Sodium ion battery precursor, positive electrode material and preparation method thereof, and sodium ion battery
Magnesium-doped precursor is prepared by co-precipitation reaction of titanium dioxide by-product ferrous sulfate with metal salt, and sintered with sodium source to prepare a positive electrode material, which solves the problems of cost and rate performance of sodium ion batteries and achieves electrochemical performance. Improvement and cost reduction.
Patent Information
- Application Number
- CN202411204149.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-08-30
AI Technical Summary
The cost advantages of layered transition metal oxide cathode materials of sodium ion batteries have not been further expanded, and the large ion radius of sodium ions affects the rate performance, limiting the practical application of sodium ion batteries.
The magnesium-doped precursor is prepared by using titanium dioxide by-product ferrous sulfate as raw material, and co-precipitation reaction with metal salt after precipitation and removal, and sintering is carried out in combination with sodium source to prepare the positive electrode material, optimizing the element ratio to improve electrochemical performance.
It reduces the cost of sodium ion batteries, improves its high-rate performance and electrochemical performance, and realizes the high-value recycling and utilization of titanium dioxide by-products.
Smart Images

Figure CN118702165B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of secondary batteries, and in particular to a sodium ion battery precursor, a positive electrode material and a preparation method thereof, and a sodium ion battery. Background Art
[0002] At present, lithium-ion batteries have been widely used. With their diversified applications, higher requirements are placed on battery performance. Lithium-ion batteries are greatly affected by fluctuations in raw material prices, which restricts their development in the market segments. As an important technical direction in the exploration of battery system diversification, sodium-ion batteries have similar electrochemical properties and lower costs to lithium-ion batteries, and are considered to be a promising alternative to lithium-ion batteries.
[0003] Among the positive electrode materials of sodium ion batteries, layered transition metal oxide positive electrodes have the advantages of large theoretical capacity, non-toxicity, and easy synthesis, and have received widespread attention. However, the cost advantage of layered transition metal oxide materials is mainly reflected in the low-priced sodium salts. The metal salts used in their precursors are basically the same as the raw materials used in the precursors of the positive electrode materials of ternary lithium batteries, resulting in the cost advantage of sodium ion batteries cannot be further expanded. At the same time, the ionic radius of sodium ions is much larger than that of lithium ions, which affects the rate performance of sodium ion batteries. These factors limit the practical application of sodium ion batteries, so it is necessary to further reduce the cost of layered transition metal oxide positive electrode materials for sodium ion batteries and optimize their performance.
[0004] In view of this, the present invention is proposed. Summary of the invention
[0005] The object of the present invention is to provide a sodium ion battery precursor, a positive electrode material and a preparation method thereof, and a sodium ion battery, aiming to reduce the cost of the sodium ion battery while improving its electrochemical performance.
[0006] The present invention is achieved in that:
[0007] In a first aspect, the present invention provides a method for preparing a sodium ion battery precursor, comprising:
[0008] The ferrous sulfate byproduct of titanium dioxide is dissolved and then precipitated to remove impurities to obtain a ferrous sulfate solution;
[0009] Using ferrous sulfate solution and metal salt as raw materials, a precursor is prepared by coprecipitation reaction of mixed salt solution;
[0010] In the mixed salt solution, the molar ratio of nickel, manganese, copper, ferrous iron and magnesium is a:b:c:d:e, a+b+c+d+e=1, 0.25 <b<0.35,0.02<c<0.06,0.20<d<0.40,19<d / e<23,a=1-b-c-d-e。
[0011] In an optional embodiment, the process of preparing a ferrous sulfate solution from ferrous sulfate, a byproduct of titanium dioxide, comprises: mixing and dissolving the ferrous sulfate, a byproduct of titanium dioxide, with water, and then mixing with liquid alkali to adjust the pH value to 5-6, reacting for 10-30 minutes, separating the solid and the liquid, and mixing the obtained liquid material with a sulfuric acid solution to adjust the pH value to 1-2 to obtain a ferrous sulfate solution containing magnesium ions;
[0012] Among them, in the titanium dioxide by-product ferrous sulfate, the mass fraction of ferrous ions is 15%-20%, the mass fraction of trivalent iron ions is 2%-7%, the mass fraction of magnesium ions is 0.5%-1.5%, and the remainder is impurity elements;
[0013] The impurity elements include at least one of titanium, manganese and aluminum, and the mass fraction of each impurity element is less than 0.3%.
[0014] In an optional embodiment, the liquid alkali is selected from at least one of a sodium hydroxide solution and a potassium hydroxide solution;
[0015] Solid-liquid separation is carried out by using precision filters with a filtration accuracy of 0.2μm-0.7μm;
[0016] The mass fraction of sulfuric acid solution is 40%-50%.
[0017] In an optional embodiment, a ferrous sulfate solution is mixed with a nickel salt, a manganese salt, and a copper salt to obtain a mixed salt solution, and a coprecipitation reaction is carried out using the mixed salt solution in the presence of a precipitant and a complexing agent;
[0018] The total concentration of metal ions in the mixed salt solution is 1.3 mol / L-2.4 mol / L;
[0019] The nickel salt, the manganese salt and the copper salt are each independently selected from at least one of sulfate, phosphate and chloride.
[0020] In an optional embodiment, the mixed salt solution, the precipitant solution and the complexing agent solution are simultaneously flowed into the base liquid, and a coprecipitation reaction is carried out under a protective gas atmosphere;
[0021] The precipitant solution is selected from at least one of a sodium hydroxide solution and a potassium hydroxide solution, and the concentration of the precipitant solution is 9 mol / L-12 mol / L;
[0022] The complexing agent solution is selected from at least one of ammonia water and sodium citrate solution, and the concentration of the complexing agent solution is 1 mol / L-10 mol / L;
[0023] The base liquid is a mixed solution of water, precipitant and complexing agent, the concentration of precipitant in the base liquid is 15%-30%, and the concentration of complexing agent is 10%-20%;
[0024] The reaction temperature of the coprecipitation reaction is 45°C-65°C, the pH of the reaction slurry is 9-12, the concentration of the complexing agent in the reaction slurry is 3g / L-6g / L, and the median particle size D50 of the obtained precursor is 3μm-4μm;
[0025] The stirring speed during the coprecipitation reaction was controlled to be 500 rpm-800 rpm.
[0026] In a second aspect, the present invention provides a sodium ion battery precursor prepared by the preparation method of any one of the aforementioned embodiments;
[0027] Its chemical formula is Ni (1-b-c-d-e) Mn b Cu c Fe d Mg e (OH)2, 0.25 <b<0.35,0.02<c<0.06,0.20<d<0.40,19<d / e<23。
[0028] In a third aspect, the present invention provides a method for preparing a positive electrode material for a sodium ion battery, using a sodium source and a sodium ion battery precursor in the aforementioned embodiment as raw materials for preparation;
[0029] In an optional embodiment, the preparation method includes: mixing and sintering a sodium source and a sodium ion battery precursor, controlling the sintering temperature to be 700° C.-900° C., and the sintering time to be 10 h-15 h;
[0030] The molar ratio of the sodium element in the sodium source to the total amount of metal elements in the sodium ion battery precursor is (1.1-1.3):1;
[0031] The sodium source is selected from at least one of sodium carbonate and sodium acetate.
[0032] In a fourth aspect, the present invention provides a sodium ion battery positive electrode material prepared by the preparation method of the aforementioned embodiment.
[0033] In a fifth aspect, the present invention provides a sodium ion battery, comprising the sodium ion battery positive electrode material of the aforementioned embodiment.
[0034] The present invention has the following beneficial effects: the present invention uses ferrous sulfate, a byproduct of titanium dioxide, as a raw material, obtains a ferrous sulfate solution after precipitation and impurity removal, and then uses the ferrous sulfate solution and a metal salt as raw materials for a coprecipitation reaction to prepare a magnesium-doped precursor, a small amount of magnesium ions play a supporting role in the sodium ion layer of the positive electrode material, improves the high rate performance of the sodium ion battery, and can improve the electrochemical performance of the product by regulating the proportion of each element. The process provided by the present invention is simple and easy to implement, with low production cost, and can improve the electrochemical performance of the layered transition metal oxide positive electrode material while realizing the high-value recycling of titanium dioxide byproducts. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.
[0036] Figure 1 This is a scanning electron microscope image of the magnesium-doped multi-element precursor prepared in Example 1;
[0037] Figure 2 This is a partial magnified scanning electron microscope image of the magnesium-doped multi-element precursor prepared in Example 1;
[0038] Figure 3 This is a scanning electron microscope image of the magnesium-doped multi-element precursor prepared in Example 2;
[0039] Figure 4 This is a partial magnified scanning electron microscope image of the magnesium-doped multi-element precursor prepared in Example 2;
[0040] Figure 5 Scanning electron microscope image of the multi-element precursor prepared in Comparative Example 2;
[0041] Figure 6 A partial enlarged view of the scanning electron microscope image of the multi-element precursor prepared in Comparative Example 2. DETAILED DESCRIPTION
[0042] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.
[0043] Ferrous sulfate heptahydrate is the main solid waste in the production of titanium dioxide by sulfuric acid method. Using it as one of the raw materials for layered transition metal oxide positive electrode materials can significantly reduce the cost of sodium ion batteries. However, the ferrous sulfate contains a large amount of impurity ions such as Ti, Mg, and Al, which to a certain extent increases the difficulty of using ferrous sulfate, a byproduct of titanium dioxide, to prepare multi-element precursors and positive electrode materials for sodium ion batteries.
[0044] To this end, the inventors creatively provided a method for preparing multi-element precursors and positive electrode materials for sodium ion batteries using ferrous sulfate, a by-product of titanium dioxide, as a raw material. Impurities were removed through a specific impurity removal process to obtain a ferrous sulfate solution, and then a magnesium-doped precursor was prepared by a co-precipitation reaction using the ferrous sulfate solution and a metal salt as raw materials.
[0045] An embodiment of the present invention provides a method for preparing a sodium ion battery precursor, comprising the following steps:
[0046] S1. Precipitation and impurity removal
[0047] The ferrous sulfate byproduct of titanium dioxide is dissolved and then precipitated to remove impurities. After solid-liquid separation, a ferrous sulfate solution is obtained. The solution obtained by precipitation and impurity removal includes a large amount of Fe 2+ and a small amount of Mg 2+ , other impurities such as Fe 3+ 、Ti 4+ 、Al 3+ Basically all of them are removed.
[0048] In some embodiments, in the titanium dioxide byproduct ferrous sulfate, the mass fraction of ferrous ions is 15%-20%, the mass fraction of ferric ions is 2%-7%, the mass fraction of magnesium ions is 0.5%-1.5%, and the remainder is impurity elements; the impurity elements include at least one of titanium, manganese and aluminum, and the mass fraction of each impurity element is less than 0.3%. The anions of the titanium dioxide byproduct are mainly sulfate ions, and the impurity anions are basically free of impurities.
[0049] In some embodiments, the process of precipitation and impurity removal includes: mixing and dissolving the titanium dioxide byproduct ferrous sulfate and water, then mixing with liquid caustic soda to adjust the pH value to 5-6, reacting for 10min-30min, separating the solid and liquid, mixing the obtained liquid material with sulfuric acid solution to adjust the pH value to 1-2, and obtaining a ferrous sulfate solution containing magnesium ions. The inventor optimizes parameters such as the pH value and reaction time of impurity removal to improve the removal effect of impurity elements. If the pH value is too small, the impurities are not completely removed, affecting the electrochemical properties of the product; if the pH value is too large, magnesium and ferrous ions will cause losses, affecting the utilization rate of the raw materials, and a large amount of solids will be deposited to clog the filtration equipment. At this pH value, only impurities such as trivalent iron ions, titanium ions, and manganese ions will be precipitated, and the effect on ferrous ions and magnesium ions will be small.
[0050] Specifically, the pH value of the system can be adjusted to 5.0, 5.3, 5.5, 5.8, 6.0, etc. with liquid alkali, the reaction time can be 10 min, 15 min, 20 min, 25 min, 30 min, etc., and stirring is carried out during the reaction. The method of solid-liquid separation is not limited, and solid-liquid separation can be carried out by filtration. After filtration, the pH value of the liquid material can be adjusted to 1.0, 1.3, 1.5, 1.8, 2.0, etc. with sulfuric acid solution.
[0051] In other embodiments, the by-product ferrous sulfate of titanium dioxide can be completely purified, that is, sulfide purification is added to the purification scheme of the present invention to prepare a ferrous sulfate solution with higher purity. If magnesium needs to be doped, a magnesium salt with higher purity needs to be additionally added, and finally the same magnesium-doped multi-component precursor and cathode material can be prepared, but the whole process will be more complex and the manufacturing cost will be higher.
[0052] Furthermore, the liquid alkali is selected from at least one of sodium hydroxide solution and potassium hydroxide solution. The liquid alkali can be any one or both of the above, and the pH value of the system is made to meet the requirements by adjusting the dosage of the liquid alkali. The mass fraction of the sulfuric acid solution used to adjust the pH value of the liquid material is 40%-50%, such as 40%, 45%, 50%, etc. The liquid alkali and the sulfuric acid solution can both be aqueous solutions.
[0053] In some embodiments, solid-liquid separation is carried out by filtration using a precision filter to fully remove solid materials, and the filtration accuracy is 0.2 μm - 0.7 μm, such as 0.2 μm, 0.3 μm, 0.4 μm, 0.5 μm, 0.6 μm, 0.7 μm, etc.
[0054] S2. Prepare a mixed salt solution
[0055] Mix the ferrous sulfate solution with nickel salt, manganese salt, and copper salt to obtain a mixed salt solution, and use this mixed salt solution to prepare a precursor so that the metal elements in the precursor are nickel, manganese, copper, iron, and magnesium.
[0056] Before mixing the ferrous sulfate solution with other metal salts, the concentrations of ferrous ions and magnesium ions in the ferrous sulfate solution in S1 can be measured so that the ratio of each element in the precursor meets the preset requirements. The molar ratio of ferrous ions to magnesium ions in the ferrous sulfate solution is x∶y, and 19 < x / y < 23. Within this range, the electrochemical performance of the cathode material can be further improved. Specifically, the value of x / y can be 19.5, 20.0, 20.5, 21.0, 21.5, 22.0, 22.5, etc.
[0057] In some embodiments, the molar ratio of nickel, manganese, copper, ferrous, and magnesium in the mixed salt solution is a:b:c:d:e, where a + b + c + d + e = 1, 0.25 < b < 0.35, 0.02 < c < 0.06, 0.20 < d < 0.40, 19 < d / e < 23, and a = 1 - b - c - d - e. The inventors adjusted the ratios of the various elements to further improve the electrochemical performance of the cathode material. Specifically, magnesium ions can promote the circulation of sodium ions in the lattice of the cathode material and improve the rate performance; the addition of copper ions helps enhance the structural stability of the material.
[0058] Specifically, the value of b can be 0.26, 0.28, 0.30, 0.32, 0.34, etc., the value of c can be 0.03, 0.04, 0.05, etc., the value of d can be 0.25, 0.30, 0.35, 0.38, etc., and the value of d / e is equal to the value of the above x / y.
[0059] In some embodiments, the total concentration of metal ions in the mixed salt solution is 1.3 mol / L - 2.4 mol / L, such as 1.3 mol / L, 1.5 mol / L, 1.8 mol / L, 2.0 mol / L, 2.2 mol / L, 2.4 mol / L, etc. The total concentration of metal ions within the above range can make the deposited precursor more uniform. The solvent for preparing the mixed salt solution can be water.
[0060] In some embodiments, the nickel salt, manganese salt, and copper salt are each independently selected from at least one of sulfates, phosphates, and chlorides. The types of the nickel salt, manganese salt, and copper salt can be the same or different, and they can each independently be selected from any one or several of the above salts.
[0061] S3. Coprecipitation reaction
[0062] Perform a coprecipitation reaction on the mixed salt solution in the presence of a precipitating agent and a complexing agent to form a precursor hydroxide.
[0063] In some embodiments, the mixed salt solution, the precipitating agent solution, and the complexing agent solution are flowed into the bottom solution in parallel, and the coprecipitation reaction is carried out under an inert gas atmosphere. The bottom solution is a mixed solution of water, a precipitating agent, and a complexing agent. During the coprecipitation process, control the flow rate of the precipitating agent solution to make the pH value of the system meet the requirements, and control the flow rate of the complexing agent solution to control uniform deposition.
[0064] In some embodiments, the precipitant solution is selected from at least one of sodium hydroxide and potassium hydroxide solution, and the precipitant solution can be any one or more of the above. The concentration of the precipitant solution is 9mol / L-12mol / L, such as 9mol / L, 10mol / L, 11mol / L, 12mol / L, etc. The complexing agent solution is selected from at least one of ammonia water and sodium citrate solution, and the complexing agent solution can be any one or more of the above, and the concentration of the complexing agent solution is 1mol / L-10mol / L, such as 1mol / L, 3mol / L, 5mol / L, 7mol / L, 8mol / L, 9mol / L, 10mol / L, etc. The complexing effect of sodium citrate is stronger and a low concentration of complexing agent solution can be used.
[0065] In some embodiments, the base liquid is a mixed solution of water, a precipitant and a complexing agent, the concentration of the precipitant in the base liquid is 15%-30%, the concentration of the complexing agent is 10%-20%, and the reaction conditions of co-deposition are met by regulating the concentrations of the precipitant and the complexing agent in the base liquid. Specifically, the concentration of the precipitant in the base liquid can be 15%, 20%, 25%, 30%, etc., and the concentration of the complexing agent can be 10%, 13%, 15%, 18%, 20%, etc.
[0066] Furthermore, the reaction temperature of the coprecipitation reaction is 45°C-65°C, the pH of the reaction slurry is 9-12, the concentration of the complexing agent in the reaction slurry is 3g / L-6g / L, and the median particle size D50 of the precursor is 3μm-4μm. After the median particle size D50 of the precursor meets the requirements, the reaction is stopped and the precursor product is obtained by filtering. By adjusting the temperature, pH value and other parameters of the coprecipitation reaction, the deposition rate can be better controlled to obtain a uniform precursor product.
[0067] Specifically, the reaction temperature of the coprecipitation reaction can be 45°C, 50°C, 55°C, 60°C, 65°C, etc., the pH value of the reaction slurry can be 9, 10, 11, 12, etc., the concentration of the complexing agent in the reaction slurry can be 5.0 g / L, 5.5 g / L, 6.0 g / L, etc., and the median particle size D50 of the precursor obtained by the reaction can be 3.0 μm, 3.5 μm, 4.0 μm, etc.
[0068] Furthermore, the coprecipitation reaction process can be carried out under stirring conditions to achieve uniform deposition, and the stirring speed is controlled to be 500 rpm-800 rpm, such as 500 rpm, 600 rpm, 700 rpm, 800 rpm, etc.
[0069] The embodiment of the present invention also provides a sodium ion battery precursor, which is prepared by the preparation method provided by the previous embodiment of the present invention and has the advantages of low cost and excellent electrochemical performance.
[0070] In some embodiments, the chemical formula of the sodium-ion battery precursor is Ni (1-b-c-d-e) Mn b Cu c Fe d Mg e (OH)2, where 0.25 < b < 0.35, 0.02 < c < 0.06, 0.20 < d < 0.40, and 19 < d / e < 23. By regulating the proportions of the various elements, the electrochemical performance of the prepared cathode material is further improved. The cathode material of the transition metal layered oxide provided in the embodiments of the present invention exhibits good cycle stability, which is of great significance for promoting the practical application process of sodium-ion batteries based on this cathode system.
[0071] The embodiments of the present invention also provide a method for preparing a cathode material for a sodium-ion battery. Using a sodium source and the sodium-ion battery precursor prepared in the embodiments of the present invention as raw materials for preparation, the electrochemical performance of the prepared cathode material is significantly improved by optimizing the composition of the precursor.
[0072] In some embodiments, the sodium source and the sodium-ion battery precursor are mixed and sintered. The sintering temperature is controlled at 700°C - 900°C, and the sintering time is 10h - 15h. It is appropriate for the sintering temperature and time to be within the above ranges to enable the reaction to proceed fully and obtain a uniform cathode material. Specifically, the sintering temperature can be 700°C, 800°C, 900°C, etc., and the sintering time can be 10h, 11h, 12h, 13h, 14h, 15h, etc. After sintering is completed, a pulverization treatment can also be carried out to obtain a magnesium-doped transition metal oxide cathode material NaNi (1-b-c-d-e) Mn b Cu c Fe d Mg e O2. Pulverization can include coarse pulverization and fine pulverization to obtain a cathode material product with a particle size meeting the requirements.
[0073] In some embodiments, the sodium source is selected from at least one of sodium carbonate and sodium acetate, and the sodium source can be any one or several of the above. The molar ratio of the sodium element in the sodium source to the total amount of metal elements in the sodium-ion battery precursor is (1.1 - 1.3):1, such as 1.1:1, 1.2:1, 1.3:1, etc.
[0074] The embodiments of the present invention also provide a cathode material for a sodium-ion battery, which is prepared by the preparation method provided in the embodiments of the present invention and has the advantages of low cost and excellent electrochemical performance.
[0075] An embodiment of the present invention further provides a sodium ion battery, comprising the above-mentioned sodium ion battery positive electrode material, wherein the above-mentioned sodium ion battery positive electrode material is present on the positive electrode plate as a positive electrode active material, and the electrochemical performance of the sodium ion battery is improved by optimizing the preparation process of the positive electrode material, and the preparation cost of the sodium ion battery is also reduced.
[0076] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.
[0077] It should be noted that the ferrous sulfate used in the preparation methods provided in the following examples and comparative examples is a by-product of the production of titanium dioxide using the sulfuric acid process. This process produces 4 tons of by-product ferrous sulfate for every ton of titanium dioxide produced. The ferrous sulfate contains a large amount of impurity ions and insoluble matter and is easily oxidized during storage.
[0078] Specifically, the composition of ferrous sulfate, a by-product of titanium dioxide, is as follows: the ferrous ion content (mass fraction, the same below) is 16%, the trivalent iron ion content is 4%, the magnesium ion content is 0.5%, and the contents of other major impurity ions such as titanium, manganese and aluminum are all less than 0.3%.
[0079] Example 1
[0080] This embodiment provides a method for preparing a sodium ion battery precursor, comprising the following steps:
[0081] (1) Ferrous sulfate, a byproduct of titanium dioxide, is dissolved in pure water to prepare a solution with a concentration of 1.5 mol / L (measured in terms of ferrous ion concentration, the same below). A 30% by mass sodium hydroxide aqueous solution is added to the solution to adjust the pH to 5.2. The solution is filtered with a precision filter with an accuracy of 0.05 μm. 49% by mass dilute sulfuric acid is added to the filtrate to adjust the pH to 1.3 to obtain a ferrous sulfate solution containing a large amount of magnesium impurities.
[0082] (2) The ferrous sulfate solution containing a large amount of magnesium impurities is mixed with nickel sulfate hexahydrate, manganese sulfate monohydrate, and copper sulfate pentahydrate to prepare a Ni solution with a total metal concentration of 2.3 mol / L. 0.27 Mn 0.28 Cu 0.05 Fe 0.38 Mg 0.02 SO4 mixed salt solution.
[0083] (3) The mixed salt solution was added to the bottom liquid in parallel with 10.8 mol / L sodium hydroxide aqueous solution and 9.7 mol / L ammonia water. The pH of the bottom liquid was 11.60 and the ammonia concentration was 5.8 g / L. Nitrogen was used as the protective gas, and the coprecipitation reaction was carried out at a speed of 700 rpm. The reaction pH was controlled to 11.6, the ammonia concentration in the reactor was 5.5 g / L, and the reaction temperature was controlled at 55 °C to obtain a precursor Ni with a median particle size D50 of 3.90 μm. 0.27 Mn 0.28 Cu 0.05 Fe 0.38 Mg 0.02 (OH)2.
[0084] (4) The precursor and sodium carbonate are mixed at a ratio of 1:1.2 (the molar ratio of the total amount of metal elements in the precursor to the sodium element in the sodium carbonate, the same below), calcined in air at a temperature of 850°C for 12 hours, and the magnesium-doped transition metal layered oxide positive electrode material NaNi is obtained after coarse crushing, fine crushing, and sieving. 0.27 Mn 0.28 Cu 0.05 Fe 0.38 Mg 0.02 O2.
[0085] The scanning electron microscope image of the magnesium-doped multi-element precursor prepared in this example is as follows: Figure 1 and Figure 2 As shown, it can be seen that the particle size uniformity of the precursor is very high, the median particle size D50 is 3.90μm, and the Span value is 0.72.
[0086] Example 2
[0087] This embodiment provides a method for preparing a sodium ion battery precursor, comprising the following steps:
[0088] (1) Ferrous sulfate, a byproduct of titanium dioxide, was dissolved in pure water to prepare a solution with a concentration of 1.5 mol / L. A 30% by mass sodium hydroxide aqueous solution was added to the solution to adjust the pH to 5.6. The solution was filtered with a precision filter with an accuracy of 0.03 μm. 49% by mass dilute sulfuric acid was added to the filtrate to adjust the pH to 1.2 to obtain a ferrous sulfate solution containing a large amount of magnesium impurities.
[0089] (2) Mix the ferrous sulfate solution containing a large amount of magnesium impurities with nickel sulfate hexahydrate, manganese sulfate monohydrate, and copper sulfate pentahydrate to prepare a Ni solution with a concentration of 1.8 mol / L. 0.285 Mn 0.30 Cu 0.05 Fe 0.35 Mg 0.015 SO4 mixed salt solution.
[0090] (3) The mixed salt solution was added to the bottom liquid in parallel with 10.8 mol / L sodium hydroxide aqueous solution and 1.0 mol / L sodium citrate solution. The pH of the bottom liquid was 11.65 and the concentration of sodium citrate was 3.2 g / L. Nitrogen was used as the protective gas, and the coprecipitation reaction was carried out at a speed of 650 rpm. The reaction pH was 11.6, the concentration of sodium citrate was 3.2 g / L, and the temperature was controlled at 50 ° C. The precursor Ni with a median particle size D50 of 3.75 μm was obtained. 0.285 Mn 0.30 Cu 0.05 Fe 0.35 Mg 0.015 (OH)2.
[0091] (4) The precursor and sodium carbonate are mixed at a ratio of 1:1.3, calcined in air at a temperature of 800°C for 15 hours, and the magnesium-doped transition metal layered oxide positive electrode material NaNi is obtained after coarse crushing, fine crushing, and sieving. 0.285 Mn 0.30 Cu 0.05 Fe 0.3 5Mg 0.015 O2.
[0092] The scanning electron microscope image of the magnesium-doped multi-element precursor prepared in this example is as follows: Figure 3 and Figure 4 As shown, it can be seen that the particle size uniformity of the precursor is high, the particle size range is 3.75μm, and the Span value is 0.75.
[0093] Example 3
[0094] The difference between this embodiment and embodiment 1 is that in step (1), sodium hydroxide aqueous solution is added to adjust the pH to 4.5, and in step (2), the ratio of each element in the mixed salt solution is Ni 0.26 Mn 0.28 Cu 0.05 Fe 0.40 Mg 0.01 SO4.
[0095] It should be noted that when the pH is 4.5, the removal effect of impurity ions may be average. Please refer to the subsequent effect test for details.
[0096] Example 4
[0097] The difference between this embodiment and embodiment 1 is that in step (1), sodium hydroxide aqueous solution is added to adjust the pH to 6.5, and in step (2), the ratio of each element in the mixed salt solution is Ni 0.325 Mn 0.28 Cu 0.05 Fe 0.32 Mg 0.025 SO4.
[0098] It should be noted that when the pH is 6.5, a lot of ferrous ions will be precipitated together. On the one hand, the ferrous ion content in the treated ferrous sulfate solution will be reduced, and the ratio of ferrous ions to magnesium ions will deviate; on the other hand, the solid content of the original solution will be increased, resulting in difficulty in filtration.
[0099] It should be added that, in Example 4-5, after adjusting the pH in step 1, the concentration of ferrous ions and the ratio of ferrous ions to magnesium ions are deviated, and the ratio of each element in the mixed salt solution prepared with the ferrous sulfate solution is also deviated. When preparing the mixed salt, the content of manganese and copper is kept unchanged, and the nickel content is used for balancing, and finally a mixed salt solution with different ratios of each element in step (2) is formed.
[0100] Comparative Example 1
[0101] Analytical pure ferrous sulfate was mixed with nickel sulfate hexahydrate, manganese sulfate monohydrate, and copper sulfate pentahydrate to prepare a Ni 0.29 Mn 0.28 Cu 0.05 Fe 0.38 SO4 mixed salt solution. The mixed salt solution was added to the bottom liquid in parallel with 10.8 mol / L sodium hydroxide aqueous solution and 1.0 mol / L sodium citrate solution. The pH of the bottom liquid was 11.65 and the concentration of sodium citrate was 3.2 g / L. Nitrogen was used as the protective gas, and the coprecipitation reaction was carried out at a speed of 650 rpm. The reaction pH was 11.6, the concentration of sodium citrate in the reactor was 3.2 g / L, and the reaction temperature was controlled at 50 ° C to obtain a precursor Ni with a median particle size D50 of 3.75 μm. 0.29 Mn 0.28 Cu 0.05 Fe 0.38 The precursor was mixed with sodium carbonate in a ratio of 1:1.3, calcined in air at 800°C for 15h, and the transition metal layered oxide positive electrode material NaNi was obtained after coarse crushing, fine crushing and sieving. 0.29 Mn 0.28 Cu 0.05 Fe 0.38 O2.
[0102] It should be added that the difference between Comparative Example 1 and Example 2 mainly lies in the ratio of each element in the mixed salt solution.
[0103] Comparative Example 2
[0104] Analytical pure ferrous sulfate was mixed with nickel sulfate hexahydrate, manganese sulfate monohydrate, and copper sulfate pentahydrate to prepare a 2.3 mol / L Ni solution with a concentration of 1.8 mol / L. 0.30 Mn 0.30 Cu 0.05 Fe0.35 SO4 mixed salt solution. The mixed salt solution was added to the bottom liquid in parallel with 10.8 mol / L sodium hydroxide aqueous solution and 9.7 mol / L ammonia water. The pH of the bottom liquid was 11.60 and the concentration of ammonia water was 5.8 g / L. Nitrogen was used as the protective gas, and the coprecipitation reaction was carried out at a speed of 700 rpm. The reaction pH was 11.6, the concentration of ammonia water in the reactor was 5.5 g / L, and the reaction temperature was controlled at 55 ° C to obtain a precursor Ni with a median particle size D50 of 3.9 μm. 0.30 Mn 0.30 Cu 0.05 Fe 0.35 The precursor was mixed with sodium carbonate at a ratio of 1:1.2, and calcined in air at a temperature of 850°C for 12 hours. After coarse crushing, fine crushing, and sieving, the magnesium-doped transition metal layered oxide positive electrode material NaNi 0.30 Mn 0.30 Cu 0.05 Fe 0.35 O2.
[0105] It should be added that the difference between Comparative Example 1 and Example 1 mainly lies in the ratio of each element in the mixed salt solution.
[0106] The scanning electron microscope image of the multi-element precursor prepared in this comparative example is as follows Figure 5 and Figure 6 As shown, it can be seen that: the particle size uniformity of the precursor is high, the particle size range is 3.95μm, and the Span value is 0.68.
[0107] Test Example 1
[0108] The performance of the positive electrode materials prepared in the test examples and comparative examples is shown in Table 1.
[0109] Test method: The transition metal layered oxide positive electrode material in the embodiment and the comparative example, the conductive agent CNT, and the binder PTFE are mixed into a slurry at a mass ratio of 80:15:5, and then coated on a copper foil to prepare a pole piece, and the pole piece is dried in an oven at 80°C. The sodium sheet is used as the counter electrode. The electrolyte is a sodium perchlorate ternary electrolyte, Celgard2400 is a diaphragm, and the battery is assembled in a hand-packed box filled with argon. The cycle performance is tested using an electrochemical workstation at a test temperature of 25°C.
[0110] Table 1 Battery test data obtained from positive electrode materials prepared in Examples and Comparative Examples
[0111]
[0112] As can be seen from Table 1, from Examples 1-4, the battery prepared from the magnesium-doped multinary precursor and positive electrode material of the present invention has a 0.1C discharge capacity of more than 140 mAh / g, a 1C discharge capacity of more than 112 mAh / g, and a capacity retention rate of more than 86% after 100 cycles. The magnesium-doped sodium ion battery multinary precursor and positive electrode material prepared from ferrous sulfate, a byproduct of titanium dioxide, have good performance and a high cycle capacity retention rate.
[0113] From the comparison between Example 1-2 and Comparative Example 1-2, it can be seen that the magnesium-doped sodium ion battery multi-element precursor prepared by the present invention using ferrous sulfate, a byproduct of titanium dioxide, and the positive electrode material further prepared have better high-rate discharge performance and cycle performance.
[0114] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a sodium ion battery precursor, characterized in that: include: The ferrous sulfate byproduct of titanium dioxide is dissolved and then precipitated to remove impurities to obtain a ferrous sulfate solution; The ferrous sulfate solution is mixed with a nickel salt, a manganese salt, and a copper salt to obtain a mixed salt solution, and a precursor is prepared by a coprecipitation reaction using the mixed salt solution in the presence of a precipitant and a complexing agent; In the mixed salt solution, the molar ratio of nickel, manganese, copper, ferrous iron and magnesium is a:b:c:d:e, a+b+c+d+e=1, 0.25 <b<0.35,0.02<c<0.06,0.20<d<0.40,19<d / e<23,a=1-b-c-d-e; The process of preparing the ferrous sulfate solution from the titanium dioxide byproduct ferrous sulfate includes: mixing and dissolving the titanium dioxide byproduct ferrous sulfate and water, then mixing with liquid alkali to adjust the pH value to 5-6, reacting for 10min-30min and separating the solid and liquid, mixing the obtained liquid material with sulfuric acid solution to adjust the pH value to 1-2, and obtaining a magnesium-doped ferrous sulfate solution.
2. The preparation method according to claim 1, characterized in that: In the titanium dioxide byproduct ferrous sulfate, the mass fraction of ferrous ions is 15%-20%, the mass fraction of trivalent iron ions is 2%-7%, the mass fraction of magnesium ions is 0.5%-1.5%, and the remainder is impurity elements; The impurity elements include at least one of titanium, manganese and aluminum, and the mass fraction of each of the impurity elements is less than 0.3%.
3. The preparation method according to claim 2, characterized in that: The liquid alkali is selected from at least one of a sodium hydroxide solution and a potassium hydroxide solution; The solid-liquid separation is carried out by filtering with a precision filter, and the filtering accuracy is 0.2μm-0.7μm; The mass fraction of the sulfuric acid solution is 40%-50%.
4. The preparation method according to claim 1, characterized in that: The total concentration of metal ions in the mixed salt solution is 1.3 mol / L-2.4 mol / L; The nickel salt, the manganese salt and the copper salt are independently selected from at least one of sulfate, phosphate and chloride.
5. The preparation method according to claim 4, characterized in that: The mixed salt solution, the precipitant solution and the complexing agent solution are simultaneously flowed into the bottom liquid to carry out a coprecipitation reaction under a protective gas atmosphere; The precipitant solution is selected from at least one of a sodium hydroxide solution and a potassium hydroxide solution, and the concentration of the precipitant solution is 9 mol / L-12 mol / L; The complexing agent solution is selected from at least one of ammonia water and sodium citrate solution, and the concentration of the complexing agent solution is 1 mol / L-10 mol / L; The base liquid is a mixed solution of water, a precipitant and a complexing agent, wherein the concentration of the precipitant in the base liquid is 15%-30%, and the concentration of the complexing agent is 10%-20%; The reaction temperature of the coprecipitation reaction is 45°C-65°C, the pH of the reaction slurry is 9-12, the concentration of the complexing agent in the reaction slurry is 3g / L-6g / L, and the median particle size D50 of the obtained precursor is 3μm-4μm; The stirring speed during the coprecipitation reaction was controlled to be 500 rpm-800 rpm.
6. A sodium ion battery precursor, characterized in that: Prepared by the preparation method according to any one of claims 1 to 5; Its chemical formula is Ni (1-b-c-d-e) Mn b Cu c Fe d Mg e (OH)2, 0.25 <b<0.35,0.02<c<0.06,0.20<d<0.40,19<d / e<23。 7. A method for preparing a positive electrode material for a sodium ion battery, characterized in that: The preparation is carried out using a sodium source and the sodium ion battery precursor according to claim 6 as raw materials.
8. The preparation method according to claim 7, characterized in that: The preparation method comprises: mixing and sintering the sodium source and the sodium ion battery precursor, controlling the sintering temperature to be 700° C.-900° C., and the sintering time to be 10 h-15 h; The molar ratio of the sodium element in the sodium source to the total amount of metal elements in the sodium ion battery precursor is (1.1-1.3):1; The sodium source is selected from at least one of sodium carbonate and sodium acetate.
9. A sodium ion battery positive electrode material, characterized in that: It is prepared by the preparation method according to claim 7 or 8.
10. A sodium ion battery, characterized in that: Including the sodium ion battery positive electrode material according to claim 9.
Citation Information
Patent Citations
Sodium-ion battery positive electrode material and preparation method thereof
CN113889603A
Method for synthesizing sodium ferric manganese phosphate by treating industrial titanium dioxide by-product
CN114436235A