Batteries and battery packs
By designing the appropriate welding area and effective area coefficient in the battery, the problem that the connecting sheet cannot take into account both the overcurrent capability and structural size is solved, the energy density and space utilization of the battery are improved, and the problem of excessive temperature and dummy welding is avoided. .
Patent Information
- Application Number
- CN202411180236.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-08-27
AI Technical Summary
The existing connecting plates cannot take into account the problems of overcurrent capability and structural size, which affects the energy density and space utilization of the battery.
By designing the appropriate solder area and effective area coefficient in the battery, the overcurrent capability of the connecting sheet is ensured, while reducing weight and space occupancy, and improving the battery's capability density.
It realizes that while ensuring the overcurrent capability of the battery, the weight and volume of the connecting piece are reduced, the temperature is too high and the problem of dummy welding is avoided, and the space utilization and performance of the battery are improved.
Smart Images

Figure CN118693472B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of batteries, and in particular to batteries and battery packs. Background Art
[0002] The connecting piece is a metal conductor used to lead the current of the electrode group. One end of the connecting piece is welded to the pole ear of the electrode group, and the other end of the connecting piece is welded to the pole column, so as to realize the current transfer inside and outside the battery. With the increasing application of power batteries in vehicles, users have higher and higher demands for fast charging of batteries. Therefore, the requirements for the overcurrent capacity of the connecting piece during the use of the battery are getting higher and higher. However, the structural design of the connecting piece also has an important influence on the energy density of the battery. Therefore, while improving the overcurrent capacity of the connecting piece, the structural size of the connecting piece should also be considered. Summary of the invention
[0003] In view of this, the present invention provides a battery and a battery pack to solve the problem that the connecting piece in the prior art cannot take into account both the overcurrent capability and the structural size.
[0004] In a first aspect, the present invention provides a battery, comprising: a pole group, provided with at least one, the pole group including a pole ear; a connecting piece, including a pole ear welding portion, the pole ear and the pole ear welding portion are welded to form a weld mark; wherein the maximum passing current of the weld mark is The total area of all the welding marks corresponding to the pole ears of the same polarity of all the pole groups is , the effective area coefficient of the weld print is , the flow coefficient of the weld print is ,satisfy , The unit is A, The unit is mm², The unit is A / mm²; the capacity of the battery is The maximum charge and discharge rate of the battery is , the overcurrent safety factor of the battery is ,satisfy , , The unit is Ah, The unit is 1 / h.
[0005] Beneficial effect: By dividing the total area of all weld marks corresponding to the same polarity of the pole ears of all pole groups The effective area coefficient of the weld print is , the current coefficient of the weld print is , the battery capacity is And the maximum charge and discharge rate of the battery is The relationship between the tab and the connecting piece is limited so that the weld mark between the tab and the connecting piece has an appropriate area, which can not only ensure the overcurrent capacity of the connecting piece during the use of the battery, but also enable the connecting piece to have an appropriate structural size, reduce the weight of the connecting piece, reduce the space occupied by the connecting piece in the battery, and improve the capacity density of the battery.
[0006] In an optional embodiment, the overcurrent safety factor of the battery satisfy .
[0007] Beneficial effect: While preventing the battery from being too hot during charge and discharge at a large rate, the connecting piece is ensured to have a suitable size.
[0008] In an optional embodiment, the battery is a blade battery, and the overcurrent safety factor of the battery is satisfy ; Or, the battery is a square shell battery, and the overcurrent safety factor of the battery is satisfy .
[0009] In an optional embodiment, the maximum charge and discharge rate of the battery satisfy .
[0010] In an optional embodiment, the effective area coefficient of the weld print is satisfy .
[0011] Beneficial effect: while ensuring that the weld mark has a sufficient effective area to ensure the flow of current through the connecting piece, the implementation of the welding process is facilitated.
[0012] In an optional embodiment, the area of the weld mark corresponding to each of the tabs is , the number of pole ears of the same polarity in each pole group is , the number of pole groups is ,satisfy , The unit is mm², , .
[0013] In an optional embodiment, the area of the electrode tab welding portion is ,satisfy , The unit is mm².
[0014] Beneficial effect: While ensuring that the welding part of the pole ear has enough area to accommodate the weld mark, the overall volume of the connecting piece is prevented from being too large, thereby improving the space utilization of the battery.
[0015] In an optional embodiment, the weld mark is a rectangular structure, and the length of the weld mark is , the width of the weld mark is ,satisfy , , .
[0016] In an optional embodiment, the minimum distance from the edge of the weld mark to the edge corresponding to the electrode tab welding portion is ,satisfy .
[0017] Beneficial effect: It prevents the edge of the weld mark from being too close to the edge of the welding part of the pole ear, thereby preventing the pole ear from being poorly welded.
[0018] In a second aspect, the present invention further provides a battery pack, comprising the above-mentioned battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0020] Figure 1 A schematic diagram of a connection structure between an electrode group and a connecting piece according to an embodiment of the present invention;
[0021] Figure 2 for Figure 1 A schematic diagram of the partial enlarged structure of the middle connecting piece and the tab;
[0022] Figure 3 A schematic diagram of a connection structure between another electrode group and a connecting piece according to an embodiment of the present invention;
[0023] Figure 4 A schematic diagram of a connection structure between another connecting sheet and a tab according to an embodiment of the present invention;
[0024] Figure 5 A schematic diagram of a connection structure between another electrode group and a connecting piece according to an embodiment of the present invention;
[0025] Figure 6 A schematic diagram of the weld print area on the outer surface of the welding point between the electrode tab and the electrode tab welding portion according to an embodiment of the present invention;
[0026] Figure 7 It is a schematic diagram of the actual welding area of the electrode tab and the electrode tab welding part in an embodiment of the present invention.
[0027] Description of reference numerals:
[0028] 1. Pole group; 11. Pole ear; 2. Connecting piece; 21. Pole ear welding part; 3. Weld mark. DETAILED DESCRIPTION
[0029] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of the present invention.
[0030] Combine the following Figures 1 to 5 , describing an embodiment of the present invention.
[0031] According to an embodiment of the present invention, on the one hand, a battery is provided, comprising: an electrode group 1, provided with at least one, the electrode group 1 includes a pole ear 11; a connecting sheet 2, including a pole ear welding portion 21, the pole ear 11 and the pole ear welding portion 21 are welded to form a weld mark 3; wherein the maximum passing current of the weld mark 3 is The total area of all weld marks 3 corresponding to the pole ears 11 of the same polarity of all pole groups 1 is , the effective area coefficient of weld mark 3 is , the current coefficient of weld 3 is ,satisfy ; The capacity of the battery is The maximum charge and discharge rate of the battery is , the overcurrent safety factor of the battery is ,satisfy , .
[0032] The total area of all the welding marks 3 corresponding to the pole ears 11 of the same polarity of all the pole groups 1 is The effective area coefficient of weld print 3 is , the current coefficient of weld 3 is , the battery capacity is And the maximum charge and discharge rate of the battery is The relationship between the tab 11 and the connecting piece 2 is limited so that the weld mark 3 between the tab 11 and the connecting piece 2 has a suitable area, which can not only ensure the overcurrent capacity of the connecting piece 2 during the use of the battery, but also enable the connecting piece 2 to have a suitable structural size, reduce the weight of the connecting piece 2, reduce the occupation of the internal space of the battery by the connecting piece 2, and improve the capacity density of the battery.
[0033] It should be noted that ,therefore, , can be obtained For a battery, the capacity of the battery And the maximum charge and discharge rate of the battery It can be determined that the effective area coefficient of weld mark 3 is It is related to the welding process, so the current coefficient of welding mark 3 can be obtained according to the actual welding process. It is related to the material of the connecting piece 2. For example, the flow coefficient of the connecting piece 2 made of aluminum is , the current coefficient of the copper connecting piece 2 In summary, the total area of all weld marks 3 corresponding to the pole lugs 11 of the same polarity of all pole groups 1 of the battery can be calculated. Further, according to The value of can be used to design the area of the pole tab welding portion 21, thereby ensuring that the pole tab welding portion 21 has a suitable area, which can not only ensure the overcurrent capacity of the connecting piece 2 during the use of the battery, but also enable the connecting piece 2 to have a suitable structural size.
[0034] It is worth noting that the electrode group 1 includes a positive electrode tab 11 and a negative electrode tab 11. indivual, It means The total area of the weld marks 3 corresponding to the positive electrode tabs 11, or The total area of the weld marks 3 corresponding to the negative electrode tabs 11. That is, the area of the weld marks 3 corresponding to each tab 11 (which can be a positive electrode tab 11 or a negative electrode tab 11) is , the number of pole group 1 is ,satisfy Therefore, both the positive and negative electrodes of the battery meet the overcurrent requirements.
[0035] For further explanation, please refer to Figures 1 to 4 , a tab 11 and the corresponding tab welding portion 21 form a welding mark 3, and the area of a welding mark 3 is ; see Figure 5 , one tab 11 and the corresponding tab welding portion 21 form two weld marks 3, and the sum of the areas of the two weld marks 3 is It can be understood that there is one or more weld marks 3 between a pole tab 11 and the corresponding pole tab welding portion 21, and the specific number of weld marks 3 can be specifically set according to actual conditions.
[0036] Of course, in other alternative embodiments, the electrode group 1 may also include a plurality of positive electrode tabs 11 and a plurality of negative electrode tabs 11, for example 11 positive electrode tabs and A negative electrode tab 11, ≥2. If pole group 1 is equipped with indivual, It means The total area of the weld marks 3 corresponding to the positive electrode tabs 11, or The total area of the weld mark 3 corresponding to each negative electrode tab 11. Therefore, the area of the weld mark 3 corresponding to each tab 11 (which can be a positive electrode tab 11 or a negative electrode tab 11) is , the number of pole group 1 is ,satisfy .
[0037] Based on the above, in this embodiment, the number of pole groups 1 is , the number of pole ears 11 of the same polarity in each pole group 1 , and, understandably, and All are integers.
[0038] It should be noted that for different battery types, when the battery is a blade battery, it has a single-pole battery pack ( ) and bipolar battery ( ); When the battery is a square shell battery, it has a bipolar battery pack ( ) and quadrupole battery ( ), for square-shell batteries with wound electrode groups, it is usually a bipolar group.
[0039] In one embodiment, the maximum current through the weld mark 3 is The unit is A, the total area of all weld marks 3 corresponding to the pole ears 11 of the same polarity of all pole groups 1 The unit is mm², the current coefficient of welding mark 3 The unit is A / mm², the capacity of the battery The unit is Ah, The unit is 1 / h.
[0040] It should be noted that the battery charge and discharge rate refers to the current value required for the battery to discharge its rated capacity within a specified time, that is, charge and discharge rate = charge and discharge current / rated capacity. For example, when a battery with a rated capacity of 100Ah is discharged at 20A, its discharge rate is 0.2C.
[0041] In one embodiment, the overcurrent safety factor of the battery satisfy While preventing the battery from overheating during charge and discharge at a large rate, the connecting piece 2 is ensured to have a suitable size.
[0042] It is worth noting that a certain safety margin should be set between the maximum overcurrent capacity of the welding mark 3 and the maximum current required by the battery. If the value of is too small, the overcurrent capacity of the connecting piece 2 is low, resulting in excessively high temperature of the battery during the maximum rate charge and discharge process, and long-term cycle use affects the battery performance and life; if If the value is too large, the overall volume of the connecting piece 2 will be too large, occupying too much internal space of the battery, which is not conducive to the internal space layout of the battery, the improvement of the battery energy density and the lightweight design of the battery.
[0043] Specifically, when the battery is a blade battery, the battery overcurrent safety factor satisfy When the battery is a square shell battery, the overcurrent safety factor of the battery satisfy .
[0044] Of course, for other battery types, the battery's overcurrent safety factor Can be designed specifically.
[0045] In one embodiment, the maximum charge and discharge rate of the battery satisfy .
[0046] In one embodiment, the effective area coefficient of the weld mark 3 is satisfy While ensuring that the weld mark 3 has a sufficient effective area to ensure the flow of current through the connecting piece 2, the implementation of the welding process is facilitated.
[0047] It should be noted that the effective area coefficient of weld mark 3 It refers to the ratio of the actual welding area to the weld area of the outer surface of the weld. In this embodiment, the tab 11 and the tab welding portion 21 of the connecting sheet 2 are connected by ultrasonic welding. Figure 6 , Figure 6 The shaded area in the middle shows the weld area on the outer surface of the weld. Figure 2 It can be seen that for the weld mark 3 with a rectangular structure, the weld mark area on the outer surface of the weld is . As for the actual welding area ( Figure 7 In actual production, the following method is usually used to measure the area: the tab 11 and the tab welding part 21 are cut off from the electrode group 1 and the connecting sheet 2, the tab 11 is peeled off from the tab welding part 21, and the area of the tab 11 remaining on the tab welding part 21 is taken as the actual welding area. For further information, please refer to Figure 6 and Figure 7 , by removing the pit (e.g. Figure 6 and Figure 7The actual welding area can be calculated by counting the number of small squares shown in the figure or the number of pits without the pole ear 11.
[0048] It is worth noting that if the effective area coefficient of weld mark 3 If the effective area coefficient of the weld mark 3 is too small, the effective area coefficient of the weld mark 3 will be insufficient, which will affect the current capacity of the connecting piece 2 and make the local temperature of the connecting piece 2 too high. The long-term cycle use will affect the battery performance and life. However, according to the current actual manufacturing capacity, it is impossible to achieve a too high effective area coefficient of the weld mark 3. .
[0049] In one embodiment, the area of the tab welding portion 21 is ,satisfy While ensuring that the electrode tab welding portion 21 has a sufficient area to accommodate the weld mark 3, the overall volume of the connecting piece 2 is prevented from being too large, thereby improving the space utilization of the battery.
[0050] It is worth noting that, according to the area of the welding mark 3 corresponding to each tab 11 , so that the area of the tab welding portion 21 is Appropriately greater than If If the value of is too small, a cold weld problem may occur when welding the tab 11 to the tab welding portion 21; If the value of is too large, the overall volume of the connecting piece 2 will be too large, and the internal space of the battery will be too large, which is not conducive to the internal space layout of the battery, the improvement of the battery energy density and the lightweight design of the battery.
[0051] It should be noted that The unit is mm², The unit is mm².
[0052] In one embodiment, Figure 2 As shown, the weld mark 3 is a rectangular structure, and the length of the weld mark 3 is , the width of weld mark 3 is ,satisfy , , Therefore, for the rectangular structure of the weld mark 3, it is necessary to use .
[0053] It should be noted that if and If the value of is too small, The value of is too small, which affects the overcurrent capability of weld mark 3; if and If the value of is too large, when the size of the electrode tab welding portion 21 is constant, the edge of the weld mark 3 is too close to the edge of the electrode tab welding portion 21, and the problem of poor welding of the electrode tab 11 may occur easily.
[0054] Of course, in other alternative embodiments, the weld mark 3 may also be in other shapes, either regular or irregular.
[0055] In one embodiment, Figure 2 As shown, the minimum distance from the edge of the weld mark 3 to the edge corresponding to the tab welding portion 21 is ,satisfy Thus, the edge of the weld mark 3 is prevented from being too close to the edge of the tab welding portion 21, thereby preventing the tab 11 from being poorly welded.
[0056] It is worth mentioning that please refer to Figure 2 The tab welding part 21 is also approximately rectangular in structure, the long side of the welding mark 3 is arranged correspondingly to the long side of the tab welding part 21, and the short side of the welding mark 3 is arranged correspondingly to the short side of the tab welding part 21. For further information, please continue to refer to Figure 2 The distance between one of the long sides of the weld mark 3 and one of the long sides of the corresponding tab welding portion 21 is The distance between the other long side of the weld mark 3 and the other long side of the corresponding electrode tab welding portion 21 is The distance between one of the short sides of the weld mark 3 and one of the short sides of the corresponding tab welding portion 21 is The distance between the other short side of the weld mark 3 and the other short side of the corresponding electrode tab welding portion 21 is ,satisfy , , , . Further, , , , The four values may all be the same, or may all be different, or any two or three of them may be the same.
[0057] The actual overcurrent condition of the aluminum connecting piece 2 is tested and evaluated below. Specifically, a temperature sensing line is arranged at the weld mark 3 between the connecting piece 2 and the tab 11 inside the battery, the battery is charged at the maximum rate, and the temperature at the weld mark 3 is monitored. The maximum temperature is lower than 60°C to meet the requirements. The monitoring results of the embodiment battery are shown in Table 1, and the monitoring results of the comparative battery are shown in Table 2. The embodiment battery is a battery whose parameters all meet the requirements of this embodiment, and correspondingly, the comparative battery is a battery whose one or more parameters do not meet the requirements of this embodiment.
[0058] Table 1 Battery monitoring results of the aluminum connecting piece 2 embodiment
[0059]
[0060] Table 2 Monitoring results of the battery with aluminum connecting piece 2 as a comparative example
[0061]
[0062] It can be seen from Table 1 that in Examples 1 to 8, the overcurrent safety factor are not less than 1, therefore, the overcurrent capacity of the weld mark 3 between the connecting piece 2 and the tab 11 meets the use requirements of the battery, and the temperature at the weld mark 3 does not exceed the maximum temperature requirement. The value of satisfies , The value of satisfies , the welding of the tab 11 and the connecting piece 2 does not cause cold welding, ensuring the welding quality; The value of satisfies , which can not only ensure sufficient effective area of the weld mark 3, but also realize welding with existing welding capacity, and avoid damage to the tab 11 and the connecting piece 2 during the welding process.
[0063] It can be seen from Table 2 that in Comparative Example 1, , The value of is not in Within the range and less than 10mm, , The value of is not in Within the range and less than 2mm, it can be calculated that ,therefore In this battery, the overcurrent capacity of the weld mark 3 between the tab 11 and the connecting piece 2 is too low, and the temperature at the weld mark 3 is higher than 60° C., which does not meet the requirements.
[0064] It can be seen from Table 2 that in Comparative Example 2, , The value of is not in Within the range and less than 10mm, , The value of is not in Within the range and less than 2mm, it can be calculated that ,therefore In this battery, the overcurrent capacity of the weld mark 3 between the tab 11 and the connecting piece 2 is too low, and the temperature at the weld mark 3 is higher than 60° C., which does not meet the requirements.
[0065] It can be seen from Table 2 that in Comparative Example 3, , The value of is not in Within the range and greater than 95%, it can be calculated that .Although The value of is greater than 1, so that the overcurrent capacity of the weld mark 3 meets the requirements. However, in the actual welding process, the ultrasonic welding pressure is too large, which makes the tab 11 and the connecting piece 2 easily deformed and damaged.
[0066] It can be seen from Table 2 that in Comparative Example 4, , The value of is not in Within the range and greater than 95%, it can be calculated that .Although The value of is greater than 1, so that the overcurrent capacity of the weld mark 3 meets the requirements. However, in the actual welding process, the ultrasonic welding pressure is too large, which makes the tab 11 and the connecting piece 2 easily deformed and damaged.
[0067] It can be seen from Table 2 that in Comparative Example 5, , The value of is not in Within the range and less than 65%, it can be calculated that ,therefore In this battery, the overcurrent capacity of the weld mark 3 between the tab 11 and the connecting piece 2 is too low, and the temperature at the weld mark 3 is higher than 60° C., which does not meet the requirements.
[0068] It can be seen from Table 2 that in Comparative Example 6, , The value of is not in Within the range and less than 65%, it can be calculated that ,therefore In this battery, the overcurrent capacity of the weld mark 3 between the tab 11 and the connecting piece 2 is too low, and the temperature at the weld mark 3 is higher than 60° C., which does not meet the requirements.
[0069] It can be seen from Table 2 that in Comparative Example 7, , The value of is not in Within the range and greater than 80mm, , The value of is not in If the range is greater than 15 mm, we can calculate that: .Although The value of is greater than 1, so that the overcurrent capacity of weld mark 3 meets the requirements, but a cold weld problem occurs after welding is completed, affecting the welding quality.
[0070] It can be seen from Table 2 that in Comparative Example 8, , The value of is not in Within the range and greater than 80mm, , The value of is not in If the range is greater than 15 mm, we can calculate that: .Although The value of is greater than 1, so that the overcurrent capacity of weld mark 3 meets the requirements, but a cold weld problem occurs after welding is completed, affecting the welding quality.
[0071] The actual overcurrent condition of the copper connecting piece 2 is tested and evaluated below. Specifically, a temperature sensing line is arranged at the weld mark 3 between the connecting piece 2 and the tab 11 inside the battery, the battery is charged at the maximum rate, and the temperature at the weld mark 3 is monitored. The maximum temperature is lower than 60°C to meet the requirements. The monitoring results of the embodiment battery are shown in Table 3, and the monitoring results of the comparative battery are shown in Table 4. The embodiment battery is a battery whose parameters all meet the requirements of this embodiment, and correspondingly, the comparative battery is a battery whose one or more parameters do not meet the requirements of this embodiment.
[0072] Table 3 Battery monitoring results of copper material connecting piece 2 embodiment
[0073]
[0074] Table 4 Monitoring results of the comparative battery of copper connecting piece 2
[0075]
[0076] It can be seen from Table 3 that in Examples 9 to 16, the overcurrent safety factor are not less than 1, therefore, the overcurrent capacity of the weld mark 3 between the connecting piece 2 and the tab 11 meets the use requirements of the battery, and the temperature at the weld mark 3 does not exceed the maximum temperature requirement. The value of satisfies , The value of satisfies , the welding of the tab 11 and the connecting piece 2 does not cause cold welding, ensuring the welding quality; The value of satisfies , which can not only ensure sufficient effective area of the weld mark 3, but also realize welding with existing welding capacity, and avoid damage to the tab 11 and the connecting piece 2 during the welding process.
[0077] It can be seen from Table 4 that in Comparative Example 9, , The value of is not in Within the range and less than 10mm, , The value of is not in Within the range and less than 2mm, it can be calculated that ,therefore In this battery, the overcurrent capacity of the weld mark 3 between the tab 11 and the connecting piece 2 is too low, and the temperature at the weld mark 3 is higher than 60° C., which does not meet the requirements.
[0078] It can be seen from Table 4 that in Comparative Example 10, , The value of is not in Within the range and less than 10mm, , The value of is not in Within the range and less than 2mm, it can be calculated that ,therefore In this battery, the overcurrent capacity of the weld mark 3 between the tab 11 and the connecting piece 2 is too low, and the temperature at the weld mark 3 is higher than 60° C., which does not meet the requirements.
[0079] It can be seen from Table 4 that in Comparative Example 11, , The value of is not in Within the range and less than 65%, it can be calculated that ,therefore In this battery, the overcurrent capacity of the weld mark 3 between the tab 11 and the connecting piece 2 is too low, and the temperature at the weld mark 3 is higher than 60° C., which does not meet the requirements.
[0080] It can be seen from Table 4 that in Comparative Example 12, , The value of is not in Within the range and less than 65%, it can be calculated that ,therefore In this battery, the overcurrent capacity of the weld mark 3 between the tab 11 and the connecting piece 2 is too low, and the temperature at the weld mark 3 is higher than 60° C., which does not meet the requirements.
[0081] It can be seen from Table 4 that in Comparative Example 13, , The value of is not in Within the range and greater than 95%, it can be calculated that .Although The value of is greater than 1, so that the overcurrent capacity of the weld mark 3 meets the requirements. However, in the actual welding process, the ultrasonic welding pressure is too large, which makes the tab 11 and the connecting piece 2 easily deformed and damaged.
[0082] It can be seen from Table 4 that in Comparative Example 14, , The value of is not in Within the range and greater than 95%, it can be calculated that .Although The value of is greater than 1, so that the overcurrent capacity of the weld mark 3 meets the requirements. However, in the actual welding process, the ultrasonic welding pressure is too large, which makes the tab 11 and the connecting piece 2 easily deformed and damaged.
[0083] It can be seen from Table 4 that in Comparative Example 15, , The value of is not in Within the range and greater than 80mm, , The value of is not in If the range is greater than 15 mm, we can calculate that: .Although The value of is greater than 1, so that the overcurrent capacity of weld mark 3 meets the requirements, but a cold weld problem occurs after welding is completed, affecting the welding quality.
[0084] It can be seen from Table 4 that in Comparative Example 16, , The value of is not in Within the range and greater than 80mm, , The value of is not in If the range is greater than 15 mm, we can calculate that: .Although The value of is greater than 1, so that the overcurrent capacity of weld mark 3 meets the requirements, but a cold weld problem occurs after welding is completed, affecting the welding quality.
[0085] In summary, the overcurrent safety factor , that is, the total area of all weld marks 3 corresponding to the pole ears 11 of the same polarity of all pole groups 1 , the overcurrent capacity of the weld mark 3 can be guaranteed during the use of the battery. Further, the effective area coefficient of the weld mark 3 satisfy , while ensuring that the weld mark 3 has a sufficient effective area to ensure the flow of the connecting piece 2, it is also possible to avoid excessive ultrasonic welding pressure during the actual welding process, which may cause deformation and damage to the tab 11 and the connecting piece 2; for the common rectangular weld mark 3, the length of the weld mark 3 is satisfy , so that the width of the weld mark 3 satisfy , while making the weld mark 3 have a sufficient area to ensure the overcurrent capacity of the weld mark 3 during the use of the battery, it is also necessary to avoid the problem of the edge of the weld mark 3 being too close to the edge of the tab welding part 21, thereby causing the tab 11 to be poorly welded.
[0086] According to another aspect of an embodiment of the present invention, a battery pack is provided, comprising the above-mentioned battery.
[0087] Although the embodiments of the present invention have been described in conjunction with the accompanying drawings, those skilled in the art may make various modifications and variations without departing from the spirit and scope of the present invention, and such modifications and variations are all within the scope defined by the appended claims.
Claims
1. A battery, characterized in that: include: A pole group, provided with at least one, the pole group including a pole lug; The connecting piece includes a pole lug welding portion, wherein the pole lugs are welded to the pole lug welding portion to form a weld mark; Among them, the maximum current passing through the welding mark is The total area of all the welding marks corresponding to the pole ears of the same polarity of all the pole groups is , the effective area coefficient of the weld print is , the flow coefficient of the weld print is ,satisfy , The unit is A, The unit is mm², The unit is A / mm²; The capacity of the battery is The maximum charge and discharge rate of the battery is , the overcurrent safety factor of the battery is ,satisfy , , The unit is Ah, The unit is 1 / h; The effective area coefficient of the weld mark satisfy ; The area of the weld mark corresponding to each of the tabs is , the number of pole ears of the same polarity in each pole group is , the number of pole groups is ,satisfy , The unit is mm², , ; The weld mark is a rectangular structure, and the length of the weld mark is , the width of the weld mark is ,satisfy , , .
2. The battery according to claim 1, characterized in that Overcurrent safety factor of the battery satisfy .
3. The battery according to claim 2, characterized in that The battery is a blade battery, and the overcurrent safety factor of the battery is satisfy ; Or, The battery is a square shell battery, and the overcurrent safety factor of the battery is satisfy .
4. The battery according to any one of claims 1 to 3, characterized in that The maximum charge and discharge rate of the battery satisfy .
5. The battery according to any one of claims 1 to 3, characterized in that The area of the electrode tab welding portion is ,satisfy , The unit is mm².
6. The battery according to any one of claims 1 to 3, characterized in that The minimum distance from the edge of the weld mark to the edge corresponding to the welding portion of the tab is ,satisfy .
7. A battery pack, characterized in that: A battery comprising the battery according to any one of claims 1 to 6.