Yttria granulated powder for plasma corrosion resistant thermal spraying and its preparation method and application
By using specific dispersants and fluxes, combined with spray granulation and low-temperature calcination processes, the problems of uneven mixing and poor density of yttrium oxide granulated powder were solved, achieving the preparation of yttrium oxide granulated powder with high yield and strong corrosion resistance, which is suitable for semiconductor coatings.
Patent Information
- Application Number
- CN202411205209.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-08-30
AI Technical Summary
Existing yttrium oxide granulated powders suffer from problems such as uneven mixing, poor density, short service life, complex preparation process, and high energy consumption during preparation. Furthermore, the coating is prone to pinking.
Yttrium oxide granulated powder is prepared by spray granulation and low-temperature calcination using a specific combination of dispersants, temporary binders and fluxes. This process controls particle size and improves density, preventing the coating from turning pink.
The prepared yttrium oxide granulated powder has controllable particle size, high yield, good density, strong corrosion resistance, long service life, and the process is simple, energy-saving and environmentally friendly.
Smart Images

Figure CN118702490B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of preparation and application of yttrium oxide granulated powder, and specifically relates to yttrium oxide granulated powder for plasma corrosion resistant thermal spraying and a preparation method and application thereof. Background Art
[0002] Semiconductor manufacturing usually uses plasma etching process, the principle is high-frequency glow discharge reaction, which activates the reaction gas into active particles, such as atoms or free radicals. These active particles diffuse to the part to be etched, and replace the "silicon-silicon" bond with the "silicon-halogen" bond, thereby producing volatile silicon-halogen compounds. Typical etching gases are fluorine-based gases, such as SF6, CF4, CHF3, ClF3, HF, or chlorine-based gases, such as Cl2, BCl3, HCl, etc. During the etching process, aluminum alloys, quartz, ceramics and other parts in contact with plasma will produce particle pollution due to bombardment and corrosion. Particles released from the surface of the equipment will cause defects on the wafer, which will cause the wafer to be scrapped. Therefore, these contamination particles will have a significant impact on the quality and output of key components.
[0003] The traditional protection method is to use aluminum anodized coating, but the corrosion resistance of the coating is not high. Because yttrium oxide has good high-temperature stability and heat resistance in harsh environments, it can be used as a corrosion-resistant coating material and has become the most widely used plasma corrosion-resistant material. Spraying a layer of 0.15-0.18mm thick yttrium oxide coating on the inner wall surface of the etcher cavity can effectively avoid the contamination of the cavity substrate on the silicon wafer etching, and at the same time extend the overhaul life of the etcher. At present, it is usually necessary to add a defoaming agent to eliminate the foam in the slurry during the preparation of yttrium oxide granulation powder, but the defoaming agent has poor hydrophilicity and low solubility, resulting in uneven mixing of the slurry, affecting its product performance.
[0004] The yttrium oxide thermal spraying powder currently produced still has certain defects in porosity, density and service life. In addition, some yttrium oxide thermal spraying powder spray coatings appear pink.
[0005] CN116102050A discloses a method for preparing plasma corrosion resistant thermal spray yttrium oxide powder, which comprises the following steps: subjecting the yttrium oxide raw material to calcination heat treatment, placing the yttrium oxide raw material in an electric arc furnace for melting and refining in batches before the calcination heat treatment, cooling naturally after the melting and refining treatment, and then crushing and selecting the molten and condensed pure yttrium oxide crystals, pulverizing, adding water for modulation, adding auxiliary agents, granulating and drying, calcination heat treatment, and cooling for particle size classification to obtain plasma corrosion resistant thermal spray yttrium oxide. The prepared thermal spray yttrium oxide powder has a high coating density, strong corrosion resistance, and excellent corrosion resistance after spraying, but the preparation process is complicated, the energy consumption is high, the equipment requirements are high, the particle size classification is limited, and it is not environmentally friendly.
[0006] CN103449816A discloses a plasma corrosion resistant granulated yttrium oxide for thermal spraying and a preparation method thereof, wherein nano or ultrafine yttrium oxide powder is prepared into a slurry with deionized water or an organic solution, and then depolymerized and reduced, and then a surfactant activator is added to the slurry for preparation, and then the granulated yttrium oxide for thermal spraying is obtained by thermal expansion ball making and high temperature densification treatment; the granulated yttrium oxide for thermal spraying obtained by adding a surfactant activator to the slurry before thermal expansion ball making has good sphericity, and the granulated yttrium oxide for thermal spraying with high sphericity, good fluidity and high density can be obtained without the need for subsequent spheroidization treatment, thereby satisfying the requirement of good fluidity during thermal spraying, and making the supply of granulated yttrium oxide for thermal spraying more stable. However, the preparation process is complicated, such as depolymerization and reduction, addition of surfactant, thermal expansion ball making and high temperature densification, and the addition of surfactant affects the stability of the final product. Summary of the invention
[0007] The technical problem to be solved by the present invention is to overcome the above-mentioned defects of the prior art and provide yttria granulated powder for plasma corrosion resistant thermal spraying, which has controllable size and high yield.
[0008] The invention also provides a method for preparing yttria granulated powder for plasma corrosion resistant thermal spraying, which has low calcination temperature, low energy consumption and small investment.
[0009] The invention also provides plasma corrosion resistant thermal spraying yttria granulated powder for use as a spray coating, which has good density, strong corrosion resistance and long service life.
[0010] The method for preparing the plasma corrosion resistant yttrium oxide granulated powder for thermal spraying of the present invention comprises the following steps:
[0011] (1) Grind and depolymerize yttrium oxide, mix it with deionized water to form a slurry, add a dispersant, and dissolve it;
[0012] (2) Adding a temporary binder and a flux to the slurry dissolved in step (1) and stirring;
[0013] (3) drying and granulating the slurry obtained after stirring in step (2) by a spray granulation process to obtain spherical yttrium oxide powder;
[0014] (4) Calcine the spherical yttrium oxide powder at a calcination temperature of 1400-1500° C. for a holding time of 4-6 hours, and screen the particle size after cooling to obtain yttrium oxide granulated powder for plasma corrosion resistant thermal spraying.
[0015] The purity of yttrium oxide in step (1) is ≥99.995wt%, the particle size D50 is 5-7μm, and the specific surface area is 3.0-4.0m 2 / g; after grinding and deagglomerating the yttrium oxide, the particle size D10 is controlled to be 0.5μm-1.0μm, and D90 is controlled to be 2.5μm-3.0μm.
[0016] Step (1) Yttrium oxide is mixed with deionized water to form a slurry, wherein the solid content of the slurry is 50%-70%. The prepared plasma corrosion resistant thermal spraying yttrium oxide granulated powder is tested for fluidity of 7.0 g / sec using a BT-102 metal powder fluidity tester (Hall flowmeter).
[0017] The dispersant in step (1) is a mixture of polyvinyl alcohol, polysaccharide and carboxylic acid preparation, wherein the mass ratio of polyvinyl alcohol, polysaccharide and carboxylic acid preparation is (1:0.3:2)-(1:0.8:4). The polysaccharide is maltodextrin or hydroxyethyl cellulose. The carboxylic acid preparation is polyacrylic acid or sodium polyacrylate.
[0018] The amount of dispersant added in step (1) is 1.0%-1.5% of the mass of yttrium oxide.
[0019] The temporary binder in step (2) is a mixture of polyvinyl alcohol, 2,3-dihydroxysuccinic acid (tartaric acid), and 2-hydroxysuccinic acid (malic acid) in a mass ratio of (2:1:1) to (3:1:1), and the amount added is 1.0-3.0% of the solid content of the slurry; the flux is one or more halides of aluminum, silicon, gadolinium, ytterbium, and yttrium, the particle size D50 of the flux is 0.2-0.5 μm, and the amount added is 1.0-3.0% of the solid content of the slurry.
[0020] The spray granulation process parameters of step (3) are: inlet temperature 250-280°C, outlet temperature 120-130°C, atomizer speed 17000-20000 r / min, slurry flow rate 1.0-1.2 kg / min.
[0021] The particle size range of the prepared plasma corrosion resistant thermal spraying yttria granulated powder is D10 of 20-25 μm, D50 of 32-36 μm, and D59 of 50-55 μm.
[0022] The invention discloses yttria granulated powder for plasma corrosion resistant thermal spraying, which is prepared by the preparation method of yttria granulated powder for plasma corrosion resistant thermal spraying.
[0023] Application of the plasma corrosion resistant thermal spraying yttria granulated powder: using it in semiconductor coating.
[0024] Specifically, the method for preparing the plasma corrosion resistant yttria granulated powder for thermal spraying comprises the following steps:
[0025] (1) Select yttrium oxide raw material with purity ≥99.995wt%, particle size D50 of 5-7μm, and specific surface area of 3.0-4.0m² / g, grind and depolymerize to D10 of 0.5μm-1.0μm and D90 of 2.5μm-3.0μm, mix with deionized water to form a slurry with a solid content of 50%-70%, and add a mixture of polyvinyl alcohol, polysaccharide, and carboxylic acid preparation (mass ratio (1:0.3:2)-(1:0.8:4)) as a dispersant. The amount of dispersant added is 1.0%-1.5% of the mass of yttrium oxide, and it is fully dissolved.
[0026] (2) Add a temporary binder (a mixture of polyvinyl alcohol, 2,3-dihydroxysuccinic acid, and 2-hydroxysuccinic acid in a mass ratio of (2:1:1) to (3:1:1), with an addition amount of 1.0-3.0% of the solid content of the slurry) and a flux (one or more halides of aluminum, silicon, gadolinium, ytterbium, and yttrium, with a particle size D50 of 0.2-0.5 μm, with an addition amount of 1.0-3.0% of the solid content of the slurry) to the above slurry and stir well.
[0027] (3) The slurry obtained in step (2) is granulated by a spray granulation process. The process parameters are set as an inlet temperature of 250-280°C, an outlet temperature of 120-130°C, an atomizer speed of 17000-20000 r / min, and a slurry flow rate of 1.0-1.2 kg / min. After drying and granulation, spherical yttrium oxide powder is obtained.
[0028] (4) The spherical yttrium oxide powder is calcined at 1400-1500°C for 4-6 hours, and after cooling, the particle size is screened to obtain yttrium oxide granulated powder for plasma corrosion resistant thermal spraying, with a particle size range of D10 of 20-25 μm, D50 of 32-36 μm, D90 of 50-55 μm, and a tap density of 1.5-1.7 g / cm³.
[0029] The preparation method of the plasma corrosion resistant thermal spray yttrium oxide granulated powder of the present invention first disperses the raw materials through a specific dispersant polyvinyl alcohol, a polysaccharide, and a specific composition of a carboxylic acid preparation to improve the uniformity and stability of the slurry, laying the foundation for the subsequent granulation process, and then adds a specific temporary binder and a flux to the slurry. The temporary binder helps to form stable spherical particles during the spray granulation process, and the flux can promote particle densification during the subsequent calcination process to improve the corrosion resistance of the product. Then, the spray granulation method is adopted, which has high efficiency and controllability, ensuring that the powder has good sphericity and particle size distribution. Finally, after low-temperature calcination, the particles are further densified and the corrosion resistance is improved.
[0030] The present invention grinds and depolymerizes the yttrium oxide precursor powder, and only needs to add deionized water and a mixed dispersant composed of polyvinyl alcohol, polysaccharide and carboxylic acid preparation. Compared with the process of purchasing anhydrous ethanol, it is more economical and safer. At the same time, because a carboxylic acid liquid organic dispersant is added during the depolymerization process, the problem of pinking of the spray coating is avoided, which helps to improve product performance. The present invention also reduces the calcination temperature of the granulated powder by adding a flux, etc. The calcination temperature is usually around 1600-1700°C, and the calcination temperature of the present invention is 1400-1500°C, which not only significantly saves energy and reduces consumption, but also reduces equipment capital investment; the yttrium oxide granulated powder prepared by the process of the present invention has a high yield rate, good density and fluidity, excellent corrosion resistance, and a long service life.
[0031] Compared with the prior art, the present invention has the following beneficial effects:
[0032] (1) The method for preparing the plasma corrosion resistant yttria granulated powder for thermal spraying of the present invention is simple to operate, consumes less energy for low-temperature calcination, and has strong preparation stability.
[0033] (2) The plasma corrosion resistant yttria granulated powder for thermal spraying prepared by the method of the present invention has a wide operating range of particle size, a high yield rate, and good density and fluidity.
[0034] (3) The yttrium oxide granulated powder prepared by the method of the present invention is used in semiconductor coatings and has strong corrosion resistance and adhesion. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 This is a scanning electron microscope image of the plasma corrosion resistant thermal spraying yttria granulated powder prepared in Example 1 at 50 μm.
[0036] Figure 2 This is a 50μm scanning electron microscope image of the plasma corrosion resistant thermal spraying yttria granulated powder prepared in Example 1 after it was prepared into a coating.
[0037] Figure 3 This is a 50 μm scanning electron microscope image of the purchased yttrium oxide granules prepared into a coating in Comparative Example 1. DETAILED DESCRIPTION
[0038] The present invention will be further described below in conjunction with specific embodiments.
[0039] The raw materials and additives used in the following examples and comparative examples are all normal commercially available products.
[0040] The yttrium oxide raw material used in the following examples has a purity of ≥99.995wt%, a particle size D50 of 5-7μm, and a specific surface area of 3.0-4.0m² / g.
[0041] The particle size D50 of the flux used (one or more of the halides of aluminum, silicon, gadolinium, ytterbium and yttrium) is 0.2-0.5 μm.
[0042] The content, purity, etc. described in the present invention all refer to quality.
[0043] Example 1
[0044] The method for preparing the plasma corrosion resistant yttria granulated powder for thermal spraying comprises the following steps:
[0045] (1) After grinding and depolymerizing the yttrium oxide raw material to a D10 of 0.5 μm-1.0 μm and a D90 of 2.5 μm-3.0 μm, the raw material is mixed with deionized water to form a slurry with a solid content of 60%, and a mixture of polyvinyl alcohol, maltodextrin, and polyacrylic acid in a mass ratio of 1:0.5:3 is added as a dispersant. The amount of the dispersant added is 1.2% of the mass of the yttrium oxide and the yttrium oxide is fully dissolved.
[0046] (2) Add a temporary binder (a mixture of polyvinyl alcohol, 2,3-dihydroxysuccinic acid, and 2-hydroxysuccinic acid in a mass ratio of 2.5:1:1, with an addition amount of 2.0% of the solid content of the slurry) and silicon chloride (an addition amount of 2.0% of the solid content of the slurry) to the above slurry and stir evenly.
[0047] (3) The slurry obtained in step (2) was granulated by a spray granulation process. The process parameters were set as an inlet temperature of 260°C, an outlet temperature of 125°C, an atomizer speed of 18000 r / min, and a slurry flow rate of 1.1 kg / min. After drying and granulation, spherical yttrium oxide powder was obtained.
[0048] (4) The spherical yttrium oxide powder is calcined at 1450° C. for 5 h, and then the particle size is screened after cooling to obtain yttrium oxide granulated powder for plasma corrosion resistant thermal spraying.
[0049] Example 2
[0050] The method for preparing the plasma corrosion resistant yttrium oxide granulated powder for thermal spraying comprises the following steps:
[0051] (1) After grinding and depolymerizing the yttrium oxide raw material to a D10 of 0.5 μm-1.0 μm and a D90 of 2.5 μm-3.0 μm, the raw material is mixed with deionized water to form a slurry with a solid content of 50%, and a mixture of polyvinyl alcohol, maltodextrin, and polyacrylic acid in a mass ratio of 1:0.3:2 is added as a dispersant. The amount of the dispersant added is 1.5% of the mass of the yttrium oxide and the yttrium oxide is fully dissolved.
[0052] (2) Add a temporary binder (a mixture of polyvinyl alcohol, 2,3-dihydroxysuccinic acid, and 2-hydroxysuccinic acid in a mass ratio of 2:1:1, with an addition amount of 3.0% of the solid content of the slurry) and yttrium chloride (an addition amount of 3.0% of the solid content of the slurry) to the above slurry and stir evenly.
[0053] (3) The slurry obtained in step (2) was granulated by a spray granulation process. The process parameters were set as an inlet temperature of 280°C, an outlet temperature of 130°C, an atomizer speed of 17000 r / min, and a slurry flow rate of 1.0 kg / min. Spherical yttrium oxide powder was obtained after drying and granulation.
[0054] (4) The spherical yttrium oxide powder is calcined at 1400°C for 6 hours, and after cooling, the particle size is screened to obtain yttrium oxide granulated powder for plasma corrosion resistant thermal spraying.
[0055] Example 3
[0056] The method for preparing the plasma corrosion resistant yttrium oxide granulated powder for thermal spraying comprises the following steps:
[0057] (1) After grinding and depolymerizing the yttrium oxide raw material to a D10 of 0.5 μm-1.0 μm and a D90 of 2.5 μm-3.0 μm, the raw material is mixed with deionized water to form a slurry with a solid content of 50%, and a mixture of polyvinyl alcohol, hydroxyethyl cellulose, and sodium polyacrylate in a mass ratio of 1:0.8:4 is added as a dispersant. The amount of the dispersant added is 1.0% of the mass of the yttrium oxide and the yttrium oxide is fully dissolved.
[0058] (2) Add a temporary binder (a mixture of polyvinyl alcohol, 2,3-dihydroxysuccinic acid, and 2-hydroxysuccinic acid in a mass ratio of 3:1:1, with an addition amount of 1.0% of the solid content of the slurry) and aluminum chloride (an addition amount of 1.0% of the solid content of the slurry) to the above slurry and stir well.
[0059] (3) The slurry obtained in step (2) was granulated by a spray granulation process. The process parameters were set as an inlet temperature of 250°C, an outlet temperature of 120°C, an atomizer speed of 20,000 r / min, and a slurry flow rate of 1.2 kg / min. Spherical yttrium oxide powder was obtained after drying and granulation.
[0060] (4) The spherical yttrium oxide powder is calcined at 1500° C. for 4 h, and after cooling, the particle size is screened to obtain yttrium oxide granulated powder for plasma corrosion resistant thermal spraying.
[0061] Example 4
[0062] The method for preparing the plasma corrosion resistant yttrium oxide granulated powder for thermal spraying comprises the following steps:
[0063] (1) After grinding and depolymerizing the yttrium oxide raw material to a D10 of 0.5 μm-1.0 μm and a D90 of 2.5 μm-3.0 μm, the raw material is mixed with deionized water to form a slurry with a solid content of 60%, and a mixture of polyvinyl alcohol, hydroxyethyl cellulose, and sodium polyacrylate in a mass ratio of 1:0.5:3 is added as a dispersant. The amount of the dispersant added is 1.2% of the mass of the yttrium oxide and the yttrium oxide is fully dissolved.
[0064] (2) Add a temporary binder (a mixture of polyvinyl alcohol, 2,3-dihydroxysuccinic acid, and 2-hydroxysuccinic acid in a mass ratio of 2.5:1:1, with an addition amount of 2.0% of the solid content of the slurry) and ytterbium chloride (an addition amount of 2.0% of the solid content of the slurry) to the above slurry and stir well.
[0065] (3) The slurry obtained in step (2) was granulated by a spray granulation process. The process parameters were set as an inlet temperature of 260°C, an outlet temperature of 125°C, an atomizer speed of 18000 r / min, and a slurry flow rate of 1.1 kg / min. After drying and granulation, spherical yttrium oxide powder was obtained.
[0066] (4) The spherical yttrium oxide powder is calcined at 1450° C. for 5 h, and then the particle size is screened after cooling to obtain yttrium oxide granulated powder for plasma corrosion resistant thermal spraying.
[0067] Comparative Example 1
[0068] This comparative example is the same as Example 1, except that the maltodextrin and polyacrylic acid in the dispersant of step (1) are removed, and the other preparations are the same as those of Example 1.
[0069] Comparative Example 2
[0070] This comparative example is the same as Example 1, except that the 2,3-dihydroxysuccinic acid and 2-hydroxysuccinic acid in the temporary binder of step (2) are removed, and the other preparation is the same as Example 1.
[0071] Comparative Example 3
[0072] This comparative example is the same as Example 1, except that the polyvinyl alcohol in the temporary adhesive in step (2) is removed, and the other preparations are the same as those in Example 1.
[0073] Comparative Example 4
[0074] This comparative example is the same as Example 1, except that the flux silicon chloride in step (2) is removed, and the other preparations are the same as Example 1.
[0075] Comparative Example 5
[0076] Yttria granulated powder imported from a Japanese company was purchased. The parameters of the granulated powder are shown in Table 1.
[0077] The yttrium oxide granulated powder prepared in the above examples and comparative examples was subjected to performance testing, and the test results are shown in Table 1.
[0078] Table 1 Yttrium oxide granulated powder test results
[0079]
[0080] The granulated powder prepared in the above examples and comparative examples was sprayed by atmospheric plasma APS according to the coating method, with a power of 40kW and a SG-100 plasma gun for spraying, and the spraying thickness was set to 150 μm. The coating was analyzed and tested, and the test results are shown in Table 2. The surface roughness was tested by the stylus method.
[0081] Table 2 Coating test results
[0082]
[0083] It can be seen from Tables 1 and 2 above that the yttrium oxide granulated powder prepared by the present invention at a lower calcination temperature has significant improvements in surface roughness and porosity after being applied to the coating, and also has improvements in dielectric constant, adhesion and hardness, and the prepared product is white.
Claims
1. A method for preparing yttrium oxide granulated powder for plasma corrosion resistant thermal spraying, characterized in that: The following steps are involved: (1) Grind and depolymerize yttrium oxide, and then mix it with deionized water to form a slurry with a solid content of 50%-70%. Add a dispersant at a concentration of 1.0%-1.5% of the mass of yttrium oxide and dissolve it; The dispersant is a mixture of polyvinyl alcohol, polysaccharide and carboxylic acid preparation in a mass ratio of (1:0.3:2)-(1:0.8:4); the polysaccharide is maltodextrin or hydroxyethyl cellulose; the carboxylic acid preparation is polyacrylic acid or sodium polyacrylate; (2) Adding a temporary binder and a flux to the slurry dissolved in step (1) and stirring; The amount of temporary binder added is 1.0-3.0% of the solid content of the slurry; the particle size D50 of the flux is 0.2-0.5μm, and the amount of addition is 1.0-3.0% of the solid content of the slurry; The flux is one or more halides of aluminum, silicon, gadolinium, ytterbium, and yttrium; the temporary binder is a mixture of polyvinyl alcohol, 2,3-dihydroxysuccinic acid, and 2-hydroxysuccinic acid in a mass ratio of (2:1:1) to (3:1:1); (3) drying and granulating the slurry obtained after stirring in step (2) by a spray granulation process to obtain spherical yttrium oxide powder; (4) Calcine the spherical yttrium oxide powder at a calcination temperature of 1400-1500° C. for a holding time of 4-6 hours, and screen the particle size after cooling to obtain yttrium oxide granulated powder for plasma corrosion resistant thermal spraying.
2. The method for preparing the plasma corrosion resistant yttrium oxide granulated powder for thermal spraying according to claim 1, characterized in that: The purity of yttrium oxide in step (1) is ≥99.995wt%, the particle size D50 is 5-7μm, and the specific surface area is 3.0-4.0m 2 / g; after grinding and deagglomerating the yttrium oxide, the particle size D10 is controlled to be 0.5μm-1.0μm, and D90 is controlled to be 2.5μm-3.0μm.
3. The method for preparing the plasma corrosion resistant yttrium oxide granulated powder for thermal spraying according to claim 1, characterized in that: The spray granulation process parameters of step (3) are: inlet temperature 250-280°C, outlet temperature 120-130°C, atomizer speed 17000-20000 r / min, slurry flow rate 1.0-1.2 kg / min.
4. The method for preparing the plasma corrosion resistant yttrium oxide granulated powder for thermal spraying according to claim 1, characterized in that: The particle size range of the prepared plasma corrosion resistant thermal spraying yttria granulated powder is D10 of 20-25 μm, D50 of 32-36 μm, and D59 of 50-55 μm.
5. A plasma corrosion resistant yttria granulated powder for thermal spraying, characterized in that: The yttrium oxide granulated powder for plasma corrosion resistant thermal spraying is prepared by the preparation method of any one of claims 1 to 4.
6. An application of the plasma corrosion resistant thermal spraying yttria granulated powder according to claim 5, characterized in that: It is used in semiconductor coatings.
Citation Information
Patent Citations
Plasma-etching-resistant granulated yttrium oxide for hot spraying and preparation method thereof
CN103449816A
Preparation method of plasma corrosion resistant thermal spraying yttrium oxide powder
CN116102050A
Preparation method of granulated yttrium oxide in favor of controlling color after spraying, capable of resisting plasma corrosion, and for thermal spraying
CN108408754A
Material for spray coating, and member with sprayed coating
CN110983227A
Preparation method of nanoscale yttrium oxide powder
CN112209420A