire and spandex. The linearity of the flexible strain sensor after 2000 cycles of stretching at 50% strain is not less than 0.964, and the sensitivity is not less than 9.86.
[0010] Patent application CN113074622A uses liquid surface self-assembly to prepare a graphene film with uniform thickness and quasi-continuous layers, which can be combined with a nano-gold layer to form a composite structure. The sensor has a high strain sensitivity to small deformations (GF>130). The high density of cracks and graphene wrinkles inhibit the penetration of a single crack, and ultimately form a high-density multi-size crack structure, allowing the sensor to maintain linear strain perception within a wide range (0~15%) and maintain good linearity (R 2 ~0.9971).
[0011] Patent application CN111649665A uses fused deposition modeling 3D printing technology to customize the spiderweb array structure, and utilizes the coordinated distribution of one-dimensional multi-walled carbon nanotubes and two-dimensional graphene nanosheets in the spiderweb-like flexible strain sensor to optimize the conductive path in the sensor. The strain sensor has a sensitivity of approximately 10020, and its linearity coefficient of determination is greater than 0.96 when the strain is 50%.
[0012] Although flexible strain sensors have made some progress in improving sensitivity, sensing range and linearity in recent years, they still have the following shortcomings:
[0013] 1. One of the most common methods for preparing flexible conductive materials for flexible strain sensors is to add conductive fillers such as metal fillers and carbon fillers into polymers. Due to the poor bonding between such fillers and the polymer matrix, sensors based on this method generally have disadvantages such as obvious hysteresis, low linearity, and poor stability. Another method is to use intrinsically conductive polymers to prepare stress-sensitive elements, among which PEDOT:PSS is widely used due to its excellent electrochemical properties and stability. However, PEDOT:PSS has poor stretchability and low intrinsic conductivity. How to prepare semi-conductive elastic sensitive elements with good stretchability and stability and PEDOT:PSS composite films with excellent conductivity based on PEDOT:PSS is an urgent problem to be solved.
[0014] 2. To improve the performance of flexible strain sensors, many researchers have introduced crack-like surface microstructures in the conductive strain layer of the sensor. This surface microstructure helps to improve the sensitivity. The network-like crack structure improves the sensitivity by making the conductive strain layer evolve from full contact to mesh contact with gaps during operation. The sensor prepared by this method has a wide sensing range, but the improvement in sensitivity is limited. Another way is to construct a sensor with a channel crack structure, but since it only contains one conductive strain layer, the conductive path of the sensor is disconnected after the crack breaks, and the sensor detection range is very small.
[0015] 3. Current crack-type flexible strain sensors often improve the linear sensing range of the sensor by limiting the crack morphology to a network-type crack. Although this design method can achieve high linearity and a wide linear sensing range, it sacrifices the sensitivity of the sensor and makes it difficult to adjust the balance between the linear sensing range and sensitivity of the sensor to adapt to the different requirements of sensor performance in different application scenarios.
[0016] 4. Crack-based flexible strain sensors often use methods such as coating strain layers or evaporating precious metals to prepare strain layers, but the prepared sensors all have poor heterogeneous interface bonding between the strain layer and the substrate. Since the bonded strain layer and the substrate or different strain layers have different mechanical moduli and elongation at break, the conductive strain layer of the sensor is prone to peeling, falling off or shifting under repeated operation, resulting in poor sensor stability.
[0017] 5. The electrode part of the flexible strain sensor often injects the wire into the conductive strain layer of the sensor or connects it to the high-conductivity layer through a conductive paste and then encapsulates it with a packaging layer. However, due to the poor mechanical properties of the strain layer and the conductive paste, the contact area with the wire is small, the connection stability is poor, and electrical separation is easy to occur, causing the sensor resistance to fluctuate greatly, affecting the stability and service life of the sensor. Summary of the invention
[0018] In view of the shortcomings of the prior art, the present invention provides a high-sensitivity and wide-linear flexible strain sensor based on a composite gradient structure and a preparation method thereof, which effectively improves the problem that flexible strain sensors are difficult to have high sensitivity, wide linear range, and high stability, and can be widely used in the fields of wearable electronics and electronic skin.
[0019] In order to solve the above problems, the present invention adopts the following technical solutions:
[0020] The present invention first discloses a highly sensitive wide linear flexible strain sensor based on a composite gradient structure. The sensor is a linear structure as a whole, including a strain sensitive element, an electrode structure and an elastic packaging tube. The linear structure of the sensor enables it to be more conveniently and fitly integrated into wearable items such as fabrics; the elastic packaging tube protects the strain sensitive element of the sensor, making it less likely to be damaged due to contact, friction and other reasons during application, thereby improving the reliability and environmental adaptability of the sensor.
[0021] Furthermore, the strain sensitive element has a core-sheath structure, consisting of a low-conductivity inner core and a high-conductivity film layer adhered to the surface of the low-conductivity inner core. The high-conductivity film layer has a wrinkled surface microstructure; the wrinkled surface microstructure is divided into N (N is any integer from 4 to 8) segments in the length direction, and each segment has a gradient wrinkle depth and elongation at break. Elongation at break refers to the relative elongation of a material when it breaks, that is, the ratio of the elongation of the material when it breaks to its initial length, expressed as a percentage.
[0022] Furthermore, the electrode structure is arranged at both ends of the strain sensitive element, and comprises a copper wire and a carbon fiber fixing junction, and the copper wire is fixed on the high conductive film layer through the carbon fiber fixing junction.
[0023] Furthermore, the elastic packaging tube is sleeved on the periphery of the strain sensitive element, and the copper wires are led out from two ends of the elastic packaging tube.
[0024] Furthermore, the low-conductivity inner core is made by dipping and curing the elastic core-wrapped fiber wire in a composite slurry of a PEDOT:PSS aqueous solution, TritonX-100 and PDMS, and then sequentially treating it with oxygen plasma and dipping it with a silane coupling agent containing a mercapto group. Furthermore, the diameter of the elastic core-wrapped fiber wire is 0.5~1mm, and the stretchable length is not less than 50%, and the stretchable length of the low-conductivity inner core formed after the elastic core-wrapped fiber wire is dipped is also not less than 50%. The mass percentage of each component in the composite slurry is: 20%~40% of PEDOT:PSS aqueous solution, 0.5%~2% of TritonX-100, and the remainder is PDMS and its curing agent, and the mass ratio of PDMS to curing agent is 10:1.
[0025] Furthermore, the high-conductivity film layer is formed by dividing the low-conductivity inner core into N segments along the length direction, and then each segment is immersed in a mixture of triethylene glycol, PEDOT:PSS aqueous solution and bovine serum albumin at a gradient tensile elongation, so that each segment of the film layer has a gradient wrinkle depth and elongation at break after releasing the pre-strain, and then immersed in a post-treatment solution containing ZnCl2. Furthermore, the mass percentage of each component in the mixed solution is: PEDOT:PSS aqueous solution 75%~85%, triethylene glycol 4%~6%, and the balance is bovine serum albumin. The composition of each raw material in the post-treatment solution according to mass percentage is: ZnCl21%~5%, DMF 75%~85%, and the balance is deionized water.
[0026] Furthermore, in the electrode structure, the two ends of the high-conductivity film layer are connected to copper wires respectively, and a layer of conductive carbon fiber wires is bundled outside the connection, and the bundled conductive carbon fiber wires form a carbon fiber fixing knot. The copper wire, the carbon fiber fixing knot and the connection of the high-conductivity film layer are injection molded into one by a conductive adhesive.
[0027] Furthermore, the conductive adhesive is prepared by blending carboxylated styrene butadiene latex, triethylene glycol, PEDOT:PSS aqueous solution, silane coupling agent KH-550 and carbon black according to the following mass percentages: 30% to 40% PEDOT:PSS aqueous solution, 2% to 5% triethylene glycol, 4% to 6% KH-550, 20% to 30% carbon black, and the balance is carboxylated styrene butadiene latex.
[0028] Furthermore, in the strain sensitive element, the conductivity of the low conductive core is not higher than 10S·cm -1 , the conductivity of the high conductive film layer is not less than 3000S·cm -1, the conductivity of the conductive adhesive is not less than 2000S·cm -1 . The sensitivity of the sensor is defined as the ratio of the change in sensor resistance to the initial resistance under unit tensile strain. The conductivity of the inner and outer conductive layers is different, and the sensing performance of the entire sensor is also different. The higher the conductivity of the high-conductive film layer in the strain-sensitive element, the smaller the initial resistance of the sensor's conductive path, and the lower the conductivity of the low-conductive inner core, the greater the resistance change that can be produced after the sensor is stretched and cracked, and thus the higher the sensitivity of the sensor. The sensor prepared according to the above-mentioned gradient conductivity of the inner and outer layers has a sensitivity of more than 200 over a strain range of 50%.
[0029] Furthermore, the two ends of the elastic packaging tube are fixed to the strain sensitive element by crimping buckles. The inner diameter of the elastic packaging tube is 0.5-1 mm, the wall thickness is 0.2-0.6 mm, the elongation at break is not less than 50%, and the Young's modulus is not less than 100 kPa.
[0030] The present invention further provides a method for preparing the highly sensitive and widely linear flexible strain sensor based on the composite gradient structure, comprising the following steps:
[0031] Step 1: Prepare low-conductivity inner core
[0032] After PDMS and its curing agent are magnetically stirred at room temperature, a TritonX-100 modifier is added and stirred evenly, and then a PEDOT:PSS aqueous solution is added and stirred evenly to obtain a composite slurry for preparing a low-conductivity inner core;
[0033] Take a section of elastic core-covered fiber line, wash and dry it, immerse it in the composite slurry at 0 strain state and heat cure it, then treat it with oxygen plasma, and then soak it in an aqueous solution of a silane coupling agent containing a mercapto group at a concentration of 15~25 mg / mL for 1.5~2 hours. After taking it out, wash it with ethanol and dry it to complete the surface mercapto grafting treatment to obtain a low conductive inner core.
[0034] Step 2: Prepare a highly conductive film layer
[0035] After the PEDOT:PSS aqueous solution, triethylene glycol and deionized water are mixed and magnetically stirred to be uniform, bovine serum albumin is added and stirred to be uniform to obtain a mixed solution for preparing a highly conductive film layer;
[0036] After fixing the two ends of the low-conductivity inner core obtained in step 1, divide it into N sections along the length direction, and immerse each section in the mixed liquid at a gradient tensile elongation in turn and dry and solidify at room temperature to form a film layer with a gradient wrinkle depth and elongation at break; wherein the tensile elongation of the nth section is A×(Nn) / N, n is 1, 2, ..., N, and A=10~50%. In the specific operation, when preparing the film layer of the first section, first stretch the low-conductivity inner core to A×(N-1) / N, and wrap the other sections except the first section with plastic wrap, immerse and solidify. Then release the tensile elongation of the low-conductivity inner core to A×(N-2) / N, and wrap the other sections except the second section with plastic wrap, immerse and solidify. And so on, the preparation of the film layer is completed.
[0037] The prepared film layer is immersed in a post-treatment solution containing ZnCl2 for 0.5 to 1 hour, then taken out and washed with deionized water and dried, so that a high conductive film layer is formed on the surface of the low conductive inner core to obtain a strain sensitive element.
[0038] Step 3: Sensor packaging and electrode preparation
[0039] After adding triethylene glycol to the PEDOT:PSS aqueous solution and stirring it evenly with a magnetic stirrer, carbon black and KH-550 are added and stirred evenly, and then carboxylated styrene butadiene latex is added and stirred evenly with a magnetic stirrer to obtain a conductive adhesive;
[0040] Select an elastic packaging tube with an inner diameter not less than the outer diameter of the strain sensitive element, and pass the strain sensitive element prepared in step 2 through the elastic packaging tube in a stretched state; fix the copper wires at both ends of the strain sensitive element through carbon fiber fixing knots, and then inject the connection between the copper wire, the carbon fiber fixing knot and the end of the high conductive film layer into one piece through a conductive adhesive to form an electrode structure;
[0041] The strain sensitive element is released, and the outer end of the carbon fiber fixing knot is aligned with the outer end of the elastic packaging tube, and wire buckles are put on the edges of both ends and clamped to fix the two ends of the elastic packaging tube and the strain sensitive element, thereby obtaining the highly sensitive wide linear flexible strain sensor based on the composite gradient structure.
[0042] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0043] 1. The flexible strain sensor of the present invention, whose strain sensitive element is made of intrinsic conductive polymer PEDOT:PSS, has a uniform and stable polymer conductive network compared to the traditional polymer conductive composite material prepared by adding solid conductive fillers to the polymer.
[0044] In order to solve the problem of poor mechanical properties of PEDOT:PSS film, the low-conductivity core of the sensor is modified mechanically by doping the high molecular polymer PDMS with excellent mechanical properties into the PEDOT:PSS material. And by using the compatibilizer TritonX-100 to treat PDMS, the hydrophobic group at one end is tightly bound to the PDMS molecular chain, and the hydrophilic group at the other end is combined with the PSS chain in PEDOT:PSS, thus achieving uniform compatibility and cross-linking of the originally incompatible PEDOT:PSS and PDMS. This material system enables the low-conductivity core to have a uniform conductive network distribution, thus having stable semi-conductive properties. At the same time, the high content of PDMS doping makes the low-conductivity core have excellent mechanical properties such as high stretchability, low hysteresis and low creep, thereby improving the stability, low hysteresis and fast response characteristics of the sensor.
[0045] In order to solve the problem that the conductivity of PEDOT:PSS film is not high enough, resulting in high initial resistance and low sensitivity of the sensor, triethylene glycol with multiple hydroxyl groups is introduced into the high conductive film layer of the sensor to electrically modify PEDOT:PSS. The hydrogen bonding between the hydroxyl groups of triethylene glycol and the PSS molecular chain weakens the electrostatic interaction between the PSS chain and the PEDOT chain, promotes the phase separation process between the two, reduces the dispersed connection of the PEDOT conductive chain, and thus improves the conductivity of PEDOT:PSS. At the same time, triethylene glycol also promotes the transformation of the PEDOT conductive main chain structure from a benzene structure to a quinone structure, reduces the energy barrier for carrier transmission on the PEDOT chain, and further enhances the conductivity of the PEDOT:PSS film. In addition, the present invention uses a DMF solution containing ZnCl2 to post-treat the surface of the prepared high conductive film layer. In this process, the interaction between the polar groups in DMF and PEDOT and PSS, as well as the Zn + and CI - PEDOT + and PSS - ion binding, synergistically weakening the PEDOT + With PSS - The Coulomb attraction between them enhances the phase separation effect of PSS and PEDOT, further improving the conductivity of the PEDOT:PSS film. These electrical modification measures jointly improve the conductivity of the high conductive film layer, reduce the initial resistance value of the sensor, and improve the sensitivity of the sensor.
[0046] 2. The strain sensor of the present invention greatly improves the sensitivity of the sensor through the through-crack microstructure design of the high-conductive film layer. At the same time, a double strain layer is designed based on the through-crack microstructure of the high-conductive film layer, in which the high-conductive film layer shell is attached to the surface of the low-conductive inner core. When strain is applied to the sensor, when a through crack is generated on the surface of the high-conductive film layer, the current is transmitted through the low-conductive inner core, and the sensor resistance will not be saturated immediately, thereby improving the sensing range of the sensor while maintaining the high sensitivity of the sensor. In addition, this dual strain layer structure design provides a variety of design parameters that can be used to control linearity, such as the thickness of the low-conductive inner core and the high-conductive film layer, stress distribution control, and surface microstructure design of the low-conductive inner core and the high-conductive film layer, which provides conditions for regulating the linearity of the sensor.
[0047] 3. While the present invention utilizes the electrical gradient structure of the dual strain layer to realize the flexible strain sensor, the surface microstructure design of multiple sections of the highly conductive film layer with different wrinkle depths allows each section of the highly conductive film layer to gradually develop cracks during the stretching process, that is, the resistance of each section increases successively during the stretching process, and the total resistance of the sensor gradually increases during the stretching process, thereby improving the linearity of the sensor. Based on the design of the electrical and mechanical composite gradient structure, the high sensitivity and wide linear sensing range of the sensor are achieved. In addition, by adjusting the number of segments of the highly conductive film layer and the wrinkle depth of each section of the wrinkle microstructure, the balance between the sensor sensitivity and the linear sensing range can be simply achieved to meet the performance requirements in different application scenarios.
[0048] 4. The low-conductivity inner core in the flexible strain sensor of the present invention is coated with a composite slurry on the surface of the elastic core-wrapped fiber line by an impregnation method. Due to the capillary force between the fiber and the low-conductivity composite slurry, the low-conductivity layer has a strong adhesion to the surface of the elastic fiber. In addition, by successively adopting oxygen plasma treatment and silane coupling agent solution immersion treatment, a large number of thiol groups are grafted on the surface of the low-conductivity layer, and a bovine serum albumin (BSA) cross-linked network is doped in the high-conductivity film layer PEDOT:PSS material system, so that the disulfide bonds of the BSA molecular chain at the interface between the high-conductivity film layer and the low-conductivity layer exchange reaction with the thiol groups on the surface of the low-conductivity layer to form a stable chemical bond, thereby improving the interface bonding force between the high-conductivity layer and the low-conductivity layer, thereby reducing the separation, peeling and new cracks at the interface between the high-conductivity layer and the low-conductivity layer during the sensor application process, and improving the stability of the sensor.
[0049] 5. In the flexible strain sensor, it is difficult to achieve a stable combination between the electrode copper wire and the high-conductive film layer. During long-term use, the unstable electrical connection between the sensor electrode copper wire and the strain sensitive element will cause the fluctuation of the sensor output resistance signal, thereby affecting the reliability and stability of the sensor. The flexible strain sensor of the present invention first uses carbon fiber wires to bundle the copper wires and the strain sensitive element at the electrodes at both ends, so that the copper wires and the high-conductive film layer are in close contact, and then the copper wires, carbon fiber wires and the high-conductive film layer are bonded by injection molding with a conductive adhesive, so that the copper wires and the high-conductive film layer always have good electrical contact, avoiding the sensor resistance fluctuation caused by loose mechanical structure and poor contact during long-term use, and improving the stability and service life of the sensor. The conductive adhesive used uses carboxyl styrene butadiene latex as the matrix material, and has good adhesion with carbon fiber wires, copper wires, and high-conductive film layers. PEDOT:PSS electrically modified with triethylene glycol and carbon black powder grafted with KH-550 are used as conductive fillers. PEDOT:PSS and carbon black powder conduct electricity synergistically. The combination of PEDOT:PSS and carbon black powder enhances the dispersion uniformity of the carbon black powder, further enhances the electrical conductivity while maintaining the excellent adhesion and film-forming properties of the binder material, reduces the contact resistance between the copper wire and the high conductive film layer, improves the stability of the electrical contact between the copper wire and the strain sensitive element, and further improves the stability and service life of the sensor. BRIEF DESCRIPTION OF THE DRAWINGS
[0050] Figure 1 This is a schematic diagram of the appearance structure of the high-sensitivity and wide-linear flexible strain sensor based on the composite gradient structure of the present invention.
[0051] Figure 2 This is a schematic diagram of the structure of each component of the high-sensitivity and wide-linear flexible strain sensor based on a composite gradient structure of the present invention.
[0052] Figure 3 This is a schematic diagram of the cross-sectional structure of the highly sensitive and wide linear flexible strain sensor based on the composite gradient structure of the present invention.
[0053] Figure 4 It is a schematic structural diagram of the controllable stretching fixture for preparing strain sensitive elements according to the present invention.
[0054] Figure 5 This is a schematic diagram of the principle of mechanical modification of PEDOT:PSS by PDMS in the low-conductive core material of the present invention.
[0055] Figure 6 Schematic diagram of the principle of electrical modification of PEDOT:PSS by triethylene glycol in the material of the high conductive film layer of the present invention.
[0056] Figure 7It is a schematic diagram of the crack propagation state of the strain sensitive element in the high-sensitivity and wide-linear flexible strain sensor based on the composite gradient structure during the strain process of the present invention.
[0057] Figure 8 Schematic diagram of the sensing mechanism and local conductive path of the flexible strain sensor of the present invention.
[0058] Fig. 9 This is the stress-strain characteristic curve of the flexible strain sensor of the present invention.
[0059] Fig.10 This is the resistance-strain characteristic curve of the flexible strain sensor of the present invention.
[0060] Fig.11 This is the frequency response characteristic of the flexible strain sensor of the present invention.
[0061] Fig.12 This is the step response characteristic curve of the flexible strain sensor of the present invention.
[0062] Fig.13 This is the repeatability test curve of the flexible strain sensor of the present invention.
[0063] The numbers in the above figure are: 1 is a low-conductivity inner core, 2 is a high-conductivity film layer, 3 is an elastic packaging tube, 4 is a carbon fiber fixing section, 5 is a copper conductor, 6 is a wire buckle; 7 is a controllable stretching fixing device. DETAILED DESCRIPTION
[0064] The embodiments of the present invention are described in detail below in conjunction with the accompanying drawings. The following embodiments are implemented on the premise of the technical solution of the present invention, and detailed implementation methods and specific operation processes are given, but the protection scope of the present invention is not limited to the following embodiments.
[0065] like Figure 1~Figure 3 As shown, they are respectively a structural model diagram, a sensor component structure diagram and a cross-sectional structure schematic diagram of the flexible strain sensor provided in this embodiment. The highly sensitive wide linear flexible strain sensor based on a composite gradient structure provided in this embodiment includes a strain sensitive element, an electrode structure and an elastic packaging tube. The strain sensitive element is a core-sheath structure, which is composed of a low-conductive inner core and a high-conductive film layer adhered to the surface of the low-conductive inner core. The high-conductive film layer has a wrinkled surface microstructure; the wrinkled surface microstructure is divided into 5 sections in the length direction, and each section has a gradient wrinkle depth and elongation at break.
[0066] The electrode structure is arranged at two ends of the strain sensitive element, and comprises a copper wire and a carbon fiber fixing junction, and the copper wire is fixed on the high-conductivity film layer through the carbon fiber fixing junction.
[0067] The elastic packaging tube is sleeved on the periphery of the strain sensitive element, and the copper wires are led out from the two ends of the outer packaging tube. The two ends of the elastic packaging tube are fixed to the strain sensitive element by means of wire buckles.
[0068] Specifically, the flexible strain sensor of this embodiment is manufactured according to the following steps:
[0069] Step 1: Prepare low-conductivity inner core
[0070] After 5 g of PDMS and 0.5 g of its curing agent were magnetically stirred at room temperature, 0.15 g of TritonX-100 modifier was added and continued to be stirred evenly, and then 3 g of PEDOT:PSS aqueous solution (the solid content of the PEDOT:PSS aqueous solution used in this embodiment is 2%) was added and stirred evenly to obtain a composite slurry for preparing a low-conductivity inner core.
[0071] Take a section of elastic core-covered fiber wire with a diameter of 0.5 mm and a length of 30 mm, wash and dry it, immerse it in the composite slurry for 15 minutes, take it out and heat it in an oven at 80°C for 6 hours, then treat it with oxygen plasma in a plasma processor for 5 minutes, and then immerse it in an aqueous solution of 3-mercaptopropyltriethoxysilane with a concentration of 20 mg / mL for 1.5 hours. After taking it out, wash it with ethanol and dry it to complete the surface thiol grafting treatment to obtain a low conductive inner core.
[0072] Step 2: Prepare a highly conductive film layer
[0073] 5 g of PEDOT:PSS aqueous solution and 0.3 g of triethylene glycol were stirred in a magnetic stirrer at room temperature for 40 minutes, and then 0.6 g of bovine serum albumin was added and stirred at room temperature for 2 hours to obtain a mixed solution for preparing a highly conductive film layer.
[0074] The two ends of the low-conductivity inner core obtained in step 1 are fixed on a controllable stretching fixture, and it is divided into 5 sections along the length direction: first, the low-conductivity inner core is pre-stretched to a stretching elongation of 40%, and the other sections except the first section are wrapped with plastic wrap, and then the low-conductivity inner core is immersed in the mixed solution for 5 minutes, taken out and dried at room temperature to obtain the first section of high-conductivity film layer; then the stretching elongation of the low-conductivity inner core is released to 30%, and the other sections except the second section are wrapped with plastic wrap, and then the low-conductivity inner core is immersed in the mixed solution again for 5 minutes, taken out and dried at room temperature to obtain the second section of high-conductivity film layer. By analogy, the preparation of the high-conductivity film layer of the third section (stretching elongation released to 20%), the fourth section (stretching elongation released to 10%), and the fifth section (stretching elongation released to 0%) is completed.
[0075] The prepared film layer was immersed in a post-treatment solution (the mass percentage of each raw material in the solution was ZnCl24%, DMF 80%, and the balance was deionized water) for 40 minutes, then taken out and washed with deionized water and dried, so that a high conductive film layer was formed on the surface of the low conductive inner core to obtain a strain sensitive element.
[0076] Step 3: Sensor packaging and electrode preparation
[0077] 0.4 g of triethylene glycol was added to 4 g of PEDOT:PSS aqueous solution and magnetically stirred for 40 minutes, then 2.5 g of carbon black and 0.6 g of KH-550 were added and stirring was continued for 1 hour, and 4 g of carboxylated styrene butadiene latex was added and magnetically stirred for 2 hours to obtain a conductive adhesive.
[0078] An elastic packaging tube with an inner diameter of 0.8 mm and a wall thickness of 0.3 mm is selected, and the strain sensitive element prepared in step 2 is passed through the elastic packaging tube under tension; the copper wires are fixed at both ends of the strain sensitive element by carbon fiber fixing knots, and then the connection between the copper wire, the carbon fiber fixing knot and the high conductive film layer is injection molded into one by a conductive adhesive to form an electrode structure; in the specific operation, carbon fiber wires are used to bundle the wires on the high conductive film layer at both ends of the strain sensitive element, and then the two ends are placed in a cylindrical slotted mold in turn, and the conductive adhesive is injection molded to bond the connection area between the copper wire and the high conductive film layer.
[0079] The strain sensitive element is released, and the outer end of the carbon fiber fixing knot is aligned with the outer end of the elastic packaging tube. Wire buckles are put on the edges of both ends and clamped to fix the two ends of the elastic packaging tube and the strain sensitive element, thereby obtaining a highly sensitive and wide linear flexible strain sensor based on a composite gradient structure.
[0080] Figure 4 The schematic diagram of the controllable stretch fixture used is shown in Figure 2. The two ends of the low-conductivity inner core are fixed to the controllable stretch fixture bracket with screws, and the sliding end of the bracket is moved to stretch the linear material to the required length and fix it, so that the pre-stretched length of the linear material can be stably controlled for dipping and preparing the coating.
[0081] Figure 5 Schematic diagram of the material system of the low-conductivity core. PEDOT:PSS is used as the conductive material, which has good semi-conductive properties and a more uniform and stable conductive network. PDMS is added as a mechanical modifier, and a composite conductive film with excellent mechanical properties is obtained through the cross-linking network design of PDMS and PEDOT:PSS. TritonX-100 is used as a compatibilizer, which has both hydrophobic groups and hydrophilic groups, and can be combined with PDMS molecular chains and PSS molecular chains respectively, so that PDMS and PEDOT:PSS are uniformly compatible and the PEDOT:PSS conductive network is evenly dispersed.
[0082] Figure 6 This is a schematic diagram of the material system of the high-conductive film layer. The intrinsic conductive polymer PEDOT:PSS is used as the conductive material. In view of its low conductivity, triethylene glycol is used as an electrical modifier. The hydrogen bond interaction between the hydroxyl group in triethylene glycol and the PSS molecular chain weakens the electrostatic interaction between PSS and PEDOT, and promotes the phase separation process between the two. In addition, triethylene glycol also promotes the transformation of the PEDOT main chain from the benzene structure to the quinone structure, reduces the energy barrier for carrier transmission, and further enhances the conductivity of PEDOT:PSS.
[0083] Figure 7 The diagram is a schematic diagram of the crack distribution and expansion process in the high conductive film layer of the strain sensitive element during different tensile strain processes. It can be seen that for each section of the high conductive film layer with different wrinkle depths prepared under different pre-stretching conditions, during the strain process, the part with shallow wrinkle depth begins to produce channel cracks under small strain, while the part with deep wrinkle depth gradually begins to produce channel cracks under large strain. During the strain process, channel cracks are generated in each section of the sensor's high conductive film layer in turn, causing the sensor resistance to gradually increase, thereby improving the sensor's linearity.
[0084] Figure 8 The sensing mechanism and local conductive path schematic diagram of the flexible strain sensor prepared in this embodiment. In the initial state, the main transmission path of electrons is the high conductive film layer of the sensor. When the sensor is stretched, due to the gradient elongation at break of the high conductive film layer and the low conductive inner core, cracks will be generated in the high conductive film layer. The transmission path of electrons at the crack is from the high conductive film layer to the low conductive inner core, bypassing the crack and then returning to the high conductive film layer, and so on, which is equivalent to connecting several low-resistance outer layers and high-resistance inner cores in series. Therefore, when the sensor is strained, the sensor resistance increases rapidly, the sensor sensitivity is high, and when a through crack is generated in the high conductive film layer, the electron transmission channel is not disconnected, and the sensor can still respond to resistance changes under large strains, so the sensor maintains high sensitivity while having a large sensing range. In the figure, R represents the resistance of the high conductive film layer when not stretched, and R' refers to the resistance of the low conductive inner core when not stretched, and R is much smaller than R'. R1, R2, and R3 represent the resistance of each segment separated by the crack in the high conductive film layer after the crack is generated. R1' and R2' refer to the resistance of the current transmitted through the low conductive core at the crack after the crack is generated. R1' and R2' are much larger than R1, R2, and R3.
[0085] Fig. 9 From the stress-strain test curve of the flexible strain sensor prepared in this embodiment, it can be seen that the sensor can withstand a large strain of 115%, which means that the sensor has good stretchability and can fully meet the needs of the human wearable field.
[0086] Fig.10 The resistance-strain characteristic curve of the flexible strain sensor prepared in this embodiment shows that the sensor has high sensitivity and a wide linear sensing range. In the strain range of 0~50%, the sensor sensitivity coefficient GF is about 362.7, and the linear correlation coefficient R 2 It is 0.9954.
[0087] Fig.11 The frequency response test results of the flexible strain sensor prepared in this embodiment show that the resistance change characteristic curve of the cyclic loading experiment with a loading frequency of 0.5 Hz to 4 Hz and a strain of 25% shows that the output resistance of the sensor does not deviate significantly, indicating that the sensor can be used to work at different frequencies of 0.5 Hz to 4 Hz.
[0088] Fig.12 This is the result of a step test on the flexible strain sensor prepared in this embodiment. It can be seen that the sensor can work stably under a strain of 0-50%.
[0089] Fig.13 The test results of 2000 periodic loading / unloading experiments on the flexible strain sensor prepared in this embodiment (strain range 0~25%) are shown. It can be seen that in the 2000 cycle test, the output resistance of the sensor did not deviate significantly, proving that the sensor has stable electrical characteristics and good repeatability.
[0090] The above-described embodiments only express exemplary embodiments of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of protection of the present invention. It should be pointed out that, for a person of ordinary skill in the art, several modifications and improvements can be made without departing from the concept of the present invention, and these all belong to the scope of protection of the present invention. Therefore, the scope of protection of the present invention shall be subject to the attached claims.
Claims
1. A highly sensitive and wide linear flexible strain sensor based on a composite gradient structure, characterized in that: The sensor is in a linear structure as a whole, including a strain sensitive element, an electrode structure and an elastic packaging tube; The strain sensitive element has a core-sheath structure, consisting of a low-conductivity inner core and a high-conductivity film layer adhered to the surface of the low-conductivity inner core; the high-conductivity film layer has a wrinkle-type surface microstructure; the wrinkle-type surface microstructure is divided into N sections in the length direction, and each section has a gradient wrinkle depth and elongation at break; The electrode structure is arranged at both ends of the strain sensitive element, and includes a copper wire and a carbon fiber fixing knot, and the copper wire is fixed on the high conductive film layer through the carbon fiber fixing knot; The elastic packaging tube is sleeved on the periphery of the strain sensitive element, and the copper wire is led out from both ends of the elastic packaging tube; The high-conductivity film layer is formed by dividing a low-conductivity inner core into N sections along the length direction, and then immersing each section in a mixed solution of triethylene glycol, PEDOT:PSS aqueous solution and bovine serum albumin at a gradient tensile elongation in turn, so that each section of the film layer has a gradient wrinkle depth and elongation at break after releasing the pre-strain, and then immersing it in a post-treatment solution containing ZnCl2; the mass percentage of each component in the mixed solution is: PEDOT:PSS aqueous solution 75%~85%, triethylene glycol 4%~6%, and the balance is bovine serum albumin; the composition of each raw material in the post-treatment solution according to mass percentage is: ZnCl21%~5%, DMF 75%~85%, and the balance is deionized water.
2. The highly sensitive and wide linear flexible strain sensor based on a composite gradient structure according to claim 1, characterized in that: The low-conductivity inner core is prepared by dipping and curing the elastic core-covered fiber wire in a composite slurry of a PEDOT:PSS aqueous solution, TritonX-100, PDMS and its curing agent, and then sequentially subjecting the fiber to oxygen plasma treatment and dip-coating treatment with a silane coupling agent containing a mercapto group. The diameter of the elastic core-spun fiber line is 0.5-1 mm, and the stretchable length is not less than 50%; The mass percentages of the components in the composite slurry are: 20% to 40% PEDOT:PSS aqueous solution, 0.5% to 2% TritonX-100, and the remainder is PDMS and its curing agent, and the mass ratio of PDMS to the curing agent is 10:
1.
3. The highly sensitive and wide linear flexible strain sensor based on a composite gradient structure according to claim 1, characterized in that: N is any integer between 4 and 8.
4. The highly sensitive and wide linear flexible strain sensor based on a composite gradient structure according to claim 1, characterized in that: In the electrode structure, the copper wire, the carbon fiber fixing junction and the connection of the high-conductivity film layer are injection-molded into one piece by a conductive adhesive.
5. The highly sensitive and wide linear flexible strain sensor based on a composite gradient structure according to claim 4, characterized in that: The conductive adhesive is prepared by blending carboxylated styrene butadiene latex, triethylene glycol, PEDOT:PSS aqueous solution, silane coupling agent KH-550 and carbon black according to the following mass percentages: 30%-40% PEDOT:PSS aqueous solution, 2%-5% triethylene glycol, 4%-6% KH-550, 20%-30% carbon black, and the balance being carboxylated styrene butadiene latex.
6. The highly sensitive and wide linear flexible strain sensor based on a composite gradient structure according to claim 1, characterized in that: In the strain sensitive element, the conductivity of the low conductive inner core is not higher than 10S·cm -1 , the conductivity of the high conductive film layer is not less than 3000S·cm -1 .
7. The highly sensitive and wide linear flexible strain sensor based on a composite gradient structure according to claim 1, characterized in that: The two ends of the elastic packaging tube are fixed to the strain sensitive element by means of wire buckles.
8. The highly sensitive and wide linear flexible strain sensor based on a composite gradient structure according to claim 1, characterized in that: The inner diameter of the elastic packaging tube is 0.5-1 mm, the wall thickness is 0.2-0.6 mm, and the elongation at break is not less than 50%.
9. A method for preparing a highly sensitive and wide linear flexible strain sensor based on a composite gradient structure according to any one of claims 1 to 8, characterized in that: The following steps are involved: Step 1: Prepare low-conductivity inner core After PDMS and its curing agent are magnetically stirred at room temperature, a TritonX-100 modifier is added and stirred evenly, and then a PEDOT:PSS aqueous solution is added and stirred evenly to obtain a composite slurry for preparing a low-conductivity inner core; A section of elastic core-spun fiber line is taken, cleaned and dried, immersed in the composite slurry and heated to cure, then treated with oxygen plasma, and then immersed in an aqueous solution of a silane coupling agent containing a mercapto group at a concentration of 15-25 mg / mL for 1.5-2 hours, taken out, washed with ethanol and dried to complete the surface mercapto grafting treatment, and obtain a low-conductive inner core; Step 2: Prepare a highly conductive film layer After the PEDOT:PSS aqueous solution, triethylene glycol and deionized water are mixed and magnetically stirred to be uniform, bovine serum albumin is added and stirred to be uniform to obtain a mixed solution for preparing a highly conductive film layer; After fixing the two ends of the low-conductivity inner core obtained in step 1, the inner core is divided into N sections along the length direction, and each section is sequentially immersed in the mixed liquid under a gradient tensile elongation and dried and solidified at room temperature to form a film layer with a gradient wrinkle depth and elongation at break; wherein the tensile elongation of the nth section is A×(Nn) / N, n is 1, 2, ..., N, and A=10%~50%; The prepared film layer is immersed in a post-treatment solution containing ZnCl2 for 0.5 to 1 hour, then taken out and washed with deionized water and dried, so that a high-conductivity film layer is formed on the surface of the low-conductivity inner core to obtain a strain sensitive element; Step 3: Sensor packaging and electrode preparation After adding triethylene glycol to the PEDOT:PSS aqueous solution and stirring it evenly with a magnetic stirrer, carbon black and KH-550 are added and stirred evenly, and then carboxylated styrene butadiene latex is added and stirred evenly with a magnetic stirrer to obtain a conductive adhesive; Select an elastic packaging tube with an inner diameter not less than the outer diameter of the strain sensitive element, and pass the strain sensitive element prepared in step 2 through the elastic packaging tube in a stretched state; fix the copper wires at both ends of the strain sensitive element through carbon fiber fixing knots, and then inject the connection between the copper wire, the carbon fiber fixing knot and the end of the high conductive film layer into one piece through a conductive adhesive to form an electrode structure; The strain sensitive element is released, and the outer end of the carbon fiber fixing knot is aligned with the outer end of the elastic packaging tube, and wire buckles are put on the edges of both ends and clamped to fix the two ends of the elastic packaging tube and the strain sensitive element, thereby obtaining the highly sensitive wide linear flexible strain sensor based on the composite gradient structure.
Citation Information
Patent Citations
Cobweb-shaped flexible strain sensor capable of identifying strain direction and preparation method thereof
CN111649665A
Crack flexible strain sensor based on graphene-gold composite film and preparation method
CN113074622A
Flexible strain sensor based on double-thread conductive yarn and preparation method thereof
CN116147475A
Flexible strain sensor with regular crack structure and manufacturing method thereof
CN110823085A
Preparation method of MXene / graphene gradient micro-fold structure with strain sensing performance
CN117053673A