A kind of solid waste modified concrete and preparation method thereof
By adding hydrated calcium silicate and fiber composite materials to solid waste-based cement and using rapid temperature-raising sintering technology, the problem of insufficient strength and hydration capacity of solid waste-based cement is solved, and the strength and durability of concrete are significantly improved.
Patent Information
- Application Number
- CN202411187269.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-08-28
AI Technical Summary
The existing solid waste-based cement has low strength and hardness, weak hydration capacity, and limited life, making it difficult to meet the needs of building materials.
By adding hydrated calcium silicate to the raw materials and adopting a rapid heating sintering method, combining specific fiber composite materials to compound them in solid waste-based cement mortar, the strength, hardness and hydration capacity of solid waste-based concrete are improved.
It significantly improves the early and later strength of solid waste-based concrete, enhances crack resistance and durability, improves the uniformity of hydration reaction and the quality of clinker, delays the settling time of gelled materials, and controls the hydration speed. , improves mechanical strength and hardness.
Smart Images

Figure CN118702454B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of building materials, and specifically discloses a solid waste-based modified concrete and a preparation method thereof. Background Art
[0002] Ordinary Portland cement has a series of excellent properties and plays an important role in the current construction, transportation, roadbed materials and other industries. However, the production process of cement clinker consumes a large amount of natural non-renewable resources such as limestone, clay and sandstone, which intensifies the exploitation of limestone and clay resources and causes ecological damage. At the same time, limestone produces a large amount of CO during thermal decomposition. 2 , which is not conducive to the low-carbon green development needs of the cement industry. Therefore, developing low-carbon alternative raw materials for cement production can effectively reduce the exploitation of natural resources.
[0003] Calcium carbide slag (CCS) is a solid waste generated in the acetylene production process. Its main component is Ca(OH) 2 , CaO and H are produced during thermal decomposition 2 O, almost no CO emissions to the outside 2 Therefore, using carbide slag to replace part of the lime raw materials can significantly reduce the carbon emissions caused by carbonate decomposition in the cement production process. However, the carbide slag produced in my country each year is not enough to meet the demand for raw materials in my country's cement production. It is necessary to further promote the coordinated use of carbide slag and other bulk solid wastes in the cement industry.
[0004] With the continuous development of urbanization and industrialization, construction waste is increasing day by day. In order to solve the ecological and environmental problems caused by construction waste and realize its efficient disposal and resource utilization, a lot of research has been carried out on the preparation, performance optimization and application of recycled aggregates from construction waste. In the recycling process of recycled aggregates, a large amount of recycled fine powder (RCP) that is difficult to use will be produced. The recycled fine powder is mainly composed of hardened cement stone and some incompletely separated aggregates. Its main chemical composition is similar to that of cement raw materials, and can be added to cement as a supplementary cementitious material.
[0005] At present, solid waste-based cement generally has the problems of low strength and hardness, weak hydration capacity and limited life. Therefore, there is an urgent need to find a solid waste-based modified concrete to solve the above problems. Summary of the invention
[0006] In response to the above technical problems, the present invention provides a solid waste-based modified concrete and a preparation method thereof, which improves the strength, hardness and hydration capacity of the solid waste-based concrete by adding hydrated calcium silicate to the raw materials, sintering the solid waste-based cement raw materials by rapidly heating up, and compounding a specific fiber composite material into the solid waste-based cement mortar.
[0007] In order to solve the above technical problems, the technical solution provided by the present invention is:
[0008] In a first aspect, the present invention provides a method for preparing solid waste-based modified concrete, comprising the following steps:
[0009] S1, mixing carbide slag, recycled micro powder, fly ash and hydrated calcium silicate, adding water, pressing, and obtaining solid waste-based cement raw material;
[0010] S2, preheating the solid waste-based cement raw material at 380°C-420°C; then heating it to 900°C-1000°C at a rate of 50°C / s-100°C / s for a first sintering; then heating it to 1300°C-1450°C at a rate of 50°C / s-100°C / s for a second sintering to obtain solid waste-based cement clinker;
[0011] S3, mixing the solid waste-based cement clinker with desulfurized gypsum, adding polyacrylamide and water to obtain solid waste-based cement mortar;
[0012] S4, adding epoxy resin and diamond powder into a solvent, and then adding basalt fiber to obtain a fiber composite material;
[0013] S5, mixing the fiber composite material and the solid waste-based cement mortar, and curing them to obtain solid waste-based modified concrete.
[0014] It should be noted that the present invention does not limit the sequence between S4 and S1 to S3.
[0015] Compared with the prior art, the preparation method of solid waste-based modified concrete provided by the present invention uses carbide slag, recycled micropowder and fly ash as main raw materials, all of which are solid wastes, and their main chemical components are similar to the chemical components of cement raw materials. The present invention uses them as cement mortar, realizing efficient disposal and resource utilization of solid waste; fly ash has a large specific surface area, high surface energy, and multiple active points such as aluminum and silicon. After fly ash is compounded with carbide slag, it plays the role of electrical neutralization and adsorption bridging, which can destroy the stability of carbide slag colloidal particles, so that the dispersed small particles gather together to form large particles, thereby improving the dehydration of carbide slag. The present invention adds hydrated calcium silicate to solid waste-based cement raw materials, reduces the heat release rate during cement hydration, is conducive to more uniform heat release of solid waste-based cement, promotes the hydration reaction, thereby reducing the hydration reaction heat caused by too fast hardening of cement, not only effectively improves the early strength and late strength of concrete, but also enhances the crack resistance and durability of concrete.
[0016] The present invention adds water to the above raw materials and presses them into blocks, thereby avoiding dust pollution during operation, reducing the loss of raw materials, increasing the utilization of space, facilitating transportation, and improving the thermal stability of raw materials during sintering; then the obtained solid waste-based cement raw material is preheated, and then gradually heated to a specific temperature for 2 sintering to obtain solid waste-based cement clinker. The preheating treatment can remove the chemical moisture and mechanical moisture inside the solid waste-based cement raw material, prevent these moistures from generating steam pressure at high temperature, and further affect the crystal form and melting degree of the solid waste-based cement clinker, and prepare for subsequent high-temperature sintering; in the first sintering and the second sintering, a rapid heating method is adopted to shorten the residence time of the material at high temperature, reduce the mass content of free CaO in the solid waste-based cement clinker, and is beneficial to the improvement of the quality of the clinker, so that the solid waste-based cement clinker has the characteristics of fine crystals, lattice defects, and large dislocation density, thereby improving the hydration rate and strength of the clinker and improving the grindability of the clinker.
[0017] The present invention adds desulfurized gypsum and polyacrylamide to the solid waste-based cement clinker. The introduction of desulfurized gypsum can effectively delay the setting time of the cementitious material, thereby controlling the hydration rate of the solid waste-based cement and improving the mechanical strength of the solid waste-based concrete. Polyacrylamide is a polymer flocculant adsorbed on the surface of the solid waste-based cement particles, and has a polymer long-chain structure. It can connect two or more colloidal particles together by "bridging" to form flocs, thereby causing flocculation precipitation. Polyacrylamide can also effectively improve the dehydration effect of carbide slag, affect the fluidity of cement mortar, and ensure the mechanical strength of solid waste-based concrete. The present invention also adds diamond-basalt fiber composite materials to the solid waste-based cement mortar, further improving the hardness and strength of the solid waste-based concrete.
[0018] Preferably, in S1, the mass ratio of the carbide slag, the regenerated micropowder, the fly ash, the hydrated calcium silicate and the water is 50:(18~22):(18~22):(9~11):(0.5~1.5).
[0019] Preferably, in S1, the method for preparing hydrated calcium silicate comprises the following steps:
[0020] Mix soluble calcium salt, surfactant and water, add silicate aqueous solution, and carry out double decomposition reaction at 45℃~55℃ to obtain hydrated calcium silicate.
[0021] Further preferably, the soluble calcium salt is calcium nitrate.
[0022] Further preferably, the surfactant is hexadecyltrimethylammonium bromide.
[0023] Further preferably, the silicate aqueous solution is a 0.13M to 0.17M sodium silicate aqueous solution.
[0024] Further preferably, the usage ratio of the soluble calcium salt, the surfactant, the water and the silicate aqueous solution is (140~160)g:(6~8)g:10L:(4.5~5.5)L.
[0025] Further preferably, the double decomposition reaction time is 5h~6h.
[0026] Further preferably, after the double decomposition reaction, the process further comprises: aging the reaction system at room temperature for 22 h to 26 h, separating the solid from the liquid, washing and drying the obtained solid to obtain hydrated calcium silicate.
[0027] For example, the obtained solid is first washed with water for 3 times, then washed with ethanol for 3 times, and finally dried at 40°C to 50°C for 10h to 13h to obtain suitable calcium silicate.
[0028] Preferably, in S1, the fineness of the carbide slag, the regenerated fine powder, the fly ash and the hydrated calcium silicate is such that the residue on the 75 μm square hole sieve is ≤5%.
[0029] For example, in S1, carbide slag, regenerated micro powder, fly ash and hydrated calcium silicate are first subjected to high-energy ball milling at 750rpm~850rpm for 30min~35min to obtain a mixed material with a sieve residue of 75μm square hole sieve ≤5%, and then water is added for subsequent operations.
[0030] Preferably, in S1, the pressing pressure is 25 MPa~35 MPa.
[0031] Preferably, in S1, after the pressing is completed, the obtained block material is dried at 100° C. to 120° C. for 10 h to 12 h to obtain solid waste-based cement raw material.
[0032] For example, in S1, the block material can be a square cake or a cylinder; the size can be selected to be 10cm×10cm×3cm or Φ5cm×10cm.
[0033] Preferably, in S2, the preheating process is carried out by means of programmed temperature increase to 380°C to 420°C, and the heating rate is 45°C / s to 55°C / s.
[0034] Preferably, in S2, the preheating holding time is 15 min to 20 min.
[0035] By limiting the preheating conditions, the present invention can further volatilize the water inside the solid waste-based cement raw material and start to decompose the organic components, which is beneficial to the smooth progress of subsequent sintering.
[0036] Preferably, in S2, the holding time of the first sintering is 25 min to 30 min.
[0037] During the first sintering process, the organic components of the solid waste-based cement are gradually decomposed, and the minerals in the raw materials are decomposed or in a semi-molten state, releasing a large amount of oxygen and carbon dioxide, resulting in weight loss.
[0038] Preferably, in S2, the holding time of the second sintering is 25 min to 30 min.
[0039] During the second sintering process, the solid waste-based cement is fully sintered, the chemical components in the raw materials are more evenly distributed, and the reaction proceeds more thoroughly.
[0040] For example, in S2, after the second sintering is completed, it also includes air cooling to room temperature to obtain solid waste-based cement clinker.
[0041] Preferably, in S3, the mass ratio of the solid waste-based cement clinker, the desulfurized gypsum, the polyacrylamide and the water is 100:(5~6):(0.02~0.05):(38~42).
[0042] Preferably, in S4, the epoxy resin is bisphenol A epoxy resin.
[0043] Preferably, in S4, the particle size of the diamond powder is 0.5 μm to 1 μm.
[0044] Preferably, in S4, the solvent is an ethanol aqueous solution with a volume concentration of 80% to 85%.
[0045] Preferably, in S4, the basalt fiber has a diameter of 0.1 μm to 0.3 μm and a length of 5 μm to 15 μm.
[0046] Preferably, in S4, the usage ratio of the epoxy resin, the diamond powder, the solvent and the basalt fiber is 10 mL:(2.8~3.2) g:(190~210) mL:(4.7~5.3) g.
[0047] Preferably, in S4, epoxy resin is first added to the solvent, stirred at 50°C~60°C and 600rpm~800rmp for 5min~10min, and then diamond powder is added, stirred at 80°C~100°C and 1000rpm~1200rmp for 1h~1.5h; then basalt fiber is added to the obtained diamond powder wrapped in epoxy resin, and stirred at 40°C~45°C and 1000rpm~1200rmp for 1.5h~2h to obtain the fiber composite material.
[0048] In the present invention, the epoxy resin can bond the diamond powder and the basalt fiber, and both the diamond powder and the basalt fiber can further improve the hardness and strength of the solid waste-based concrete. In the present invention, a specific amount of epoxy resin, diamond powder and basalt fiber are mixed at a specific temperature and rotation speed, which can exert the synergistic effect of each substance, facilitate the subsequent mixing with the solid waste-based cement mortar, and further improve the strength and hardness of the solid waste-based modified concrete.
[0049] Preferably, in S5, the mass ratio of the fiber composite material to the solid waste-based cement mortar is (2.3~2.6):10.
[0050] Preferably, in S5, the curing time is 7 to 10 days.
[0051] In a second aspect, the present invention provides a solid waste-based modified concrete prepared by the above-mentioned method for preparing solid waste-based modified concrete.
[0052] The results of the embodiments show that the 7d compressive strength of the solid waste-based modified concrete provided by the present invention is above 45MPa, the 28d compressive strength is above 69MPa, the hardness can reach above 80HV, and under acid, alkali and salt conditions, there is no cracking, peeling or shedding and the state is maintained in good condition. BRIEF DESCRIPTION OF THE DRAWINGS
[0053] Figure 1 The SEM image of the mixture of carbide slag, regenerated micropowder, fly ash and hydrated calcium silicate in Example 1 of the present invention;
[0054] Figure 2 is a SEM image of the basalt fiber of the present invention;
[0055] Figure 3 This is a SEM image of a mixed system of a fiber composite material and solid waste-based cement mortar in Example 1 of the present invention;
[0056] Figure 4 This is a SEM image of the solid waste-based modified concrete of Example 1 of the present invention;
[0057] Figure 5 This is a SEM image of the solid waste-based modified concrete of Example 2 of the present invention;
[0058] Figure 6 This is the SEM image of the solid waste-based modified concrete of Example 3 of the present invention. DETAILED DESCRIPTION
[0059] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0060] Example 1
[0061] This embodiment provides a method for preparing solid waste-based modified concrete, comprising the following steps:
[0062] Sa, will Ca (NO 3 ) 2 ·4H 2 O, cetyl trimethyl ammonium bromide and water were mixed, and 0.15 M Na 2 SiO 3 9H 2 O aqueous solution, mix evenly; carry out double decomposition reaction at 50°C for 5.5h, then age the reaction system at room temperature for 24h, separate the solid and the liquid, wash the obtained solid with water 3 times, then wash it with ethanol 3 times, and dry it at 45°C for 12h to obtain hydrated calcium silicate.
[0063] Ca(NO 3 ) 2 ·4H 2 O, hexadecyltrimethylammonium bromide, water and Na 2 SiO 3 9H 2 The dosage ratio of O aqueous solution is 150g:7g:10L:5L.
[0064] Sb, firstly, carbide slag, regenerated micro powder, fly ash and hydrated calcium silicate were subjected to high energy ball milling at 800 rpm for 30 min to obtain a mixed material with a sieve residue of 75 μm square hole sieve ≤ 5% (the SEM image of the mixed material is shown in FIG. Figure 1 As shown), water was added and mixed evenly; the mixture was pressed into a square cake of 10 cm × 10 cm × 3 cm at 30 MPa, and dried at 110°C for 11 hours to obtain solid waste-based cement raw material.
[0065] The mass ratio of carbide slag, recycled micropowder, fly ash, hydrated calcium silicate and water is 50:20:20:10:1.
[0066] Sc, put the solid waste-based cement raw material into a vacuum furnace, heat it to 400℃ at a rate of 50℃ / s for preheating, and keep it warm for 18min; then heat it to 950℃ at a rate of 80℃ / s for the first sintering, and keep it warm for 28min; then heat it to 1400℃ at a rate of 80℃ / s for the second sintering, keep it warm for 27min, and air-cool it to room temperature to obtain solid waste-based cement clinker.
[0067] Sd, mix the solid waste-based cement clinker with the desulfurized gypsum, add polyacrylamide and water, mix well, and obtain the solid waste-based cement mortar.
[0068] The mass ratio of solid waste-based cement clinker, desulfurized gypsum, polyacrylamide and water is 100:5.5:0.03:40.
[0069] Se, first add bisphenol A epoxy resin to ethanol aqueous solution with a volume concentration of 83%, stir at 55°C and 700 rpm for 8 minutes, then add diamond powder with a particle size of 0.5 μm~1 μm, stir at 90°C and 1100 rpm for 1.2 hours; then add basalt fiber (SEM image of basalt fiber is shown in Figure 2) to the diamond powder wrapped by epoxy resin. Figure 2 As shown), the mixture was stirred at 43°C and 1100 rpm for 1.8 h to obtain a fiber composite material.
[0070] The usage ratio of epoxy resin, diamond powder, ethanol aqueous solution and basalt fiber is 10mL:3g:200mL:5g.
[0071] Sf, the fiber composite material and solid waste-based cement mortar with a mass ratio of 2.4:10 were mixed and cured for 8 days to obtain solid waste-based modified concrete. The SEM image of the mixed system of fiber composite material and solid waste-based cement mortar is shown in Figure 3 As shown in Figure 2, it can be seen that the materials are aggregated or wrapped together; the SEM image of solid waste-based modified concrete is shown in Figure 2 Figure 4 It should be noted that there is no order of precedence between Se and Sa~Sd.
[0072] Example 2
[0073] This embodiment provides a method for preparing solid waste-based modified concrete, comprising the following steps:
[0074] Sa, will Ca (NO 3 ) 2 ·4H 2 O, cetyl trimethyl ammonium bromide and water were mixed, and 0.13 M Na 2 SiO 3 9H 2 O aqueous solution, mix evenly; carry out double decomposition reaction at 45°C for 6h, then age the reaction system at room temperature for 22h, separate the solid and the liquid, wash the obtained solid with water 3 times, then wash it with ethanol 3 times, and dry it at 40°C for 13h to obtain hydrated calcium silicate.
[0075] Ca(NO 3 ) 2 ·4H 2 O, hexadecyltrimethylammonium bromide, water and Na 2 SiO 3 9H 2 The dosage ratio of O aqueous solution is 140g:6g:10L:5.5L.
[0076] Sb, firstly subject carbide slag, recycled micro powder, fly ash and hydrated calcium silicate to high-energy ball milling at 750rpm for 35min to obtain a mixture with a sieve residue of 75μm square hole sieve ≤5%, then add water and mix evenly; press into a Φ5cm×10cm cylinder at 25MPa, dry at 100℃ for 12h to obtain solid waste-based cement raw material.
[0077] The mass ratio of carbide slag, recycled micropowder, fly ash, hydrated calcium silicate and water is 50:18:18:10:0.5.
[0078] Sc, put the solid waste-based cement raw material into a vacuum furnace, heat it to 380℃ at a rate of 55℃ / s for preheating, and keep it warm for 20min; then heat it to 900℃ at a rate of 100℃ / s for the first sintering, and keep it warm for 30min; then heat it to 1300℃ at a rate of 100℃ / s for the second sintering, keep it warm for 30min, and air-cool it to room temperature to obtain solid waste-based cement clinker.
[0079] Sd, mix the solid waste-based cement clinker with the desulfurized gypsum, add polyacrylamide and water, mix well, and obtain the solid waste-based cement mortar.
[0080] The mass ratio of solid waste-based cement clinker, desulfurized gypsum, polyacrylamide and water is 100:5:0.05:38.
[0081] Se, first add bisphenol A epoxy resin to an ethanol aqueous solution with a volume concentration of 80%, stir at 50°C and 600rpm for 10min, then add diamond powder with a particle size of 0.5μm~1μm, and stir at 80°C and 1000rpm for 1.5h; then add basalt fiber (the same as Example 1) to the obtained diamond powder wrapped by epoxy resin, stir at 40°C and 1000rpm for 2h to obtain a fiber composite material.
[0082] The usage ratio of epoxy resin, diamond powder, ethanol aqueous solution and basalt fiber is 10mL:2.8g:210mL:4.7g.
[0083] Sf, the fiber composite material and solid waste-based cement mortar with a mass ratio of 2.3:10 were mixed and cured for 7 days to obtain solid waste-based modified concrete. Figure 5 shown.
[0084] It should be noted that there is no order of precedence between Se and Sa~Sd.
[0085] Example 3
[0086] This embodiment provides a method for preparing solid waste-based modified concrete, comprising the following steps:
[0087] Sa, will Ca (NO 3 ) 2 ·4H 2 O, cetyl trimethyl ammonium bromide and water were mixed, and 0.17 M Na 2 SiO 3 9H 2 O aqueous solution, mix evenly; carry out double decomposition reaction at 55°C for 5h, then age the reaction system at room temperature for 26h, separate the solid and the liquid, wash the obtained solid with water 3 times, then wash it with ethanol 3 times, and dry it at 50°C for 10h to obtain hydrated calcium silicate.
[0088] Ca(NO 3 ) 2 ·4H 2 O, hexadecyltrimethylammonium bromide, water and Na 2 SiO 3 9H 2 The dosage ratio of O aqueous solution is 160g:8g:10L:4.5L.
[0089] Sb, firstly carry out high-energy ball milling of carbide slag, recycled micro powder, fly ash and hydrated calcium silicate at 850 rpm for 30 min to obtain a mixture with a sieve residue of 75 μm square hole sieve ≤ 5%, then add water and mix evenly; press into a Φ5 cm × 10 cm cylinder at 35 MPa, dry at 120 ° C for 10 h, and obtain solid waste-based cement raw material.
[0090] The mass ratio of carbide slag, recycled micropowder, fly ash, hydrated calcium silicate and water is 50:22:22:11:1.5.
[0091] Sc, put the solid waste-based cement raw material into a vacuum furnace, heat it to 420℃ at a rate of 45℃ / s for preheating, and keep it warm for 15min; then heat it to 1000℃ at a rate of 50℃ / s for the first sintering, and keep it warm for 25min; then heat it to 1450℃ at a rate of 50℃ / s for the second sintering, keep it warm for 25min, and air-cool it to room temperature to obtain solid waste-based cement clinker.
[0092] Sd, mix the solid waste-based cement clinker with the desulfurized gypsum, add polyacrylamide and water, mix well, and obtain the solid waste-based cement mortar.
[0093] The mass ratio of solid waste-based cement clinker, desulfurized gypsum, polyacrylamide and water is 100:6:0.02:42.
[0094] Se, first add bisphenol A epoxy resin to an ethanol aqueous solution with a volume concentration of 85%, stir at 60°C and 800 rpm for 5 minutes, then add diamond powder with a particle size of 0.5 μm~1 μm, and stir at 100°C and 1200 rpm for 1 hour; then add basalt fiber (the same as in Example 1) to the obtained diamond powder wrapped by epoxy resin, stir at 45°C and 1200 rpm for 1.5 hours to obtain a fiber composite material.
[0095] The usage ratio of epoxy resin, diamond powder, ethanol aqueous solution and basalt fiber is 10mL:3.2g:190mL:5.3g.
[0096] Sf, the fiber composite material and solid waste-based cement mortar with a mass ratio of 2.6:10 were mixed and cured for 10 days to obtain solid waste-based modified concrete. Figure 6 shown.
[0097] It should be noted that there is no order of precedence between Se and Sa~Sd.
[0098] from Figures 4 to 6 It can be seen that the solid waste-based modified concrete has high density, low porosity, good surface flatness, fine particles, and no tiny cracks. Lower porosity means that the interior of the concrete is denser and the contact between particles is closer, thereby improving the compressive and tensile strengths of the concrete; low porosity also reduces the penetration channels of moisture and harmful substances, reduces the risk of concrete erosion, and improves its durability. Fine particles can fill the voids in the concrete, increase the density of the concrete, and thus improve the compressive and tensile strengths of the concrete; in addition, fine particles can slow down the shrinkage of the concrete, reduce cracking caused by shrinkage, and improve the crack resistance of the concrete. Good surface flatness is conducive to the smooth progress of subsequent construction, such as laying floors and painting.
[0099] Comparative Example 1
[0100] This comparative example provides a method for preparing solid waste-based modified concrete, which is similar to Example 1, except that calcium silicate hydrate is omitted from the raw materials and step Sa is omitted. The remaining operations are the same as those in Example 1 and will not be described in detail.
[0101] Comparative Example 2
[0102] This comparative example provides a method for preparing solid waste-based modified concrete, which is similar to Example 1, except that fly ash is replaced with carbide slag of equal mass in Sb. The remaining operations are the same as those in Example 1 and will not be described in detail.
[0103] Comparative Example 3
[0104] This comparative example provides a method for preparing solid waste-based modified concrete, which is similar to Example 1, except that the preheating step is omitted in Sc, and the solid waste-based cement raw material is directly sintered twice. The remaining operations are the same as those in Example 1 and will not be repeated.
[0105] Comparative Example 4
[0106] This comparative example provides a method for preparing solid waste-based modified concrete, which is similar to Example 1, except that the first sintering is omitted in Sc, and the preheated solid waste-based cement raw material is directly subjected to the second sintering, and the insulation time of the second sintering is 50 minutes. The remaining operations are the same as those in Example 1 and will not be repeated.
[0107] Comparative Example 5
[0108] This comparative example provides a method for preparing solid waste-based modified concrete, which is similar to Example 1, except that the heating rates of the first sintering and the second sintering in Sc are both 80°C / min, and the insulation time of the first sintering and the second sintering is both 20min. The remaining operations are the same as those in Example 1 and will not be repeated.
[0109] Comparative Example 6
[0110] This comparative example provides a method for preparing solid waste-based concrete, which is similar to Example 1, except that step Se of Example 1 is omitted, and the solid waste-based cement mortar is directly cured. Specifically, the following steps are included:
[0111] Sa~Sd are the same as those in Example 1 and will not be described in detail.
[0112] Se, the solid waste based cement mortar is cured for 8 days to obtain the solid waste based concrete.
[0113] Comparative Example 7
[0114] This comparative example provides a method for preparing solid waste-based concrete, which is similar to Example 1, except that the bisphenol A epoxy resin and solvent (ethanol aqueous solution) in Example 1 are omitted, and diamond powder and basalt fiber are directly mixed with solid waste-based cement mortar. Specifically, the following steps are included:
[0115] Sa~Sd are the same as those in Example 1 and will not be described in detail.
[0116] Se, diamond powder and basalt fiber with a particle size of 0.5 μm to 1 μm (the same as in Example 1) were added to the solid waste-based cement mortar, mixed evenly, and cured for 8 days to obtain solid waste-based concrete.
[0117] The mass ratio of solid waste-based cement mortar, diamond powder and basalt fiber is 10:0.9:1.5 (the same as in Example 1).
[0118] Comparative Example 8
[0119] This comparative example provides a method for preparing solid waste-based modified concrete, which is similar to Example 1, except that the basalt fiber in Example 1 is omitted. Specifically, the method comprises the following steps:
[0120] Sa~Sd are the same as those in Example 1 and will not be described in detail.
[0121] Se, first add bisphenol A epoxy resin into ethanol aqueous solution with a volume concentration of 83%, stir at 55°C and 700 rpm for 8 minutes, then add diamond powder with a particle size of 0.5μm~1μm, stir at 90°C and 1100 rpm for 1.2 hours to obtain a fiber composite material.
[0122] The mass volume ratio of epoxy resin, diamond powder and solvent is 10mL:3g:200mL.
[0123] Sf is the same as that in Example 1 and will not be described in detail.
[0124] Verification test
[0125] In order to verify that the solid waste-based modified concrete provided by the present invention has excellent comprehensive performance, the solid waste-based concrete provided by Examples 1 to 3 and Comparative Examples 1 to 8 were subjected to corresponding performance tests in accordance with GB / T50081-2002 standard.
[0126] Compressive strength: A 100-ton Instron microcomputer-controlled hydraulic servo testing machine was used for displacement control, with a loading rate of 0.2 mm / min and a strain rate of 2.36×10 -5 / s.
[0127] Hardness: The hardness of the sample was tested using a HV-1000 micro Vickers hardness tester under an external load of 50 g.
[0128] The test results are shown in Table 1. It can be seen from the test results in Table 1 that the solid waste-based modified concrete provided by the present invention uses carbide slag, recycled micropowder, fly ash and hydrated calcium silicate in a specific ratio as the main raw materials. The addition of hydrated calcium silicate reduces the heat release rate during cement hydration, which is conducive to more uniform heat release of solid waste-based cement, promotes the hydration reaction, effectively improves the early and late strengths of concrete, and can also enhance the crack resistance and durability of concrete; preheating treatment can remove chemical moisture and mechanical moisture in the solid waste-based cement raw materials, avoid these moistures from generating steam pressure at high temperature, and then affect the solid waste-based cement clinker. The crystal form and melting degree of the solid waste-based cement clinker are improved, and preparation is made for subsequent high-temperature sintering; in the first sintering and the second sintering, a rapid heating method is adopted to shorten the residence time of the material at high temperature, reduce the mass content of free CaO in the solid waste-based cement clinker, which is beneficial to the improvement of the quality of the clinker, and make the solid waste-based cement clinker have the characteristics of fine crystals, lattice defects, and high dislocation density, thereby improving the hydration rate and strength of the clinker and improving the grindability of the clinker; the present invention also adds a basalt fiber composite material with epoxy resin-wrapped diamond powder to the solid waste-based cement mortar, further improving the hardness and strength of the solid waste-based concrete.
[0129] Table 1 Performance test results of solid waste-based concrete provided by the embodiments and comparative examples
[0130]
[0131] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modification, equivalent substitution or improvement made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing solid waste-based modified concrete, characterized in that: The following steps are involved: S1, mixing carbide slag, recycled micro powder, fly ash and hydrated calcium silicate, adding water, pressing, and obtaining solid waste-based cement raw material; The mass ratio of the carbide slag, the regenerated micropowder, the fly ash, the hydrated calcium silicate and the water is 50:(18-22):(18-22):(9-11):(0.5-1.5); The preparation method of the hydrated calcium silicate comprises the following steps: Mix soluble calcium salt, surfactant and water, add silicate aqueous solution, and perform double decomposition reaction at 45℃~55℃ to obtain hydrated calcium silicate; S2, preheating the solid waste-based cement raw material at 380°C-420°C; then heating it to 900°C-1000°C at a rate of 50°C / s-100°C / s for a first sintering; then heating it to 1300°C-1450°C at a rate of 50°C / s-100°C / s for a second sintering to obtain solid waste-based cement clinker; S3, mixing the solid waste-based cement clinker with desulfurized gypsum, adding polyacrylamide and water to obtain solid waste-based cement mortar; S4, adding epoxy resin and diamond powder into a solvent, and then adding basalt fiber to obtain a fiber composite material; The diameter of the basalt fiber is 0.1 μm to 0.3 μm, and the length is 5 μm to 15 μm; the usage ratio of the epoxy resin, the diamond powder, the solvent and the basalt fiber is 10 mL: (2.8 to 3.2) g: (190 to 210) mL: (4.7 to 5.3) g; S5, mixing the fiber composite material and the solid waste-based cement mortar, wherein the mass ratio of the fiber composite material to the solid waste-based cement mortar is (2.3-2.6):10; and curing to obtain solid waste-based modified concrete.
2. The method for preparing solid waste-based modified concrete according to claim 1, characterized in that: In S3, the mass ratio of the solid waste-based cement clinker, the desulfurized gypsum, the polyacrylamide and the water is 100:(5~6):(0.02~0.05):(38~42).
3. The method for preparing solid waste-based modified concrete according to claim 1, characterized in that: In S1, the soluble calcium salt is calcium nitrate; The surfactant is hexadecyltrimethylammonium bromide; The silicate aqueous solution is a 0.13M to 0.17M sodium silicate aqueous solution; The usage ratio of the soluble calcium salt, the surfactant, the water and the silicate aqueous solution is (140-160) g: (6-8) g: 10 L: (4.5-5.5) L; The double decomposition reaction time is 5h~6h.
4. The method for preparing solid waste-based modified concrete according to claim 1, characterized in that: In S1, the fineness of the carbide slag, the regenerated micro powder, the fly ash and the hydrated calcium silicate is ≤5% of the sieve residue of a 75 μm square hole sieve; In S1, the pressing pressure is 25MPa~35MPa.
5. The method for preparing solid waste-based modified concrete according to claim 1, characterized in that: In S2, the preheating process is carried out by heating the temperature to 380°C to 420°C in a programmed heating manner, and the heating rate is 45°C / s to 55°C / s; In S2, the preheating holding time is 15min~20min; In S2, the first sintering holding time is 25min~30min; In S2, the second sintering heat preservation time is 25min~30min.
6. The method for preparing solid waste-based modified concrete according to claim 1, characterized in that: In S4, the epoxy resin is bisphenol A epoxy resin; In S4, the particle size of the diamond powder is 0.5 μm to 1 μm; In S4, the solvent is an ethanol aqueous solution with a volume concentration of 80% to 85%.
7. The method for preparing solid waste-based modified concrete according to claim 1, characterized in that: In S4, epoxy resin is first added to the solvent, and stirred at 50°C~60°C and 600rpm~800rmp for 5min~10min, and then diamond powder is added, and stirred at 80°C~100°C and 1000rpm~1200rmp for 1h~1.5h; then basalt fiber is added to the obtained diamond powder wrapped in epoxy resin, and stirred at 40°C~45°C and 1000rpm~1200rmp for 1.5h~2h to obtain the fiber composite material.
8. The method for preparing solid waste-based modified concrete according to claim 1, characterized in that: In S5, the curing time is 7 to 10 days.
9. A solid waste-based modified concrete prepared by the method for preparing solid waste-based modified concrete according to any one of claims 1 to 8.