A highly disordered hard carbon material
By preoxidizing and condensing the resin precursor and carbonizing in an inert atmosphere, a high disordered hard carbon material was prepared, which solved the reversible specific capacity and cycle performance of resin hard carbon materials in sodium ion batteries. The problem of the problem has achieved excellent electrochemical properties.
Patent Information
- Application Number
- CN202411165122.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-08-23
AI Technical Summary
The reversible specific capacity and cycling performance of existing resin-based hard carbon materials in the negative electrode field of sodium ion battery are not ideal, which limits its further development.
By preoxidizing the resin precursor and condensing reaction with maleic acid, a resin carbon precursor is formed, and then carbonized in an inert atmosphere, a high disorder with a layered graphite domain structure is prepared. Hard carbon material.
The hard carbon material exhibits excellent reversible specific capacity, good cycle stability and high first-time Coulomb efficiency, solving the problem of insufficient cycle performance and reversible specific capacity of existing resin-based hard carbon materials.
Smart Images

Figure CN118693275B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of new energy batteries, and in particular to a hard carbon material with a high degree of disorder, a preparation method thereof, and a battery. Background Art
[0002] In sodium-ion batteries, graphite is not suitable for storing sodium ions as a commercial negative electrode material for lithium-ion batteries because the intercalation compounds formed by sodium and graphite are thermodynamically unstable and the ionic radius of sodium ions is larger than that of lithium ions. Therefore, there is currently a lack of negative electrode materials with good electrochemical properties for sodium-ion batteries. In recent years, hard carbon has been considered a promising negative electrode material for sodium-ion batteries due to its suitable interlayer spacing, good structural stability and high reversible capacity.
[0003] Hard carbon negative electrode materials are mostly prepared by pyrolysis of biomass carbon precursors. The biomass route for preparing hard carbon has the advantages of both high performance and low cost. However, the preparation of biomass hard carbon is subject to differences in region, season, etc., which leads to unstable performance of the prepared hard carbon materials. In addition, polymer resin materials are often used to prepare hard carbon negative electrodes. Compared with natural biomass polymers, the resin precursor structure is simpler and the molecular weight is controllable. In addition, the relevant molecular structure can be selected or designed to achieve the purpose of constructing closed-cell structure and carbon defect active sites, which is operational. However, the existing resin hard carbon materials are limited in their further development in the field of sodium ion battery negative electrodes due to their poor reversible specific capacity and cycle performance. Summary of the invention
[0004] In view of this, the present invention is committed to providing a hard carbon material with a high degree of disorder, a preparation method thereof and a battery. The present invention modifies the pre-oxidized resin to prepare a resin-based hard carbon for application in sodium ion batteries. The sodium ion battery prepared using the negative electrode material exhibits excellent reversible specific capacity, good cycle stability and high first coulombic efficiency, so as to solve the problems of poor cycle performance and low reversible specific capacity of resin-based hard carbon materials in the prior art.
[0005] In order to solve the above technical problems, this application is implemented as follows:
[0006] The first aspect of the present invention provides a hard carbon material with a high degree of disorder, wherein the hard carbon material has a layered graphite-like domain structure; the carbon interlayer spacing of the hard carbon material is 0.36-0.42 nm; in the Raman spectrum of the hard carbon material, ID / IG is 0.9-1.1, wherein ID represents the Raman spectrum wavelength of 1350 cm -1 The peak intensity at IG is the wavelength of 1580 cm in the Raman spectrum. -1 The peak intensity at .
[0007] Optionally, the specific surface area of the hard carbon material is 5 to 20 m 2 / g.
[0008] Optionally, the pore volume of the hard carbon material is 0.70-0.95 cm 3 / g; and / or, the porosity of the hard carbon material is 0.1-1%; and / or, the pore size of the hard carbon material is 2-50 nm.
[0009] Optionally, the hard carbon material contains carbon, oxygen, hydrogen and nitrogen; based on the total weight of the hard carbon material, the carbon content is 85~95% by weight, the oxygen content is 0~5% by weight, the hydrogen content is 0~5% by weight, and the nitrogen content is 0~5% by weight.
[0010] A second aspect of the present invention provides a method for preparing a hard carbon material, the preparation method comprising the following steps:
[0011] S1, pre-oxidizing the resin precursor to obtain a pre-oxidized resin;
[0012] S2, mixing the pre-oxidized resin with maleic acid and a solvent to obtain a mixture, and subjecting the mixture to a condensation reaction to obtain a resin carbon precursor;
[0013] S3, placing the resin carbon precursor in an inert atmosphere for carbonization treatment.
[0014] Optionally, the resin precursor is selected from at least one of phenolic resin, epoxy resin, urea-formaldehyde resin, melamine-formaldehyde resin, acrylic resin, vinyl resin, polyester resin and polyether resin.
[0015] Optionally, the mass ratio of the preoxidized resin to maleic acid is 5-10:1; and / or, in the mixed material, the concentration of the preoxidized resin is 0.1-1 g / mL.
[0016] Optionally, the solvent is a mixed solution of ethanol and water; the volume ratio of the mixture of ethanol and water is 1:2~5.
[0017] Optionally, in step S1, the pre-oxidation treatment is carried out in an oxygen-containing atmosphere; the gas flow rate during the pre-oxidation treatment is 50~100 mL / min; the conditions for the pre-oxidation treatment include: a heating rate of 0.5~2℃ / min, a temperature of 80~200℃, and a time of 10~30h; and / or, in step S2, the conditions for the condensation reaction include: a temperature of 25~50℃, and a time of 5~10h; and / or, in step S3, the conditions for the carbonization treatment include: a heating rate of 0.5~5℃ / min, a temperature of 1000~1400℃, and a time of 3~5h; the inert atmosphere is selected from at least one of nitrogen, argon and helium.
[0018] A third aspect of the present invention provides a battery, the battery comprising a negative electrode, the negative electrode comprising a negative electrode active material, the negative electrode active material comprising the hard carbon material mentioned above and / or the hard carbon material prepared according to the above preparation method.
[0019] Through the above technical solution, the hard carbon material and its preparation method provided by the present invention have the following technical effects:
[0020] (1) The present invention performs a pre-oxidation treatment on the resin precursor to increase the oxygen-containing functional groups of the resin precursor. At the same time, since the temperature of the pre-oxidation treatment is relatively low, the movement between the polymer chains is enhanced while the network macromolecular structure is not destroyed, so that the polymer chains are cross-linked more tightly.
[0021] (2) The present invention uses maleic acid as a modifier to undergo a polycondensation reaction with a pre-oxidized or post-oxidized phenolic resin containing a large number of oxygen functional groups to crosslink into a layered network. The carboxyl functional group of maleic acid and the hydroxyl functional group of the pre-oxidized phenolic resin undergo a condensation reaction, and the originally relatively dispersed polymer chains are connected by maleic acid through new chemical bonds to form a structurally stable layered network macromolecule. Maleic acid not only has a linking effect to enhance the degree of crosslinking between phenolic resin polymers, but also inhibits the directional growth of the carbon layer during subsequent carbonization, so that it forms a layered graphite-like domain structure. The hard carbon material prepared by the method of the present invention has an enlarged interlayer spacing, an increased pore structure, and improved stability. The electrochemical performance shows a high sodium storage capacity and excellent rate and cycle stability.
[0022] Other features and advantages of the present invention will be described in detail in the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] The accompanying drawings are used to provide further understanding of the present invention and constitute a part of the specification. Together with the following specific embodiments, they are used to explain the present invention, but do not constitute a limitation of the present invention.
[0024] Figure 1 Shown is the TEM image of the hard carbon material prepared in Example 1.
[0025] Figure 2 Shown are the thermal gravimetric curves of the maleic acid-modified phenolic resin carbon precursor (MA-PF) prepared in Example 1 and the common phenolic resin (PF).
[0026] Figure 3 Shown is the Raman spectrum of the hard carbon material prepared in Example 1.
[0027] Figure 4Shown are XRD patterns of the hard carbon material prepared from the maleic acid-modified phenolic resin carbon precursor (MA-PF) in Example 1 and a common phenolic resin (PF)-based hard carbon material. DETAILED DESCRIPTION
[0028] The present invention discloses a hard carbon material with high disorder, a preparation method thereof and a battery. Those skilled in the art can refer to the content of this article and appropriately improve the process parameters to achieve the same. It should be particularly noted that all similar substitutions and modifications are obvious to those skilled in the art, and they are all deemed to be included in the present invention. The methods and applications of the present invention have been described through preferred embodiments, and relevant personnel can obviously modify or appropriately change and combine the methods and applications described herein without departing from the content, spirit and scope of the present invention to implement and apply the technology of the present invention.
[0029] In the description of the present invention, a list of items connected by the term "at least one of" or other similar terms may mean any combination of the listed items. For example, if items A, B are listed, the phrase "at least one of A, B" means only A; only B; or A and B. In another example, if items A, B, C are listed, the phrase "at least one of A, B, C" means only A; or only B; only C; A and B (excluding C); A and C (excluding B); B and C (excluding A); or all of A, B, and C. Item A may include a single element or multiple elements. Item B may include a single element or multiple elements. Item C may include a single element or multiple elements.
[0030] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range or the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0031] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.
[0032] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.
[0033] If there is no special explanation, the "include" and "comprising" mentioned in this application represent open-ended or closed-ended expressions. For example, the "include" and "comprising" may represent that other components not listed may also be included or only the listed components may be included or only the listed components may be included.
[0034] In order to solve the problem of unsatisfactory reversible specific capacity and cycle performance of resin-based hard carbon materials in the prior art, the present invention adopts the following technical solution:
[0035] The first aspect of the present invention provides a hard carbon material with a high degree of disorder, wherein the hard carbon material has a layered graphite-like domain structure; the carbon interlayer spacing of the hard carbon material is 0.36-0.42 nm; in the Raman spectrum of the hard carbon material, ID / IG is 0.9-1.1, wherein ID represents the Raman spectrum wavelength of 1350 cm -1 The peak intensity at IG is the wavelength of 1580 cm in the Raman spectrum. -1 The peak intensity at .
[0036] The hard carbon material provided by the present invention has a layered graphite-like domain structure and an increased interlayer spacing, showing good sodium storage capacity and excellent rate and cycle performance.
[0037] In the Raman spectrum of the hard carbon material provided by the present invention, ID / IG is 0.9-1.1, and ID represents the wavelength of the Raman spectrum of 1350 cm -1 The peak intensity at IG belongs to the boundary vibration mode of the disorder-induced hexagonal Brillouin zone, which represents the defects of the C atom lattice. Specifically, it can indicate the lattice vibration intensity caused by the edge defects of the hard carbon material or the impurities in the hard carbon material, reflecting the disorder degree of the hard carbon material. IG indicates that the wavelength of the Raman spectrum is 1580 cm -1 The peak intensity at can specifically represent the in-plane stretching vibration intensity of sp2 hybridized C atoms in hard carbon materials, which belongs to the stretching vibration mode of in-plane bonds of carbon atoms and is related to the degree of graphitization. The disorder of hard carbon materials can be determined by the ratio of ID / IG. The larger the ID / IG value, the greater the disorder of hard carbon materials, the more sodium ion migration paths there are, which is beneficial to improving battery electrical performance.
[0038] According to the present invention, the specific surface area of the hard carbon material can be 5 to 20 m 2 / g; For example, the specific surface area of the hard carbon material can be 5 m 2 / g, 10 m 2 / g, 15 m 2 / g and 20 m 2 / g or any value in the range of any two of the above values. In the present invention, if the specific surface area of the hard carbon material is too large, it will increase the initial gram capacity and reduce the initial coulombic efficiency; if the specific surface area of the hard carbon material is too small, it will reduce the sodium ion active sites, which is not conducive to the improvement of the sodium storage capacity. Preferably, the specific surface area of the hard carbon material can be 5~10m 2 / g.
[0039] The hard carbon material in the present invention has a rich mesoporous structure, which is beneficial to increase the sodium capacity. Among them, the ultra-micropores, large pore volume, low specific surface area and closed pores of the hard carbon material can reduce the influence of the solid electrolyte interface film on sodium storage, which is beneficial to the insertion / extraction of sodium ions.
[0040] According to the present invention, the pore volume of the hard carbon material can be 0.70~0.95cm 3 / g, and illustratively, the pore volume of the hard carbon material may be 0.70 cm 3 / g, 0.75 cm 3 / g, 0.80 cm 3 / g, 0.85 cm 3 / g, 0.9 cm 3 / g and 0.95 cm 3 / g or any value within the range of values formed by any two of the above values. In the present invention, the pore volume provides sodium storage capacity for sodium ions, which is beneficial to the improvement of platform capacity and cycle stability. However, if the pore volume barrier is too large, sodium ions will be difficult to embed, which is not conducive to the improvement of rate performance and kinetic performance. If the pore volume is too large, sodium ions cannot be stored therein, and excessive electrolyte will be consumed, reducing the initial coulombic efficiency. Preferably, the pore volume of the hard carbon material is 0.85~0.95cm 3 / g.
[0041] According to the present invention, the porosity of the hard carbon material affects its storage efficiency for sodium ions. The presence of pores can change the solvation structure of the electrolyte, and through pre-desolvation, a highly aggregated electrolyte structure is generated, thereby improving the reduction decomposition efficiency of the electrolyte, and then improving the coulombic efficiency of the hard carbon negative electrode. The porosity of the hard carbon material in the present invention can be 0.1~1%. For example, the porosity of the hard carbon material can be any value in 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9% and 1%, or any value in the range of any two of the above values. In the present invention, too high a porosity will reduce the density of the material, because the pores are non-entity gaps, which reduce the density of the material and are not conducive to the energy density of the battery. The pores will become the concentration point of stress in the material, causing the material to easily crack when subjected to load, thereby reducing the strength and hardness of the material. Preferably, the porosity of the hard carbon material is 0.2~0.5%.
[0042] According to the present invention, the pore structure of the hard carbon material can provide a sodium ion transmission channel, which is beneficial to the migration of sodium ions and can improve the kinetic performance. In the present invention, the pore size of the hard carbon material can be 2 to 50 nm. Exemplarily, the pore size of the hard carbon material can be any value among 2 nm, 10 nm, 20 nm, 30 nm, 40 nm and 50 nm or any value within the range of any two of the above values. In the present invention, too small an pore size will make it difficult for sodium ions to embed, and too large an pore size will lead to an increase in the specific surface area, affecting the first coulombic efficiency. Preferably, the pore size of the hard carbon material is 2 to 10 nm.
[0043] In one embodiment of the present invention, the hard carbon material may contain carbon, oxygen, hydrogen and nitrogen. Based on the total weight of the hard carbon material, the carbon content may be 85-95% by weight, the oxygen content may be 0-5% by weight, the hydrogen content may be 0-5% by weight, and the nitrogen content may be 0-5% by weight.
[0044] As a preferred embodiment of the present invention, based on the total weight of the hard carbon material, the carbon content is 90-95% by weight, the oxygen content is 1-2% by weight, the hydrogen content is 1-2% by weight, and the nitrogen content is 2-5% by weight.
[0045] A second aspect of the present invention provides a method for preparing a hard carbon material, the preparation method comprising the following steps:
[0046] S1, pre-oxidizing the resin precursor to obtain a pre-oxidized resin;
[0047] S2, mixing the pre-oxidized resin with maleic acid and a solvent to obtain a mixture, and subjecting the mixture to a condensation reaction to obtain a resin carbon precursor;
[0048] S3, placing the resin carbon precursor in an inert atmosphere for carbonization treatment.
[0049] The method of the present invention adds pre-oxidation treatment to the resin precursor to increase its oxygen-containing functional groups. At the same time, since the low temperature is not high, the movement between the polymer chains is strengthened while the reticular macromolecular structure is not destroyed, so that the polymer chains are more closely cross-linked. Then maleic acid is added as a modifier to react with the pre-oxidized phenolic resin. The polymer chains that are originally more dispersed are connected into a layered reticular macromolecule with a stable structure through maleic acid by using new chemical bonds. Thereby, the directional growth of the carbon layer is suppressed in the subsequent carbonization, so that it forms a layered graphite-like domain structure, increases the disorder, increases the interlayer spacing, and increases the pore content, showing good sodium storage capacity and excellent rate and cycle performance.
[0050] According to the present invention, the resin precursor can be selected from at least one of phenolic resin, epoxy resin, urea-formaldehyde resin, melamine formaldehyde resin, acrylic resin, vinyl resin, polyester resin and polyether resin. The polyester resin involved in the present invention is also called oil-free alkyd resin, which is formed by polycondensation of polyols and polyacids through ester bonds. It is distinguished according to its monomers. Specifically, the monomers include ethylene glycol, propylene glycol, 2-methyl-1,3-propanediol, butanediol, hexanediol, diethylene glycol, 1,4-cyclohexanedimethanol, propylene glycol, trimethylolpropane, pentaerythritol, etc.; the polyacids include isophthalic acid, phthalic anhydride, terephthalic acid, adipic acid, sebacic acid, glutaric acid, and succinic acid; illustratively, the polyester resin selected from the polyester resin can be selected from at least one of propylene glycol and isophthalic acid / phthalic anhydride / terephthalic acid. The polyether resin involved in the present invention is a composite material with polyetheretherketone (PEEK) resin as the matrix and fiber (or its fabric) reinforced. Polyetheretherketone is prepared by polycondensation using 4,4'-difluorobenzophenone, hydroquinone and sodium carbonate or potassium carbonate as raw materials and phenol as solvent. Exemplarily, the polyether resin can be selected from at least one of silane-terminated polyether-based resin and polyphenylene ether resin.
[0051] In a preferred embodiment of the present invention, the resin precursor is a phenolic resin. Phenolic resin has abundant oxygen functional groups, and cross-linking reaction with maleic acid effectively improves the stability of the resin molecular chain, and also inhibits the directional growth of the carbon layer in the subsequent carbonization, eliminates oxygen defects, enhances the structural disorder of the carbon material, and expands the interlayer spacing.
[0052] The preparation process of the present invention may further include a cooling step of the pre-oxidized resin. For example, the pre-oxidized resin prepared in step S1 may be cooled to room temperature and then mixed with maleic acid and a solvent to obtain a mixed material.
[0053] According to the present invention, the mass ratio of the preoxidized resin to the maleic acid may be 5 to 10:1; illustratively, the mass ratio of the preoxidized resin to the maleic acid may be any value among 5:1, 6:1, 7:1, 8:1, 9:1 and 10:1 or any value within the range of any two of the above values. Preferably, the mass ratio of the preoxidized resin to the maleic acid may be 5:1.
[0054] According to the present invention, in the mixed material, the concentration of the preoxidized resin can be 0.1-1 g / mL. Exemplarily, the concentration of the preoxidized resin can be any value among 0.1 g / mL, 0.2 g / mL, 0.3 g / mL, 0.4 g / mL, 0.5 g / mL, 0.6 g / mL, 0.7 g / mL, 0.8 g / mL, 0.9 g / mL and 1 g / mL or any value within the range of any two of the above values.
[0055] According to the present invention, the solvent is a conventional solvent in the art, for example, can be selected from ethanol and / or water.
[0056] In a preferred embodiment of the present invention, the solvent is a mixed solution of ethanol and water. Further preferably, the volume ratio of ethanol and water is 1:2 to 5. Exemplarily, the volume ratio of ethanol and water can be any value among 1:2, 1:3, 1:4 and 1:5 or any value within the range of any two of the above values.
[0057] As an embodiment of the present invention, in step S1, the pre-oxidation treatment is carried out in an oxygen-containing atmosphere; preferably, the oxygen-containing atmosphere is air and / or oxygen; the conditions of the pre-oxidation treatment include: a heating rate of 0.5~2°C / min, a temperature of 80~200°C, and a time of 10~30h; preferably, the temperature of the pre-oxidation treatment is 80~150°C; air and / or oxygen need to be introduced during the pre-oxidation treatment, and the gas flow rate of air and / or oxygen is 50~100 mL / min.
[0058] As an embodiment of the present invention, in step S2, the conditions for the condensation reaction may include: a temperature of 25-50° C. and a time of 5-10 hours.
[0059] As an embodiment of the present invention, in step S3, the conditions of the carbonization treatment may include: a heating rate of 0.5-5°C / min, a temperature of 1000-1400°C, and a time of 3-5h; and an inert atmosphere selected from at least one of nitrogen, argon, and helium. Optionally, an inert gas needs to be introduced during the carbonization treatment, and the gas flow rate of the inert gas is 40-80 mL / min.
[0060] A third aspect of the present invention provides a battery, which includes a negative electrode, wherein the negative electrode includes a negative electrode active material, and the negative electrode active material includes the hard carbon material mentioned above and / or the hard carbon material prepared according to the above preparation method.
[0061] In the embodiment of the present invention, the battery structure includes but is not limited to button batteries, soft-pack batteries, cylindrical batteries, etc.
[0062] The present invention has no particular restrictions on the positive electrode sheet, separator, and electrolyte in the battery, and those skilled in the art can select them according to actual needs as long as the purpose of the present invention can be achieved.
[0063] The present invention is further described in detail by way of examples. The raw materials used in the examples can be obtained through commercial sources.
[0064] Example 1
[0065] This embodiment provides a method for preparing a hard carbon material, and the specific preparation steps are as follows:
[0066] (1) 50 g of phenolic resin was placed in a porcelain boat for pre-oxidation treatment to obtain a pre-oxidized phenolic resin rich in oxygen-containing functional groups, wherein the pre-oxidation treatment conditions included: heating to 120° C. at a heating rate of 1° C. / min in an air atmosphere and maintaining the temperature for 20 hours.
[0067] (2) After the prepared pre-oxidized phenolic resin is cooled to room temperature, 40 g of the pre-oxidized phenolic resin powder is weighed and added to a mixture of 20 ml of ethanol and 60 ml of deionized water. After mixing evenly, 8 g of maleic acid is added dropwise to obtain a mixed material; the mixed material is subjected to a condensation reaction, wherein the condensation reaction step comprises: stirring at 40°C for 5 hours to obtain a condensed material, and the condensed material is washed, filtered, freeze-dried, and then obtained to obtain a maleic acid-modified phenolic resin carbon precursor. The thermal weight loss comparison curves of the maleic acid-modified phenolic resin carbon precursor prepared in this embodiment and the ordinary phenolic resin (phenolic resin not pre-oxidized in step (1)) are shown in FIG. Figure 2 shown.
[0068] (3) High-temperature carbonization of the maleic acid-modified phenolic resin carbon precursor obtained above, wherein the high-temperature carbonization reaction step includes: heating to 1200°C at a heating rate of 2°C / min in a nitrogen atmosphere and maintaining for 5 hours, and finally obtaining the hard carbon material of this embodiment. The TEM image of the hard carbon material prepared in this embodiment is as follows: Figure 1 The Raman spectrum of the hard carbon material prepared in this embodiment is shown in Figure 3 As shown in FIG. 1 , the ID / IG of the hard carbon material is 1.02. The XRD pattern of the hard carbon material prepared in this embodiment is shown in FIG. Figure 4 As shown, the interlayer spacing in XRD is calculated using the Bragg equation (2dSinθ=nλ), that is, the (002) crystal plane angle shifts to the left, indicating that the interlayer spacing increases.
[0069] Example 2
[0070] This embodiment provides a method for preparing a hard carbon material, and the specific preparation steps are as follows:
[0071] (1) 50 g of phenolic resin was placed in a porcelain boat for pre-oxidation treatment to obtain a pre-oxidized phenolic resin rich in oxygen-containing functional groups, wherein the pre-oxidation treatment conditions included: heating to 80° C. at a heating rate of 1° C. / min in an air atmosphere and maintaining the temperature for 20 hours.
[0072] (2) After the prepared pre-oxidized phenolic resin is cooled to room temperature, 40 g of the pre-oxidized phenolic resin powder is weighed and added to a mixture of 20 ml of ethanol and 60 ml of deionized water. After mixing evenly, 8 g of maleic acid is added dropwise to obtain a mixture; the mixture is subjected to a condensation reaction, wherein the condensation reaction comprises the steps of: stirring at 40° C. for 5 hours to obtain a condensed material, washing the condensed material, filtering, and freeze-drying to obtain a maleic acid-modified phenolic resin carbon precursor.
[0073] (3) High-temperature carbonization of the maleic acid-modified phenolic resin carbon precursor obtained above, wherein the high-temperature carbonization reaction step comprises: heating to 1200°C at a heating rate of 2°C / min in a nitrogen atmosphere and maintaining for 5 hours, thereby finally obtaining the hard carbon material of this embodiment.
[0074] Example 3
[0075] This embodiment provides a method for preparing a hard carbon material, and the specific preparation steps are as follows:
[0076] (1) 50 g of phenolic resin was placed in a porcelain boat for pre-oxidation treatment to obtain a pre-oxidized phenolic resin rich in oxygen-containing functional groups, wherein the pre-oxidation treatment conditions included: heating to 120° C. at a heating rate of 1° C. / min in an air atmosphere and maintaining the temperature for 20 hours.
[0077] (2) After the prepared pre-oxidized phenolic resin is cooled to room temperature, 40 g of the pre-oxidized phenolic resin powder is weighed and added to a mixture of 20 ml of ethanol and 60 ml of deionized water. After mixing evenly, 4 g of maleic acid is added dropwise to obtain a mixture; the mixture is subjected to a condensation reaction, wherein the condensation reaction comprises the steps of: stirring at 40° C. for 5 h to obtain a condensed material, washing the condensed material, filtering, and freeze-drying to obtain a maleic acid-modified phenolic resin carbon precursor.
[0078] (3) High-temperature carbonization of the maleic acid-modified phenolic resin carbon precursor obtained above, wherein the high-temperature carbonization reaction step comprises: heating to 1200°C at a heating rate of 2°C / min in a nitrogen atmosphere and maintaining for 5 hours, thereby finally obtaining the hard carbon material of this embodiment.
[0079] Example 4
[0080] This embodiment provides a method for preparing a hard carbon material, and the specific preparation steps are as follows:
[0081] (1) 50 g of phenolic resin was loaded into a porcelain boat and subjected to a pre-oxidation treatment to obtain a pre-oxidized phenolic resin having abundant oxygen-containing functional groups, wherein the pre-oxidation treatment conditions included: heating to 200° C. at a heating rate of 1° C. / min in an air atmosphere and maintaining the temperature for 20 hours.
[0082] (2) After the prepared pre-oxidized phenolic resin is cooled to room temperature, 40 g of the pre-oxidized phenolic resin powder is weighed and added to a mixture of 20 ml of ethanol and 60 ml of deionized water. After mixing evenly, 8 g of maleic acid is added dropwise to obtain a mixture; the mixture is subjected to a condensation reaction, wherein the condensation reaction comprises the steps of: stirring at 40° C. for 5 hours to obtain a condensed material, washing the condensed material, filtering, and freeze-drying to obtain a maleic acid-modified phenolic resin carbon precursor.
[0083] (3) High-temperature carbonization of the maleic acid-modified phenolic resin carbon precursor obtained above, wherein the high-temperature carbonization reaction step comprises: heating to 1200°C at a heating rate of 5°C / min in a nitrogen atmosphere and maintaining for 5 hours, thereby finally obtaining the hard carbon material of this embodiment.
[0084] Example 5
[0085] This embodiment provides a method for preparing a hard carbon material, and the specific preparation steps are as follows:
[0086] (1) 50 g of phenolic resin was placed in a porcelain boat for pre-oxidation treatment to obtain a pre-oxidized phenolic resin rich in oxygen-containing functional groups, wherein the pre-oxidation treatment conditions included: heating to 200° C. at a heating rate of 1° C. / min in an air atmosphere and maintaining the temperature for 20 hours.
[0087] (2) After the prepared pre-oxidized phenolic resin is cooled to room temperature, 40 g of the pre-oxidized phenolic resin powder is weighed and added to a mixture of 10 ml of ethanol and 30 ml of deionized water, and 8 g of maleic acid is added dropwise after mixing evenly to obtain a mixed material; the mixed material is subjected to a condensation reaction, wherein the condensation reaction comprises the steps of: stirring at 40° C. for 5 hours to obtain a condensed material, washing the condensed material, filtering, and freeze-drying to obtain a maleic acid-modified phenolic resin carbon precursor;
[0088] (3) High-temperature carbonization of the maleic acid-modified phenolic resin carbon precursor obtained above, wherein the high-temperature carbonization reaction step comprises: heating to 1200°C at a heating rate of 2°C / min in a nitrogen atmosphere and maintaining for 5 hours, thereby finally obtaining the hard carbon material of this embodiment.
[0089] Comparative Example 1
[0090] The specific preparation steps of the carbon material of this comparative example are as follows:
[0091] (1) 50 g of phenolic resin was placed in a porcelain boat for pre-oxidation treatment to obtain a pre-oxidized phenolic resin rich in oxygen-containing functional groups, wherein the pre-oxidation treatment conditions included: heating to 120° C. at a heating rate of 1° C. / min in an air atmosphere and maintaining the temperature for 20 hours.
[0092] (2) The prepared pre-oxidized phenolic resin is cooled to room temperature and then subjected to high-temperature carbonization, wherein the high-temperature carbonization reaction step comprises: heating to 1200° C. at a heating rate of 2° C. / min in a nitrogen atmosphere and maintaining for 5 h, thereby finally obtaining the carbon material of this comparative example.
[0093] Comparative Example 2
[0094] The specific preparation steps of the carbon material of this comparative example are as follows:
[0095] (1) Weighing 40 g of phenolic resin and adding it to a mixture of 20 ml of ethanol and 60 ml of deionized water, mixing evenly, and then dropping 8 g of maleic acid to obtain a mixture; subjecting the mixture to a condensation reaction, wherein the condensation reaction comprises: stirring at 40° C. for 5 h to obtain a condensed material, washing the condensed material, filtering, freeze-drying, and obtaining a maleic acid-modified phenolic resin carbon precursor.
[0096] (2) The maleic acid-modified phenolic resin carbon precursor obtained above is subjected to high temperature carbonization, wherein the high temperature carbonization reaction step comprises: heating to 1200° C. at a heating rate of 2° C. / min in a nitrogen atmosphere and maintaining for 5 h, thereby finally obtaining the carbon material of this comparative example.
[0097] Comparative Example 3
[0098] The specific preparation steps of the carbon material of this comparative example are as follows:
[0099] (1) 50 g of phenolic resin was placed in a porcelain boat for pre-oxidation treatment to obtain a pre-oxidized phenolic resin rich in oxygen-containing functional groups, wherein the pre-oxidation treatment conditions included: heating to 80° C. at a heating rate of 1° C. / min in an air atmosphere and maintaining the temperature for 20 hours.
[0100] (2) After the prepared pre-oxidized phenolic resin is cooled to room temperature, 40 g of the pre-oxidized phenolic resin powder is weighed and added to a mixture of 20 ml of ethanol and 60 ml of deionized water, and 8 g of maleic anhydride is added dropwise after mixing evenly to obtain a mixed material; the mixed material is subjected to a condensation reaction, wherein the condensation reaction comprises the steps of: stirring at 40° C. for 5 hours to obtain a condensed material, washing the condensed material, filtering, and freeze-drying to obtain a maleic anhydride-modified phenolic resin carbon precursor;
[0101] (3) The maleic anhydride-modified phenolic resin carbon precursor obtained above is subjected to high temperature carbonization, wherein the high temperature carbonization reaction step comprises: heating to 1200°C at a heating rate of 2°C / min in a nitrogen atmosphere and maintaining for 5 hours, thereby finally obtaining the hard carbon material of this comparative example.
[0102] Performance Testing
[0103] The resin hard carbon material in Examples 1 to 5 and Comparative Examples 1 to 3 was used as the negative electrode, the metal sodium sheet was used as the positive electrode, and 1.0 mol / LLiPF6 / EC (ethylene carbonate) + DMC (dimethyl carbonate) + FEC (fluoroethylene carbonate) (the volume ratio of EC, DMC and FEC was 4.5:4.5:1) was used as the electrolyte, and CR2032 button batteries were assembled in an argon glove box.
[0104] The GCD was tested using the LAND battery test system in a voltage window of 0-2V. The test conditions and results are as follows:
[0105] Test method for first discharge capacity, first charge capacity and first coulombic efficiency: button cells are tested for constant current charge and discharge at a current density of 100 mA / g, with a voltage range of 0.01~2 V. Specifically: discharge at a constant current of 100 mA / g to 0.01V, and record the discharge capacity at this time as the first discharge capacity; then charge at a constant current of 100 mA / g to 2V, and record the charge capacity at this time as the first charge capacity; first coulombic efficiency = first charge capacity / first discharge capacity*100%. Specific values are shown in Table 1 (first discharge capacity, first charge capacity and first coulombic efficiency of button half-cells prepared in Examples 1~5 and Comparative Examples 1~3).
[0106] Cycle performance test method: button battery is subjected to constant current charge and discharge test at a current density of 500mA / g, with a voltage range of 0.01~2V and 200 cycles. Specifically: discharge at a constant current of 500 mA / g to 0.01V, and record the discharge capacity at this time as the first discharge capacity; then charge at a constant current of 500 mA / g to 2V, and record the charge capacity at this time as the first charge capacity; repeat the above charge and discharge cycle for 200 cycles, record the discharge capacity of the 200th cycle, and the capacity retention rate = discharge capacity of the 200th cycle / first discharge capacity*100%. See Table 2 for specific values (capacity retention rate of button half-batteries of electrode materials prepared in Examples 1~5 and Comparative Examples 1~3 after 200 cycles).
[0107] Table 1
[0108]
[0109] Table 2
[0110]
[0111] It can be seen from Table 1 and Table 2 that the button-type half-cells prepared from the hard carbon materials of Examples 1 to 5 have a high first coulombic efficiency (over 85%), while the first coulombic efficiency of the button-type half-cell prepared from Comparative Example 1 is only 68%. The button-type half-cells prepared from the hard carbon materials of Examples 1 to 5 all have a good cycle retention rate (greater than 89%), showing excellent cycle stability. The capacity retention rate of the comparative example is only about 70-80%.
[0112] Comparing the embodiments with the comparative examples, compared with embodiment 1, embodiment 2 reduces the pre-oxidation treatment temperature, resulting in a slight decrease in the content of oxygen functional groups, fewer groups that can participate in cross-linking later, a decrease in the degree of cross-linking during high-temperature carbonization, and an increase in porosity, so that the first coulombic efficiency decreases; embodiment 3 uses a lower content of the modifier maleic acid, the modification effect decreases, so that some oxygen-containing functional groups fail to react, oxygen defects increase, resulting in more active substances consumed, and irreversible capacity increases; embodiment 4 improves the heating rate of high-temperature carbonization, so that the plane incompleteness increases during the growth of the carbon layer, defects increase, specific surface area increases, and the irreversible capacity of the first cycle increases; embodiment 5 increases the concentration of the pre-oxidized phenolic resin, Thereby affecting the dehydration condensation reaction of the modifier and the pre-oxidized phenolic resin, there is an insufficient reaction due to the insufficient amount of the modifier maleic acid, and the functional groups that do not participate in the reaction are prone to form oxygen vacancy defects in the subsequent carbonization process, thereby reducing the first coulomb efficiency; the preparation process of comparative example 1 does not involve modification, and the pre-oxidized phenolic resin is directly carbonized at high temperature, and the prepared material has too many defects, and the first coulomb efficiency and capacity retention rate are greatly reduced; comparative example 2 does not involve a pre-oxidation process, so that the modifier cannot regulate the cross-linking process, and thus cannot affect the growth of the subsequent carbon layer; comparative example 3 uses maleic anhydride without a carboxyl group as a modifier, and cannot modify the defects generated by pre-oxidation and change the interlayer spacing. In summary, it can be seen that the hard carbon material prepared in Examples 1 to 5 of the present invention eliminates defects and enhances the structural disorder of the carbon material by adjusting the cross-linking reaction between the phenolic resin and maleic acid during the preparation process, and enhances the structural stability while expanding the interlayer spacing, which is beneficial to the rate and cycle performance.
[0113] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a hard carbon material, characterized in that: The preparation method comprises the following steps: S1, pre-oxidizing the resin precursor to obtain a pre-oxidized resin; S2, mixing the pre-oxidized resin with maleic acid and a solvent to obtain a mixture, and subjecting the mixture to a condensation reaction to obtain a resin carbon precursor; S3, placing the resin carbon precursor in an inert atmosphere for carbonization treatment; The hard carbon material has a layered graphite-like domain structure; the carbon interlayer spacing of the hard carbon material is 0.36-0.42 nm; in the Raman spectrum of the hard carbon material, ID / IG is 0.9-1.1, wherein ID represents the wavelength of the Raman spectrum of 1350 cm -1 The peak intensity at IG is 1580 cm -1 The peak intensity at .
2. The preparation method according to claim 1, characterized in that: The resin precursor is selected from at least one of phenolic resin, epoxy resin, urea-formaldehyde resin, melamine-formaldehyde resin, acrylic resin, vinyl resin, polyester resin and polyether resin.
3. The preparation method according to claim 1, characterized in that: The mass ratio of the pre-oxidized resin to the maleic acid is 5-10:1; And / or, in the mixed material, the concentration of the pre-oxidized resin is 0.1-1 g / mL.
4. The preparation method according to claim 1, characterized in that: The solvent is a mixed solution of ethanol and water; the volume ratio of the mixed solution of ethanol and water is 1:2-5.
5. The preparation method according to claim 1, characterized in that: In step S1, the pre-oxidation treatment is carried out in an oxygen-containing atmosphere; the gas flow rate during the pre-oxidation treatment is 50-100 mL / min; The pre-oxidation treatment conditions include: a heating rate of 0.5-2°C / min, a temperature of 80-200°C, and a time of 10-30h; And / or, in step S2, the conditions of the condensation reaction include: temperature of 25-50° C., time of 5-10 h; And / or, in step S3, the conditions of the carbonization treatment include: a heating rate of 0.5-5°C / min, a temperature of 1000-1400°C, and a time of 3-5h; and the inert atmosphere is selected from at least one of nitrogen, argon and helium.
6. A highly disordered hard carbon material, characterized in that: The hard carbon material is prepared according to any one of the preparation methods of claims 1 to 5.
7. The hard carbon material according to claim 6, characterized in that The specific surface area of the hard carbon material is 5 to 20 m 2 / g.
8. The hard carbon material according to claim 6, characterized in that The pore volume of the hard carbon material is 0.70-0.95 cm 3 / g; and / or, the porosity of the hard carbon material is 0.1-1%; And / or, the pore size of the hard carbon material is 2-50 nm.
9. The hard carbon material according to claim 6, characterized in that The hard carbon material contains carbon, oxygen, hydrogen and nitrogen. Based on the total weight of the hard carbon material, the carbon content is 85-95% by weight, the oxygen content is 0-5% by weight, the hydrogen content is 0-5% by weight, and the nitrogen content is 0-5% by weight.
10. A battery, characterized in that: The battery comprises a negative electrode, the negative electrode comprises a negative electrode active material, and the negative electrode active material comprises the hard carbon material according to any one of claims 6 to 9.
Citation Information
Patent Citations
Hard carbon material, preparation method and application thereof, and battery
CN118448630A