Rare earth doped zinc oxide functional polyamide polymer and preparation method and application thereof
By synergistic doping of rare earth ions and zinc-based antibacterial agents, a white rare earth-doped zinc oxide functional polyamide polymer was prepared, which solved the problems of easy oxidation and discoloration and insufficient antibacterial ability of existing antibacterial materials, and achieved efficient and stable antibacterial performance and wide application.
Patent Information
- Application Number
- CN202411179005.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-08-27
AI Technical Summary
Existing nano-silver and copper-based antibacterial agents are expensive and prone to oxidation and discoloration, while nano-zinc oxide-based antibacterial agents have weak antibacterial ability and cannot meet the needs of a wide range of applications. Furthermore, traditional antibacterial materials are prone to bacterial growth in humid environments.
Rare earth-doped zinc oxide functional polyamide polymers are prepared by synergistic doping of rare earth ions and zinc-based antibacterial agents through a three-stage continuous polymerization process. The rare earth ions and zinc compounds work together to form a white antibacterial material, which can be applied to antibacterial fibers, films and engineering plastics.
It achieves efficient and stable antibacterial properties, the material does not leach and has good thermal stability, is suitable for a variety of downstream applications, is not limited by color, and has long-lasting antibacterial function.
Smart Images

Figure CN118702911B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polymer materials, and in particular relates to a rare earth doped zinc oxide functional polyamide polymer and a preparation method and application thereof. Background Art
[0002] Polyamide has excellent properties such as light weight, high strength, wear resistance, resistance to weak acids and alkalis and some organic solvents, and easy molding and processing. It is widely used in the fields of fibers, engineering plastics and films.
[0003] With the improvement of living standards and the development of society, people have an increasing demand for products with antibacterial functions. For example, under the immersion of sweat, skin oil or in a humid and hot environment, fibers and fabrics have a large specific surface area and a porous structure, which can easily attach and breed bacteria, causing the fiber fabrics to mold, discolor, and deform, etc. Long-term contact with the human body can harm health. Plastic products and film products, which are indispensable in our daily lives, come into contact with food, oil, the environment, and bacteria carried by the human body, and are prone to attaching and breeding bacteria, causing cross-infection of bacteria, and then spreading diseases. Therefore, giving polyamide antibacterial functions has received increasing attention from researchers.
[0004] Inorganic heavy metal antimicrobial agents such as nanosilver, copper, and nanozinc oxide have significant antibacterial properties. Among them, nanosilver has the strongest antibacterial ability, but silver ions are expensive and easily oxidized or reduced to black, which limits their scope of use; copper antimicrobial agents themselves are colored and easily oxidized and discolored during back-end application, which narrows their scope of use; nanozinc oxide has weaker antibacterial ability than nanosilver and copper antimicrobial agents.
[0005] Rare earth ions have good antibacterial properties and are non-toxic, safe and environmentally friendly. Rare earth ions can interact with bacterial cell walls, cell membranes, and DNA, enzymes, proteins, etc. in cells, thereby changing cell structures, hindering / interfering with the normal physiological activities of bacteria, inhibiting bacterial growth and reproduction, and ultimately causing bacterial death.
[0006] Therefore, if rare earth ions are doped into inorganic heavy metal antibacterial materials, materials with better antibacterial effects will be obtained. Summary of the invention
[0007] In view of this, the present invention aims to propose a rare earth doped zinc oxide functional polyamide polymer and its preparation method and application. The polymer uses rare earth ions and zinc antibacterial agents to synergistically resist bacteria, has good antibacterial properties, does not dissolve antibacterial components, has good thermal stability, and has stable and lasting antibacterial function. The polymer is white, and downstream applications are not limited by color, and can be applied to antibacterial fibers, films, engineering plastics and other fields.
[0008] To achieve the above object, the technical solution of the present invention is achieved as follows:
[0009] A method for preparing a rare earth doped zinc oxide functional polyamide polymer, the method comprising the following steps:
[0010] 1) Preparation of rare earth doped zinc oxide nanomaterials
[0011] The zinc compound is dissolved in deionized water, and then a rare earth metal compound is added and stirred evenly, and then an alkyl silane compound is added, and stirred at 50-80° C. for 3-7 hours, and then an alkaline solution is added and stirred for 3-8 hours; after the reaction is completed, the solid material is filtered and dried and calcined in a muffle furnace, and then taken out after natural cooling to obtain a rare earth doped zinc oxide nanomaterial;
[0012] 2) Preparation of water-based nanofunctional slurry
[0013] Weigh the rare earth doped zinc oxide nanomaterial and deionized water by mass, mix them evenly, then add a dispersant, grind them evenly in a sand mill, and obtain a stable and non-settling water system nano functional slurry;
[0014] 3) Preparation of rare earth doped zinc oxide functional polyamide polymer
[0015] The invention adopts aqueous solution of caprolactam, nylon diamine diacid salt, additives and water-based nano-functional slurry as raw materials, adopts three-stage continuous polymerization process of prepolymerization, front polymerization and post-polymerization, and then is prepared through pelletizing, extraction and drying; wherein the water-based nano-functional slurry is added after the prepolymerization reaction.
[0016] In the prepolymerization stage, caprolactam is rapidly hydrolyzed and ring-opened to form aminoacetic acid under high temperature and high pressure, and the caprolactam molecules are connected to the aminoacetic acid molecular chain one by one to form short-chain polyamide molecules of a certain length. At the same time, nylon diamine diacid undergoes dehydration and polycondensation to form short-chain molecules.
[0017] In the pre-polymerization stage, short-chain molecules form long-chain molecules through condensation polymerization, accompanied by addition reactions with lower reaction rates. Rare earth-doped zinc oxide nanomaterials are grafted onto polyamide molecular chains through addition and condensation polymerization reactions.
[0018] In the post-polymerization stage, chain exchange reactions are dominant, and eventually the molecular weight of the polymer reaches equilibrium and the molecular weight distribution becomes narrower.
[0019] Furthermore, in step 1), by weight, the zinc compound is 20-60 parts, deionized water is 40-100 parts, the rare earth metal compound is 20-70 parts, the alkylsilane compound is 10-50 parts, and the alkaline solution is 5-40 parts.
[0020] Furthermore, the mass ratio of the zinc compound to the rare earth metal compound is 1:1.1-2;
[0021] The zinc compound is one of zinc nitrate, zinc sulfate or zinc acetate;
[0022] The alkaline solution is one of ammonia water, urea, ammonium carbonate or sodium hydroxide.
[0023] Furthermore, the rare earth metal compound is a mixture of lanthanum chloride heptahydrate, gadolinium nitrate hexahydrate, and cerium chloride heptahydrate, and the mass ratio of the three substances is (2-5):2:1.
[0024] Furthermore, in step 1), the solid drying temperature is 50-100° C., the muffle furnace calcination temperature is 800-1200° C., and the calcination time is 2-6 hours.
[0025] Further, in step 2), the mass ratio of rare earth doped zinc oxide nanomaterial: deionized water: dispersant is (25-40): (57-74.5): (0.5-3);
[0026] The dispersant is one or more of hexadecyltrimethylammonium bromide, polyvinylpyrrolidone, modified styrene maleic acid copolymer solution, modified polymer block copolymer, and high molecular weight silane copolymer containing pigment-affinity groups;
[0027] The particle size of the water-based nano-functional slurry is 100-350nm.
[0028] Further, the specific steps of step 3) are:
[0029] A. uniformly mixing caprolactam, an aqueous solution of nylon diamine diacid salt and an additive to obtain a first mixture, and performing a prepolymerization reaction under high temperature and pressure to obtain a polyamide oligomer;
[0030] B. After the prepolymerization reaction, the polyamide oligomer obtained in step A is mixed with the aqueous nano-functional slurry to obtain a second mixture;
[0031] C. The second mixture obtained in step B is subjected to pre-polymerization reaction and post-polymerization reaction to form a rare earth doped zinc oxide functional polyamide polymer.
[0032] Further, the nylon diamine diacid salt is one of nylon 66 salt, nylon 610 salt, nylon 612 salt, nylon 56 salt, nylon 510 salt, and nylon 512 salt;
[0033] The concentration of the nylon diamine diacid aqueous solution is 50-80wt%;
[0034] Nylon diamine diacid salt accounts for 5-25wt% of the total feed;
[0035] Rare earth doped zinc oxide nanomaterials account for 0.5-5wt% of the total feed;
[0036] The additive is one or more of acetic acid, benzoic acid, purified terephthalic acid and hexamethylenediamine. The amount of the additive is 0.05-0.3% of the mass of caprolactam. Adding the additive can prevent the further growth of the macromolecular chain and stabilize the molecular weight of the polymer.
[0037] Further, the prepolymerization pressure is controlled at 10-40 bar, the prepolymerization temperature is controlled at 240-270° C., and the residence time is 1-4 h;
[0038] The prepolymerization reaction pressure is controlled at 2-4 bar, the prepolymerization temperature is controlled at 255-275° C., and the residence time is 1-4 hours;
[0039] The post-polymerization reaction pressure is controlled at 10-30 mbar, the post-polymerization temperature is controlled at 240-250° C., and the residence time is 8-12 hours.
[0040] The present invention also provides a rare earth-doped zinc oxide functional polyamide polymer prepared by the above-mentioned preparation method. The polymer is white and its downstream applications are not restricted by color, thus reducing the difficulty and cost of color matching.
[0041] The present invention also provides the application of the rare earth doped zinc oxide functional polyamide polymer as described above in antibacterial fibers, films, and engineering plastics. The rare earth doped zinc oxide functional polyamide polymer is pelletized, extracted, and dried to obtain rare earth doped zinc oxide functional polyamide slices. The slices have an extractable content of 0.3-0.5%, a water content of 200-400 ppm, and a relative viscosity of 2.4-4.0. The slices have a wide relative viscosity range, a wide application field, and strong practicality.
[0042] Compared with the prior art, the rare earth doped zinc oxide functional polyamide polymer and its preparation method and application described in the present invention have the following advantages:
[0043] (1) The rare earth-doped zinc oxide functional polyamide polymer of the present invention has synergistic antibacterial properties through rare earth ions and zinc compounds, and the antibacterial properties can be significantly improved compared with the use of rare earth ions or zinc oxide alone.
[0044] (2) The present invention adopts a three-stage continuous polymerization process and adds a water-based nano-functional slurry after the prepolymerization reaction, thereby reducing the influence of rare earth-doped zinc oxide nanomaterials on the polymer molecular chain, so that the obtained polymer has a higher melt viscosity and good antibacterial properties.
[0045] (3) Rare earth doped zinc oxide functional polyamide polymer was prepared by in situ polymerization method, so that rare earth doped zinc oxide nanomaterials were evenly distributed in polyamide, the nanomaterials did not undergo obvious agglomeration, the polymer had good uniformity, and excellent antibacterial properties.
[0046] (4) The rare earth doped zinc oxide functional polyamide polymer prepared by the present invention is white, and its downstream applications are not limited by color. It can be applied to the fields of antibacterial fibers, engineering plastics, films, etc. Its antibacterial components do not dissolve, have good thermal stability, and have stable and long-lasting antibacterial functions. BRIEF DESCRIPTION OF THE DRAWINGS
[0047] The accompanying drawings constituting a part of the present invention are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the accompanying drawings:
[0048] Figure 1 This is a flow chart for the preparation of rare earth doped zinc oxide functional polyamide polymers. DETAILED DESCRIPTION
[0049] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features in the embodiments may be combined with each other.
[0050] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0051] Example 1
[0052] A method for preparing a rare earth doped zinc oxide functional polyamide polymer, the method comprising the following steps:
[0053] 1) Preparation of rare earth doped zinc oxide nanomaterials:
[0054] Weigh 25 parts of zinc nitrate by mass and put it into a round-bottom flask, add 50 parts of deionized water and stir to dissolve; then add 30 parts of rare earth metal compounds (15 parts of lanthanum chloride heptahydrate, 10 parts of gadolinium nitrate hexahydrate, and 5 parts of cerium chloride heptahydrate) and stir evenly, then add 25 parts of polytetramethylsilane and continue stirring at 50°C for 4 hours; then add 15 parts of ammonium carbonate to the solution and continue stirring for 4 hours; after the reaction is completed, filter the suspension in the flask, dry the obtained solid material at 70°C, and then put it into a muffle furnace at 1000°C and calcine it for 3 hours, and then take it out and grind it after natural cooling to obtain rare earth doped zinc oxide nanomaterials.
[0055] 2) Preparation of water-based nano-functional slurry:
[0056] Weigh 31 parts of the above rare earth-doped zinc oxide nanomaterial and 67.5 parts of deionized water by mass and mix them evenly in a sand mill, then add 1.5 parts of polyvinyl pyrrolidone and perform multi-stage grinding and dispersion in a sand mill to obtain a water-based nano-functional slurry with a slurry particle size of 179 nm.
[0057] (3) Preparation of rare earth doped zinc oxide functional polyamide polymer:
[0058] A. 90 kg of caprolactam, 10 kg of 60 wt% nylon 66 saline solution, and 0.1 kg of benzoic acid are uniformly mixed by a static mixer to obtain a first mixture, and a prepolymerization reaction is performed under high temperature and pressure to obtain a polyamide oligomer;
[0059] B. mixing the polyamide oligomer with 3.37 kg of water-based nano-functional slurry to obtain a second mixture, wherein the rare earth-doped zinc oxide nanomaterial accounts for 1 wt % of the total feed amount;
[0060] C. subjecting the second mixture to pre-polymerization reaction and post-polymerization reaction to form a rare earth-doped zinc oxide functional polyamide polymer.
[0061] The polymer obtained in Example 1 was prepared into fibers:
[0062] 1) pelletizing, extracting and drying the rare earth doped zinc oxide functional polyamide polymer melt obtained above to obtain rare earth doped zinc oxide functional polyamide slices;
[0063] 2) Add the dried rare earth doped zinc oxide functional polyamide slices into a screw extruder, melt and extrude at high temperature of the screw to form a melt, which is metered by a metering pump and enters the channel of the spinneret, extruded through the spinneret holes, cooled, oiled, stretched, and wound to obtain rare earth doped zinc oxide functional polyamide fibers. The heating temperature of each zone of the screw extruder is 255-265°C.
[0064] Example 2
[0065] 1) Preparation of rare earth doped zinc oxide nanomaterials:
[0066] Weigh 35 parts of zinc acetate by mass and put them into a round-bottom flask, add 60 parts of deionized water in the flask and stir to dissolve; then add 50 parts of rare earth metal compounds (20 parts of lanthanum chloride heptahydrate, 20 parts of gadolinium nitrate hexahydrate, and 10 parts of cerium chloride heptahydrate) and stir evenly, then add 30 parts of polytetramethylsilane and continue stirring at 60°C for 5 hours; then add 25 parts of sodium hydroxide to the solution and continue stirring for 5 hours; after the reaction is completed, filter the suspension in the flask, dry the obtained solid material at 70°C, and then put it into a muffle furnace at 1100°C and calcine it for 3 hours, and then take it out and grind it after natural cooling to obtain rare earth doped zinc oxide nanomaterials.
[0067] 2) Preparation of water-based nano-functional slurry:
[0068] Weigh 35 parts of the above rare earth-doped zinc oxide nanomaterial and 63 parts of deionized water by mass and mix them evenly in a sand mill, then add 2 parts of hexadecyltrimethylammonium bromide and perform multi-stage grinding and dispersion in a sand mill to obtain a water-based nano-functional slurry with a slurry particle size of 190 nm.
[0069] (3) Preparation of rare earth doped zinc oxide functional polyamide polymer:
[0070] A. 85 kg of caprolactam, 15 kg of 71 wt% nylon 510 saline solution, and 0.2 kg of purified terephthalic acid were uniformly mixed by a static mixer to obtain a first mixture, and a prepolymerization reaction was performed under high temperature and pressure to obtain a polyamide oligomer;
[0071] B. mixing the polyamide oligomer with 5.7 kg of water-based nano-functional slurry to obtain a second mixture, wherein the rare earth-doped zinc oxide nanomaterial accounts for 1.9 wt % of the total feed amount;
[0072] C. subjecting the second mixture to pre-polymerization reaction and post-polymerization reaction to form a rare earth-doped zinc oxide functional polyamide polymer.
[0073] The polymer obtained in Example 2 is prepared into plastic:
[0074] 1) pelletizing, extracting and drying the rare earth doped zinc oxide functional polyamide polymer melt obtained above to obtain rare earth doped zinc oxide functional polyamide slices;
[0075] 2) Melting and injection molding the dried rare earth doped zinc oxide functional polyamide slices to obtain rare earth doped zinc oxide functional polyamide plastics.
[0076] Example 3
[0077] 1) Preparation of rare earth doped zinc oxide nanomaterials:
[0078] Weigh 45 parts of zinc sulfate by mass and put them into a round-bottom flask, add 70 parts of deionized water in the flask and stir to dissolve; then add 64 parts of rare earth metal compounds (40 parts of lanthanum chloride heptahydrate, 16 parts of gadolinium nitrate hexahydrate, and 8 parts of cerium chloride heptahydrate) and stir evenly, then add 35 parts of polytetramethylsilane and continue stirring at 60°C for 5 hours; then add 30 parts of urea to the solution and continue stirring for 5 hours; after the reaction is completed, filter the suspension in the flask, dry the obtained solid material at 80°C, then put it into a muffle furnace at 1200°C and calcine it for 4 hours, and then take it out and grind it after natural cooling to obtain rare earth doped zinc oxide nanomaterials.
[0079] 2) Preparation of water-based nano-functional slurry:
[0080] Weigh 38 parts of the above rare earth doped zinc oxide nanomaterial powder and 60 parts of deionized water by mass and mix them evenly in a sand mill, then add 2 parts of modified styrene maleic acid copolymer solution, perform multi-stage grinding and disperse evenly in a sand mill to obtain a water-based nano functional slurry with a slurry particle size of 200 nm.
[0081] 3) Preparation of rare earth doped zinc oxide functional polyamide polymer:
[0082] A. 87 kg of caprolactam, 8 kg of 75 wt % nylon 56 salt solution, and 0.25 kg of hexamethylenediamine were mixed uniformly by a static mixer to obtain a first mixture, and a prepolymerization reaction was performed under high temperature and pressure to obtain a polyamide oligomer;
[0083] B. mixing the polyamide oligomer with 8 kg of water-based nano-functional slurry to obtain a second mixture, wherein the rare earth-doped zinc oxide nanomaterial accounts for 2.9 wt % of the total feed amount;
[0084] C. subjecting the second mixture to pre-polymerization reaction and post-polymerization reaction to form a rare earth-doped zinc oxide functional polyamide polymer.
[0085] The polymer obtained in Example 3 was prepared into a film
[0086] 1) pelletizing, extracting and drying the rare earth doped zinc oxide functional polyamide polymer melt obtained above to obtain rare earth doped zinc oxide functional polyamide slices;
[0087] 2) The dried rare earth doped zinc oxide functional polyamide slices are melt extruded at a temperature of 250°C. The melt flows through a filter, a metering pump, a static mixer, and a die head to a cooling drum surface at 30°C. Under the action of the electrostatic film attachment device, the formation of crystals is minimized to avoid the generation of larger crystal nuclei, and a sheet with good thickness is made. The sheet is longitudinally stretched at a temperature of 50°C, and the longitudinal stretching multiple is 2.7. After stretching, the film is cooled at a temperature of about 30°C and then enters a transverse stretching machine. After passing through a preheating zone at 70°C and at a slightly higher temperature, it is stretched 2.7 times, heat-set at 220°C, and finally naturally cooled to make a nylon film.
[0088] Comparative Example 1: Only zinc compounds are added
[0089] (1) Preparation of aqueous zinc oxide nano-functional slurry: 31 parts of zinc oxide nano-material and 67.5 parts of deionized water were weighed and mixed evenly in a sand mill. Then 1.5 parts of polyvinyl pyrrolidone were added and the mixture was evenly dispersed by multi-stage grinding in a sand mill to obtain an aqueous zinc oxide nano-functional slurry with a particle size of 210 nm.
[0090] (2) The preparation of zinc oxide functional polyamide polymer and fiber is the same as in Example 1.
[0091] Comparative Example 2: Only rare earth is added
[0092] (1) Preparation of rare earth nanomaterials:
[0093] The reaction raw materials do not contain 25 parts of zinc nitrate, and the rest are the same as in Example 1.
[0094] (2) The preparation of functional polyamide polymer and fiber is the same as in Example 1.
[0095] Comparative Example 3
[0096] The steps of adding the water-based nano-functional slurry are different from those in Example 3.
[0097] 8 kg of water-based nano-functional slurry was added to the first mixture before the prepolymerization reaction, and no more was added after the prepolymerization reaction. The rest was the same as in Example 3.
[0098] Comparative Example 4
[0099] 1) Preparation of rare earth doped zinc oxide nanomaterials:
[0100] Weigh 60 parts of zinc acetate by mass and put them into a round-bottom flask, add 60 parts of deionized water in the flask and stir to dissolve; then add 50 parts of rare earth metal compounds (20 parts of lanthanum chloride heptahydrate, 20 parts of gadolinium nitrate hexahydrate, and 10 parts of cerium chloride heptahydrate) and stir evenly, then add 30 parts of polytetramethylsilane and continue stirring at 60°C for 5 hours; then add 25 parts of sodium hydroxide to the solution and continue stirring for 5 hours; after the reaction is completed, filter the suspension in the flask, dry the obtained solid material at 70°C, then put it into a muffle furnace at 1100°C and calcine it for 3 hours, and then take it out and grind it after natural cooling to obtain rare earth doped zinc oxide nanomaterials.
[0101] 2) Other details are the same as in Example 2.
[0102] Comparative Example 5
[0103] 1) Preparation of rare earth doped zinc oxide nanomaterials:
[0104] Weigh 35 parts of zinc acetate by mass and put them into a round-bottom flask, add 60 parts of deionized water in the flask and stir to dissolve; then add 50 parts of rare earth metal compounds (25 parts of lanthanum chloride heptahydrate and 25 parts of gadolinium nitrate hexahydrate) and stir evenly, then add 30 parts of polytetramethylsilane and continue stirring at 60°C for 5 hours; then add 25 parts of sodium hydroxide to the solution and continue stirring for 5 hours; after the reaction is completed, filter the suspension in the flask, dry the obtained solid material at 70°C, then put it into a muffle furnace at 1100°C and calcine it for 3 hours, and then take it out and grind it after natural cooling to obtain rare earth doped zinc oxide nanomaterials.
[0105] 2) Other details are the same as in Example 2.
[0106] Comparative Example 6
[0107] 1) Preparation of rare earth doped zinc oxide nanomaterials:
[0108] Weigh 35 parts of zinc acetate by mass and put them into a round-bottom flask, add 60 parts of deionized water in the flask and stir to dissolve; then add 50 parts of rare earth metal compounds (33.3 parts of lanthanum chloride heptahydrate and 16.7 parts of cerium chloride heptahydrate) and stir evenly, then add 30 parts of polytetramethylsilane and continue stirring at 60°C for 5 hours; then add 25 parts of sodium hydroxide to the solution and continue stirring for 5 hours; after the reaction is completed, filter the suspension in the flask, dry the obtained solid material at 70°C, then put it into a muffle furnace at 1100°C and calcine it for 3 hours, and then take it out and grind it after natural cooling to obtain rare earth doped zinc oxide nanomaterials.
[0109] 2) Other details are the same as in Example 2.
[0110] Comparative Example 7
[0111] 1) Preparation of rare earth doped zinc oxide nanomaterials:
[0112] Weigh 35 parts of zinc acetate by mass and put them into a round-bottom flask, add 60 parts of deionized water in the flask and stir to dissolve; then add 50 parts of rare earth metal compounds (33.3 parts of gadolinium nitrate hexahydrate and 16.7 parts of cerium chloride heptahydrate) and stir evenly, then add 30 parts of polytetramethylsilane and continue stirring at 60°C for 5 hours; then add 25 parts of sodium hydroxide to the solution and continue stirring for 5 hours; after the reaction is completed, filter the suspension in the flask, dry the obtained solid material at 70°C, then put it into a muffle furnace at 1100°C and calcine it for 3 hours, and then take it out and grind it after natural cooling to obtain rare earth doped zinc oxide nanomaterials.
[0113] 2) Other details are the same as in Example 2.
[0114] Comparative Example 8
[0115] 1) Preparation of rare earth doped zinc oxide nanomaterials:
[0116] Weigh 35 parts of zinc acetate by mass and put them into a round-bottom flask, add 60 parts of deionized water in the flask and stir to dissolve; then add 50 parts of rare earth metal compounds (10 parts of lanthanum chloride heptahydrate, 10 parts of gadolinium nitrate hexahydrate, and 30 parts of cerium chloride heptahydrate) and stir evenly, then add 30 parts of polytetramethylsilane and continue stirring at 60°C for 5 hours; then add 25 parts of sodium hydroxide to the solution and continue stirring for 5 hours; after the reaction is completed, filter the suspension in the flask, dry the obtained solid material at 70°C, then put it into a muffle furnace at 1100°C and calcine it for 3 hours, and then take it out and grind it after natural cooling to obtain rare earth doped zinc oxide nanomaterials.
[0117] 2) Other details are the same as in Example 2.
[0118] Comparative Example 9
[0119] The polyamide oligomer is mixed with 29 kg of water-based nano-functional slurry to obtain a second mixture, in which the rare earth-doped zinc oxide nanomaterial accounts for 7 wt % of the total feed amount.
[0120] The rest is the same as in Example 1.
[0121] Comparative Example 10
[0122] 2) Preparation of water-based nano-functional slurry:
[0123] Weigh 31 parts of the above rare earth-doped zinc oxide nanomaterial and 67.5 parts of deionized water by mass and mix them evenly in a sand mill, then add 1.5 parts of polyvinyl pyrrolidone and perform multi-stage grinding and dispersion in a sand mill to obtain a water-based nano-functional slurry with a slurry particle size of 820 nm.
[0124] The rest is the same as in Example 1.
[0125] When the prepared slices were spun, it was found that the pressure of the components was unstable during the spinning process, and there were many floating and broken filaments, and the spinnability was poor.
[0126] Test Case
[0127] The polymerization processes and slicing indicators of Examples 1-3 and Comparative Examples 1-10 are shown in the table below.
[0128] Table 1 Example polymerization process and slicing index
[0129]
[0130] Table 2 Comparative polymerization process and slicing index
[0131]
[0132] Table 3 Antimicrobial performance testing of polymer downstream applications
[0133]
[0134] From the data in Tables 1-3, it can be seen that the rare earth-doped zinc oxide functional polyamide polymer prepared by the present invention has a strong bactericidal effect on Gram-positive bacteria (Staphylococcus aureus), Gram-negative bacteria (Escherichia coli), and fungi (Candida albicans), and the process is highly controllable.
[0135] From the data in Table 3, by comparing Example 1, Comparative Example 1 and Comparative Example 2, it can be seen that the antibacterial property of the composite material of rare earth doped zinc oxide functional polyamide fiber prepared by the present invention is better than the antibacterial property of using rare earth ions or zinc oxide alone, and the antibacterial component of the composite material achieves synergistic antibacterial, improves the antibacterial ability of the material itself and saves costs.
[0136] From the data of Table 1-3, Comparative Example 3 and Comparative Example 3, it can be seen that adding water system nano functional slurry before prepolymerization can significantly reduce the relative viscosity and antibacterial rate of polymer slices. Because rare earth doped zinc oxide nano material can be partially hydrolyzed under high temperature and water system, some rare earth ions after hydrolysis can react with aminoacetic acid in the prepolymerization stage, affecting the addition reaction in the prepolymerization stage, changing the molecular chain structure, interrupting the molecular chain growth, and reducing the molecular weight and relative viscosity of the final polymer. At the same time, some rare earth ions participate in the reaction, reducing the antibacterial properties of the polymer. Therefore, the present invention adds water system nano functional slurry after prepolymerization, reduces the influence of rare earth doped zinc oxide nano material on the polymer molecular chain, and makes the obtained polymer have higher melt viscosity and good antibacterial properties.
[0137] It can be seen from the data of Comparative Example 4 and Example 2 that when the mass ratio of the zinc compound and the rare earth metal compound is changed beyond a specified ratio and the zinc compound is more than the rare earth metal compound, the antibacterial property of the product deteriorates.
[0138] It can be seen from the data of Comparative Examples 5-7 and Example 2 that when the composition of the rare earth metal compound is changed, the antibacterial performance of the product deteriorates, indicating that lanthanum chloride heptahydrate, gadolinium nitrate hexahydrate, and cerium chloride heptahydrate are three indispensable substances. The lack of any one of them will lead to the deterioration of the antibacterial performance of the material.
[0139] It can be seen from the data of Comparative Example 8 and Example 2 that when the mass ratio of the three substances in the rare earth metal compound is changed and the ratio exceeds a given range, the antibacterial performance of the product deteriorates, indicating that the mass ratio of the three substances needs to be controlled within a certain range.
[0140] It can be seen from the data of Comparative Example 9 and Example 1 that when the content of rare earth doped zinc oxide nanomaterial is 7wt%, it exceeds a certain ratio range, and the viscosity and antibacterial properties of the polymer are significantly reduced. This indicates that when the content of rare earth doped zinc oxide nanomaterial is too high, part of the nanomaterial agglomerates, destroying the uniformity of the polymer matrix, resulting in a decrease in viscosity and a deterioration in antibacterial properties.
[0141] It can be seen from the data of Comparative Example 10 and Example 1 that when the particle size of the functional slurry is too large, the viscosity of the polymer and the antibacterial properties of the fiber are significantly reduced. This may be because when the particle size of the slurry is too large, the slurry cannot exist in a stable and uniform state during the polymerization process, and partial sedimentation may occur during the polymerization process, in which some nanomaterials agglomerate together, resulting in a decrease in the viscosity of the polymer, and larger agglomerates will block the spinneret during spinning, resulting in poor spinnability.
[0142] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a rare earth doped zinc oxide functional polyamide polymer, characterized in that: The method comprises the following steps: 1) Preparation of rare earth doped zinc oxide nanomaterials The zinc compound is dissolved in deionized water, and then a rare earth metal compound is added and stirred evenly, and then an alkyl silane compound is added, and stirred at 50-80° C. for 3-7 hours, and then an alkaline solution is added and stirred for 3-8 hours; after the reaction is completed, the solid material is filtered and dried and calcined in a muffle furnace, and then taken out after natural cooling to obtain a rare earth doped zinc oxide nanomaterial; 2) Preparation of water-based nano-functional slurry Weigh the rare earth doped zinc oxide nanomaterial and deionized water by mass, mix them evenly, then add a dispersant, grind them evenly in a sand mill, and obtain a stable and non-settling water system nano functional slurry; 3) Preparation of rare earth doped zinc oxide functional polyamide polymer The method is prepared by using aqueous solution of caprolactam, nylon diamine diacid salt, additives and water-based nano-functional slurry as raw materials, adopting a three-stage continuous polymerization process of prepolymerization, prepolymerization and postpolymerization, and then pelletizing, extracting and drying; wherein the water-based nano-functional slurry is added after the prepolymerization reaction; Wherein, the mass ratio of the zinc compound to the rare earth metal compound is 1:1.1-2; The rare earth metal compound is a mixture of lanthanum chloride heptahydrate, gadolinium nitrate hexahydrate and cerium chloride heptahydrate, and the mass ratio of the three substances is (2-5):2:1; The particle size of the water-based nano-functional slurry is 100-350nm; The rare earth doped zinc oxide nanomaterial accounts for 0.5-5wt% of the total feed.
2. The method for preparing a rare earth doped zinc oxide functional polyamide polymer according to claim 1, characterized in that: In step 1), by weight, the zinc compound is 20-60 parts, deionized water is 40-100 parts, the rare earth metal compound is 20-70 parts, the alkylsilane compound is 10-50 parts, and the alkaline solution is 5-40 parts.
3. The method for preparing a rare earth doped zinc oxide functional polyamide polymer according to claim 2, characterized in that: The zinc compound is one of zinc nitrate, zinc sulfate or zinc acetate; The alkaline solution is one of ammonia water, urea, ammonium carbonate or sodium hydroxide.
4. The method for preparing rare earth doped zinc oxide functional polyamide polymer according to claim 1, characterized in that: In step 1), the solid drying temperature is 50-100°C, the muffle furnace calcination temperature is 800-1200°C, and the calcination time is 2-6 hours.
5. The method for preparing rare earth doped zinc oxide functional polyamide polymer according to claim 1, characterized in that: In step 2), the mass ratio of rare earth doped zinc oxide nanomaterial: deionized water: dispersant is (25-40): (57-74.5): (0.5-3); The dispersant is one or more of hexadecyltrimethylammonium bromide, polyvinylpyrrolidone, modified styrene maleic acid copolymer solution, modified polymer block copolymer, and high molecular weight silane copolymer containing pigment affinity groups.
6. The method for preparing rare earth doped zinc oxide functional polyamide polymer according to claim 1, characterized in that: The specific steps of step 3) are: A. uniformly mixing caprolactam, an aqueous solution of nylon diamine diacid salt and an additive to obtain a first mixture, and performing a prepolymerization reaction under high temperature and pressure to obtain a polyamide oligomer; B. After the prepolymerization reaction, the polyamide oligomer obtained in step A is mixed with the aqueous nano-functional slurry to obtain a second mixture; C. The second mixture obtained in step B is subjected to pre-polymerization reaction and post-polymerization reaction to form a rare earth doped zinc oxide functional polyamide polymer.
7. The method for preparing rare earth doped zinc oxide functional polyamide polymer according to claim 6, characterized in that: The nylon diamine dicarboxylic acid salt is one of nylon 66 salt, nylon 610 salt, nylon 612 salt, nylon 56 salt, nylon 510 salt and nylon 512 salt; The concentration of the nylon diamine diacid aqueous solution is 50-80wt%; Nylon diamine diacid salt accounts for 5-25wt% of the total feed; The additive is one or more of acetic acid, benzoic acid, purified terephthalic acid and hexamethylenediamine, and the dosage of the additive is 0.05-0.3% of the mass of caprolactam.
8. A rare earth doped zinc oxide functional polyamide polymer prepared by the preparation method according to any one of claims 1 to 7, characterized in that: The polymer is white.
9. The use of the rare earth doped zinc oxide functional polyamide polymer in antibacterial fibers, films, and engineering plastics as claimed in claim 8, characterized in that: The rare earth doped zinc oxide functional polyamide polymer is pelletized, extracted and dried to obtain rare earth doped zinc oxide functional polyamide slices, wherein the slices have an extractable content of 0.3-0.5%, a water content of 200-400 ppm and a relative viscosity of 2.4-4.0.