Composite material and preparation method thereof

By introducing array carbon nanotubes and graphite into glass carbon materials, combined with microwave processing technology, the problem of insufficient thermal conductivity and bending resistance of glass carbon materials is solved, and the high thermal conductivity and mechanical properties are improved, suitable for heat dissipation systems and Thermal management equipment.

CN118703018BActive Publication Date: 2024-11-15湖南德智新材料股份有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411198525.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-11-15
Estimated Expiration
2044-08-29

AI Technical Summary

Technical Problem

The low thermal conductivity and bending resistance of glass carbon materials limit their application in heat dissipation systems and thermal management equipment, and the poor dispersion of carbon nanotubes and glass carbon leads to a low mechanical strength of composite materials and less significant improvement in thermal conductivity.

Method used

Array carbon nanotubes were deposited on a catalyst-containing substrate by CVD method, and mixed with graphite and linear resin for molding treatment, followed by microwave treatment to form a composite material containing glass carbon. By adjusting the ratio of graphite and array carbon nanotubes and density to improve the thermal conductivity and mechanical properties of composite materials.

Benefits of technology

A composite material with high thermal conductivity and good flexural strength is obtained, which is suitable for industrial production and improves the thermal expansion coefficient and mechanical properties of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118703018B_ABST
    Figure CN118703018B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of carbon nanotube / glassy carbon composite materials, and provides a composite material and a preparation method thereof. The preparation method of the composite material comprises: depositing array carbon nanotubes on a substrate containing a catalyst by a CVD method; mixing graphite, a linear resin, a curing agent and a coupling agent to obtain a first mixture; applying the first mixture to the surface of the array carbon nanotubes and performing a molding process; performing a microwave treatment on the product after the molding process to obtain a composite material containing glassy carbon; the average particle size of the graphite and the density of the array carbon nanotubes satisfy the relationship: 10≤A / B≤120, wherein A is the average particle size of the graphite, in μm, and B is the density of the array carbon nanotubes, in g / cm 3 The composite material provided by the present invention has good thermal conductivity and mechanical properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of carbon nanotube / glassy carbon composite materials, and in particular to a composite material and a preparation method thereof. Background Art

[0002] Glassy carbon is a nanomaterial composed of carbon atoms, with excellent properties such as high strength, low density and good chemical resistance. However, glassy carbon is an amorphous or partially crystalline structure, which limits the speed of energy propagation in the material, thereby reducing the efficiency of heat conduction. The presence of micropores and mesopores in glassy carbon increases the porosity of the material, and the increase in porosity further reduces the thermal conductivity of the material. Therefore, the relatively low thermal conductivity of glassy carbon limits its application in the fields of heat dissipation systems and thermal management equipment, and its high strength also makes its bending resistance poor, further limiting its application in the fields of heat dissipation systems and thermal management equipment.

[0003] Therefore, there is an urgent need to provide a composite material containing glassy carbon and having good thermal conductivity. Summary of the invention

[0004] The purpose of the present invention is to overcome the above problems existing in the prior art and to provide a composite material and a preparation method thereof. A composite material with higher thermal conductivity can be prepared by the method described in the present invention.

[0005] In order to achieve the above-mentioned object, the first aspect of the present invention provides a method for preparing a composite material, which comprises: (1) depositing array carbon nanotubes on a substrate containing a catalyst by a CVD method; (2) mixing graphite, a linear resin, a curing agent and a coupling agent to obtain a first mixture; (3) applying the first mixture to the surface of the array carbon nanotubes and performing a molding process, wherein the molding process comprises: a temperature of 50°C-100°C, a pressure of 0.5MPa-2MPa, and a time of 5h-15h; (4) performing a microwave treatment on the product after the molding process to obtain a composite material containing glassy carbon; wherein the microwave treatment process comprises: a temperature of 900°C-1600°C and a power of 700W-1400W; and the average particle size of the graphite and the density of the array carbon nanotubes satisfy the relationship: 10≤A / B≤120, wherein A is the average particle size of the graphite, in μm, and B is the density of the array carbon nanotubes, in g / cm 3 Compared with 100 parts by mass of the first mixture, the amount of the graphite is 5-30 parts by mass, the amount of the linear resin is 55-93 parts by mass, the amount of the curing agent is 1-5 parts by mass, the amount of the coupling agent is 1-10 parts by mass, and the amount of the array carbon nanotube is 16-50 parts by mass.

[0006] In some embodiments, the amount of the array carbon nanotubes is 16-50 parts by mass relative to 100 parts by mass of the first mixture.

[0007] In some embodiments, the method for preparing the array carbon nanotubes comprises depositing the array carbon nanotubes on a substrate containing a catalyst by a CVD method under the conditions of applying an external electric field and pressure; wherein the direction of the external electric field is perpendicular to the substrate.

[0008] The second aspect of the present invention provides a composite material prepared by the method described in the first aspect.

[0009] In some embodiments, the composite material includes arrayed carbon nanotubes, graphite, and glassy carbon dispersed in the arrayed carbon nanotubes; a single carbon nanotube in the arrayed carbon nanotubes has a diameter of 50 nm-200 nm and a length of 100 μm-500 μm.

[0010] In some embodiments, the composite material contains 10 wt %-25 wt % of array carbon nanotubes, ≤5 wt % of graphite, and 70 wt %-85 wt % of glassy carbon.

[0011] Glassy carbon has excellent properties such as high strength, low density and good chemical resistance. However, the relatively low thermal conductivity of glassy carbon limits its application in fields such as heat dissipation systems and thermal management equipment. Carbon nanotubes have the advantages of good thermal conductivity and good mechanical properties. During the experiment, it was found that the use of carbon nanotubes can enhance the thermal conductivity and mechanical properties of glassy carbon. However, it was also found that the affinity between the functional groups on the surface of carbon nanotubes and the surface of glassy carbon was not high enough, resulting in low mechanical strength of the final composite material. Carbon nanotubes are not easy to disperse evenly on glassy carbon, and due to the agglomeration characteristics of carbon nanotubes, the number of carbon nanotubes loaded on glassy carbon is limited, and the thermal conductivity of the obtained composite material is not significantly improved. Further research found that a composite material containing arrayed carbon nanotubes, graphite and glassy carbon was formed by the above means, and the composite material had high thermal conductivity and good mechanical properties.

[0012] The present invention adopts the above technical solution to achieve the following beneficial effects:

[0013] In the preparation process of the composite material of the present invention, the array carbon nanotubes with certain directionality are used, combined with graphite and linear resin, which is more conducive to reducing the thermal expansion coefficient and improving the mechanical properties of the composite material compared with conventional carbon nanotubes, so that the composite material has good thermal conductivity and bending strength. In addition, the good thermal conductivity of the array carbon nanotubes itself can also further improve the thermal conductivity and mechanical properties of the composite material.

[0014] The preparation method of the composite material provided by the invention has simple process and high production efficiency and is suitable for industrial production.

[0015] The endpoints and any values ​​of the range disclosed in this article are not limited to the precise range or value, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article. Herein, in the absence of special instructions, data ranges include endpoints. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 Shown is a SEM image of the surface of the composite material in Example 3.

[0017] Figure 2 Shown is the SEM image of the array carbon nanotubes in Example 3. DETAILED DESCRIPTION

[0018] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.

[0019] Unless otherwise defined, all scientific and technical terms used in the present invention have the same meanings as commonly understood by one of ordinary skill in the art to which the present invention relates.

[0020] A first aspect of the present invention provides a method for preparing a composite material, the method comprising:

[0021] (1) depositing array carbon nanotubes on a substrate containing a catalyst by a CVD method; (2) mixing graphite, a linear resin, a curing agent and a coupling agent to obtain a first mixture; (3) applying the first mixture to the surface of the array carbon nanotubes and performing a molding process, wherein the molding process comprises: a temperature of 50°C-100°C, for example, 50°C, 60°C, 70°C, 80°C, 90°C and 100°C, a pressure of 0.5MPa-2MPa, for example, 0.5MPa, 1MPa, 1.5MPa and 2MPa, and a time of 5h-15h, for example, 5h, 7h, 9h, 10h, 11h, 13h and 15h; (4) subjecting the molding process to a heating process. The treated product is subjected to microwave treatment to obtain a composite material containing glassy carbon; the microwave treatment conditions include: a temperature of 900°C-1600°C, for example, 900°C, 1000°C, 1100°C, 1200°C, 1300°C, 1400°C, 1500°C and 1600°C, and a power of 700W-1400W, for example, 700W, 800W, 900W, 1000W, 1100W, 1200W and 1400W; the average particle size of the graphite and the density of the array carbon nanotubes satisfy the relationship: 10≤A / B≤120, wherein A is the average particle size of the graphite, in μm, and B is the density of the array carbon nanotubes, in g / cm 3 Compared with 100 parts by mass of the first mixture, the amount of the graphite is 5-30 parts by mass, the amount of the linear resin is 55-93 parts by mass, the amount of the curing agent is 1-5 parts by mass, the amount of the coupling agent is 1-10 parts by mass, and the amount of the array carbon nanotube is 16-50 parts by mass.

[0022] In some embodiments, the microwave treatment time is 100 min-320 min, for example, 100 min, 150 min, 200 min, 250 min, 300 min and 320 min.

[0023] By subjecting the molded product to microwave treatment, microwave energy can be directly converted into heat inside the material, causing the material temperature to rise rapidly, causing the organic matter in the molded product to decompose, and the volatile matter in the raw material to escape, leaving behind a composite material containing glassy carbon as solid carbon. After microwave curing, the linear resin in the molded product is converted into glassy carbon, while the array carbon nanotubes in the composite material can be retained.

[0024] In some embodiments, the molding mold is a conventional mold in the art, so that the product after the molding process is formed into a preform with a certain size or shape.

[0025] In the present invention, the average particle size of the graphite and the density of the array carbon nanotubes satisfy the relationship: 10≤A / B≤120, for example, it can be 10, 15, 20, 30, 40, 50, 60, 70, 80, 90, 100, 110 and 120, wherein A is the average particle size of the graphite, in μm, and B is the density of the array carbon nanotubes, in g / cm 3 When the average particle size A of graphite and the density B of the array carbon nanotubes satisfy the above relationship, the composite material has good thermal conductivity and bending strength, and a small thermal expansion coefficient.

[0026] In some embodiments, the average particle size of the graphite and the density of the array carbon nanotubes satisfy the relationship: 15≤A / B≤100, wherein A is the average particle size of the graphite, in μm, and B is the density of the array carbon nanotubes, in g / cm 3 .

[0027] In some embodiments, the average particle size of the graphite is 20 μm-100 μm, for example, 20 μm, 30 μm, 40 μm, 50 μm, 60 μm, 70 μm, 80 μm, 90 μm and 100 μm. Preferably, the average particle size of the graphite is 30 μm-55 μm. The test method for the average particle size of the graphite is "Graphite Anode Materials for Lithium Ion Batteries" (GB / T 24533-2019).

[0028] The density of the array carbon nanotubes is 0.7 g / cm 3 -1.4g / cm 3 , for example, it can be 0.7 g / cm 3 , 0.8g / cm 3 , 0.9g / cm 3 , 1g / cm 3 , 1.1g / cm 3 , 1.2g / cm 3 and 1.4g / cm 3 The density of the carbon nanotube array is the ratio of the amount of the carbon nanotube array to the volume of the carbon nanotube array.

[0029] In the present invention, graphite, linear resin, curing agent and coupling agent are mixed to obtain a first mixture. In the present invention, compared with 100 parts by mass of the first mixture, the amount of the graphite is 5-30 parts by mass, for example, it can be 5 parts by mass, 8 parts by mass, 10 parts by mass, 12 parts by mass, 14 parts by mass, 16 parts by mass, 18 parts by mass, 20 parts by mass, 22 parts by mass, 24 parts by mass, 26 parts by mass, 28 parts by mass and 30 parts by mass; the amount of the linear resin is 55-93 parts by mass, for example, it can be 55 parts by mass, 60 parts by mass, 65 parts by mass, 70 parts by mass, 75 parts by mass, 80 parts by mass, 85 parts by mass, 90 parts by mass and 93 parts by mass; the amount of the curing agent is 1-5 parts by mass, for example, it can be 1 part by mass, 2 parts by mass, 3 parts by mass, 4 parts by mass and 5 parts by mass; the amount of the coupling agent is 1-10 parts by mass, for example, it can be 1 part by mass, 2 parts by mass, 4 parts by mass, 6 parts by mass, 8 parts by mass and 10 parts by mass.

[0030] In some embodiments, the epoxy value of the linear resin is 0.1 mol / 100 g-0.3 mol / 100 g, such as 0.1 mol / 100 g, 0.15 mol / 100 g, 0.2 mol / 100 g, 0.25 mol / 100 g, and 0.3 mol / 100 g.

[0031] In some embodiments, the free phenol of the linear resin is ≤ 10%, such as 2%, 4%, 6%, 8% and 10%.

[0032] In some embodiments, the linear resin has a solid content of 80%-90%, such as 80%, 82%, 84%, 86%, 88% and 90%.

[0033] In some embodiments, the linear resin includes linear phenolic resin and / or linear furfural resin. Studies have shown that the use of linear resins can make the prepared composite material have higher thermal conductivity and better mechanical properties, while the thermal conductivity of the composite material prepared by nonlinear resins such as branched resins and cross-linked resins is poor.

[0034] In some embodiments, the curing agent includes at least one of ammonium persulfate, potassium dihydrogen phosphate, and a phenolic resin self-condensation agent.

[0035] In some embodiments, the coupling agent includes glass fibers and / or viscose fibers.

[0036] In some embodiments, compared to 100 parts by mass of the first mixture, the amount of glass fiber used is 1-5 parts by mass, for example, 1 part by mass, 2 parts by mass, 3 parts by mass, 4 parts by mass and 5 parts by mass, and the amount of viscose fiber used is 1-5 parts by mass, for example, 1 part by mass, 1.2 parts by mass, 1.4 parts by mass, 1.6 parts by mass, 1.8 parts by mass, 2 parts by mass, 3 parts by mass, 4 parts by mass and 5 parts by mass.

[0037] In the present invention, the arrayed carbon nanotubes are mixed with the first mixture to obtain a product after molding.

[0038] In some embodiments, a vibration device is used to vibrate the substrate or the bottom plate of the reaction chamber to uniformly mix the first mixture with the arrayed carbon nanotubes. The vibration is achieved by a mechanical vibrator or an ultrasonic vibrator.

[0039] In some embodiments, compared to 100 parts by mass of the first mixture, the amount of the array carbon nanotubes is 16-50 parts by mass, for example, 16 parts by mass, 20 parts by mass, 25 parts by mass, 30 parts by mass, 35 parts by mass, 40 parts by mass, 45 parts by mass and 50 parts by mass, preferably 20-35 parts by mass. The array carbon nanotubes are hollow structures, so the addition of the array carbon nanotubes is beneficial to improving the flexural strength of the composite material.

[0040] In some embodiments, the method for preparing the array carbon nanotubes comprises depositing the array carbon nanotubes on a substrate containing a catalyst by a CVD method under the conditions of applying an external electric field and pressure; wherein the direction of the external electric field is perpendicular to the substrate.

[0041] In some embodiments, the conditions for applying an external electric field include: the electric field strength is 0.2MV / m-3MV / m, for example, it can be 0.2MV / m, 0.6MV / m, 1MV / m, 1.4MV / m, 1.8MV / m, 2MV / m, 2.4MV / m, 2.8MV / m and 3MV / m; the distance between electrodes is 8μm-20μm, for example, it can be 8μm, 10μm, 12μm, 14μm, 16μm, 18μm and 20μm.

[0042] In some embodiments, the electrodes are parallel plate electrodes, the distance between the electrodes is the distance between any two positive electrodes or any two negative electrodes, and an electric field is applied between the positive plate and the negative plate.

[0043] In some embodiments, the direction of the electric field can affect the growth direction of the array carbon nanotubes, so that the array carbon nanotubes are arranged perpendicular to the substrate. A higher electric field strength can promote the longitudinal growth speed of the array carbon nanotubes.

[0044] In some embodiments, the direction of the electric field is a forward electric field or a reverse electric field, wherein the forward electric field is the direction from the negative electrode to the positive electrode, and the direction in which the array carbon nanotubes grow is consistent with the direction of the electric field. The reverse electric field is the direction from the positive electrode to the negative electrode, and the direction in which the array carbon nanotubes grow is opposite to the direction of the electric field.

[0045] In some embodiments, the pressure applied in the growth direction of the array carbon nanotubes is 10-30 MPa, such as 10 MPa, 15 MPa, 20 MPa, 25 MPa and 30 MPa. By applying an external electric field, and making the direction of the external electric field perpendicular to the substrate, a certain pressure is applied in the growth direction of the array carbon nanotubes, thereby affecting the growth density of the array carbon nanotubes.

[0046] In some embodiments, the pressure applied in the shear direction of the array carbon nanotubes is 1-5MPa, such as 1MPa, 2MPa, 3MPa, 4MPa and 5MPa. The device or means for applying pressure is that the reaction chamber must contain multiple parallel plates and grid structures, and shear force will be generated when the gas passes through these structures. Then, a specific flow effect is generated through a carefully designed airflow pattern, which can indirectly introduce shear force during the deposition process. By adjusting the position, shape and size of the gas inlet and outlet, different airflow patterns such as vortex, laminar flow or jet can be generated, which can affect the density of the carbon nanotubes.

[0047] In some embodiments, the pressure applied by the external electric field refers to setting the external electric field in a direction perpendicular to the substrate or perpendicular to the growth direction of the carbon nanotubes. In some embodiments, the pressure applied by the external electric field in the growth direction of the array carbon nanotubes is 10-30 MPa. That is, at this time, the direction in which the pressure applied by the external electric field is the growth direction of the array carbon nanotubes.

[0048] In some embodiments, the pressure applied by the external electric field in the shear direction of the carbon nanotube array is 1-5 MPa, that is, the direction in which the pressure applied by the external electric field is the shear direction of the carbon nanotube array.

[0049] In some embodiments, the direction of applying pressure includes applying pressure in the growth direction of the carbon nanotube array and applying pressure in the shear direction of the carbon nanotube array.

[0050] In some embodiments, the substrate is graphite, quartz, or silicon.

[0051] In some embodiments, before applying the catalyst to the substrate, the substrate is surface treated by vacuum high temperature annealing at 1200° C.-1600° C. to remove impurities on the substrate surface and improve the adhesion of the substrate surface.

[0052] In some embodiments, the catalyst may be added to the substrate by immersing the substrate in a solution containing the catalyst, or by coating the solution containing the catalyst on the surface of the substrate.

[0053] In some embodiments, the catalyst is an iron-containing catalyst.

[0054] In some embodiments, the catalyst may be at least one of triacetylcyclopentadienyl iron, iron-molybdenum alloy (Fe-Mo alloy), Fe3O4 nanoparticles, copper ferrite, and iron nanoparticles.

[0055] In some embodiments, the deposition conditions include: a deposition temperature of 700°C-1000°C, for example, 700°C, 750°C, 800°C, 850°C, 900°C, 950°C and 1000°C; a deposition pressure of 6kPa-10kPa, for example, 6kPa, 6.5kPa, 7kPa, 7.5kPa, 8kPa, 8.5kPa, 9kPa, 9.5kPa and 10kPa; and a deposition time of 4h-7h, for example, 4h, 5h, 6h and 7h.

[0056] In some embodiments, the heating method can be resistive heating.

[0057] In some embodiments, the gas system used in the deposition process includes a carbon source gas and hydrogen, and the flow ratio of the carbon source gas to hydrogen is 1:(2-50), for example, 1:2, 1:5, 1:10, 1:15, 1:20, 1:25, 1:30, 1:35, 1:40, 1:45 and 1:50.

[0058] In some embodiments, the carbon source gas includes at least one of C1-C4 alkanes and C2-C4 alkenes. In some embodiments, the carbon source gas includes at least one of ethylene, methane and propylene.

[0059] In some embodiments, the gas system further includes a diluent gas.

[0060] In some embodiments, the flow rate of the diluent gas is 55-85% of the total flow rate of the gas system used in the deposition process, for example, 55%, 60%, 65%, 70%, 75%, 80% and 85%. In some embodiments, the diluent gas is an inert gas, such as argon (Ar) and helium (He).

[0061] In some embodiments, after the substrate containing the catalyst is placed in the CVD reaction chamber, pre-treatment is performed, that is, vacuum extraction is performed under an inert atmosphere to remove oxygen, moisture and other impurities in the reaction chamber to ensure that the environment in the reaction chamber is clean and oxygen-free.

[0062] In some embodiments, the method for preparing the array carbon nanotubes further includes a post-processing process, that is, taking out the prepared array carbon nanotubes and performing cleaning and annealing steps to remove residual catalysts or other impurities to enhance the structure and performance of CNTs.

[0063] In some embodiments, the method for preparing the array carbon nanotube further comprises peeling off the substrate.

[0064] The second aspect of the present invention provides a composite material prepared by the method described in the first aspect.

[0065] In some embodiments, the composite material includes arrayed carbon nanotubes, graphite, and glassy carbon dispersed in the arrayed carbon nanotubes.

[0066] In some embodiments, the diameter of a single carbon nanotube in the array carbon nanotube is 50nm-200nm, for example, 50nm, 80nm, 100nm, 120nm, 150nm, 180nm and 200nm, preferably 100nm-150nm; the diameter of the array carbon nanotube is the diameter of a single carbon nanotube; the length is 100μm-500μm, for example, 100μm, 120μm, 150μm, 200μm, 250μm, 300μm, 350μm, 400μm, 450μm and 500μm, preferably, the length is 200μm-300μm. When the diameter of a single carbon nanotube is within the above range, it is beneficial to improve the thermal conductivity of the composite material. When the amount of the first mixture added is certain, when the first mixture is completely mixed with the array carbon nanotubes and the length of the array carbon nanotubes is less than 100μm, the bending strength of the composite material is poor.

[0067] In the present invention, the density of the array carbon nanotubes is tested according to GB_T 25995-2010, "Test method for density and apparent porosity of fine ceramics".

[0068] In some embodiments, the content of array carbon nanotubes in the composite material is 10wt%-25wt%, for example, it can be 10wt%, 12wt%, 14wt%, 16wt%, 18wt%, 20wt%, 22wt%, 24wt% and 25wt%; the graphite content is ≤5wt%, for example, it can be 0.5wt%, 1wt%, 2wt%, 3wt%, 4wt% and 5wt%; the glassy carbon content is 70wt%-85wt%, for example, it can be 70wt%, 72wt%, 74wt%, 75wt%, 76wt%, 78wt%, 80wt%, 82wt%, 84wt% and 85wt%.

[0069] In some embodiments, the thermal conductivity of the composite material is 120 W / mK-200 W / mK, for example, 120 W / mK, 130 W / mK, 140 W / mK, 150 W / mK, 160 W / mK, 170 W / mK, 180 W / mK, 190 W / mK and 200 W / mK.

[0070] In the present invention, the thermal conductivity test method is GB_T 22588-2008 flash method for measuring thermal diffusion coefficient or thermal conductivity.

[0071] In some embodiments, the thermal expansion coefficient of the composite material is 3×10 -6 / ℃-5×10 -6 / ℃, for example, it can be 3×10 -6 / ℃、3.2×10 -6 / ℃、3.5×10 -6 / ℃、3.7×10 -6 / ℃、4×10 -6 / ℃、4.2×10 -6 / ℃、4.4×10 -6 / ℃、4.5×10 -6 / ℃ and 5×10 -6 / ℃.

[0072] In the present invention, the test method of the thermal expansion coefficient is the ejector method of GB_T 16535-2008 Test method for thermal expansion coefficient of fine ceramics.

[0073] In some embodiments, the resistivity of the composite material is 8µΩ·m-30µΩ·m, for example, 8µΩ·m, 10µΩ·m, 12µΩ·m, 14µΩ·m, 16µΩ·m, 18µΩ·m, 20µΩ·m, 22µΩ·m, 24µΩ·m, 26µΩ·m, 28µΩ·m and 30µΩ·m. In the present invention, the test method for the resistivity is GB_T 31838.2-2019 Dielectric and resistive properties of solid insulating materials Part 2 Resistive properties (DC method) Volume resistance and volume resistivity.

[0074] In some embodiments, the flexural strength of the composite material is 55 MPa-80 MPa, for example, 55 MPa, 60 MPa, 65 MPa, 70 MPa, 75 MPa and 80 MPa.

[0075] In some embodiments, the compressive strength of the composite material is 120 MPa-180 MPa, for example, 120 MPa, 130 MPa, 140 MPa, 150 MPa, 160 MPa, 170 MPa and 180 MPa.

[0076] In the present invention, the compressive strength test method is GB_T 8489-2006 Fine Ceramics Compression Strength Test Method.

[0077] In some embodiments, the shear strength of the composite material is 60MPa-90MPa, for example, 60MPa, 65MPa, 70MPa, 75MPa, 80MPa, 85MPa and 90MPa. The shear strength of the composite material is relatively large, that is, the interface compatibility between the array carbon nanotubes and the glassy carbon is good, which helps to form a strong interface bond, and good interface contact is conducive to reducing thermal resistance, thereby promoting heat transfer and improving the thermal conductivity of the composite material.

[0078] In the present invention, the shear strength is tested by the cross-cross method of GB_T 31541-2015 Test method for fine ceramic interface tensile and shear bond strength.

[0079] In some embodiments, the elastic modulus of the composite material is 12 GPa-25 GPa, for example, 12 GPa, 14 GPa, 16 GPa, 18 GPa, 20 GPa, 22 GPa and 25 GPa.

[0080] In the present invention, the elastic modulus test method is the bending method of GB / T 10700-2006 fine ceramic elastic modulus test method.

[0081] In some embodiments, the hardness of the composite material is 60HSD-80HSD, for example, it can be 60HSD, 62HSD, 64HSD, 66HSD, 68HSD, 70HSD, 72HSD, 74HSD, 76HSD, 78HSD and 80HSD.

[0082] In the present invention, the test method for hardness is GBT_4340_1-2009 Metallic Materials Vickers Hardness Test Part 1: Test Method.

[0083] The ordered arrangement structure and high aspect ratio of the arrayed carbon nanotubes are conducive to making full use of the space of the arrayed carbon nanotubes and increasing the loading amount of glassy carbon inside the arrayed carbon nanotubes, thereby enhancing the performance of the composite material. The high loading amount can also achieve better stress transfer and load dispersion, further improving the mechanical properties of the composite material.

[0084] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0085] Unless otherwise specified, the materials and reagents used in the following examples can be obtained from commercial sources.

[0086] The present invention is described in detail below in conjunction with specific embodiments, which are used to understand but not to limit the present invention.

[0087] Example 1

[0088] This example is used to illustrate the preparation method of the composite material of the present invention.

[0089] (1) A graphite substrate was immersed in a solution of triacetylcyclopentadienyl iron with a concentration of 0.5 wt% and placed in a CVD reaction chamber. A negative electrode was placed at the bottom and a positive electrode was placed at the top in a direction perpendicular to the substrate. The distance between the electrodes was 12 μm and the electric field strength was 1.5 MV / m.

[0090] Ethylene gas and H2 are introduced into the CVD reaction chamber, and the dilution gas is argon. During the deposition process of the array carbon nanotubes, force is applied in the growth direction and shear direction of the array carbon nanotubes at the same time. The pressure in the growth direction is 18.4MPa, and the pressure in the shear direction is 2.8MPa.

[0091] Among them, the flow ratio of ethylene gas and H2 is 1:6, the flow rate of dilution gas is 70% of the total flow rate of the gas system used in the deposition process, and the deposition process parameters are set: deposition temperature is 950℃, deposition pressure is 7KPa, deposition time is 5.5h, after the chemical vapor deposition is completed, stop the introduction of reaction gas, and continue to introduce protective gas argon to cool down the temperature to obtain array carbon nanotubes. The density of array carbon nanotubes is 1.1g / cm 3 The diameter of a single carbon nanotube is 126nm and the length of the carbon nanotube is 282μm.

[0092] (2) Graphite with an average particle size of 40 μm, linear phenolic resin PF-8216, a curing agent (phenolic resin self-condensation agent), glass fiber and viscose fiber are mixed to obtain a first mixture, wherein, in 100 parts by mass of the first mixture, the amount of graphite is 15 parts by mass, the amount of linear phenolic resin is 75.5 parts by mass, the amount of phenolic resin self-condensation agent is 3.5 parts by mass, the amount of glass fiber is 4 parts by mass, and the amount of viscose fiber is 2 parts by mass. The epoxy value of the linear phenolic resin is 0.16 mol / 100 g, the free phenol is 0.2%, and the solid content of the linear phenolic resin is 85%.

[0093] (3) The array carbon nanotubes containing the base are placed in a mold with the base in contact with the bottom of the mold, and the first mixture is poured into the mold so that the first mixture covers the array carbon nanotubes and the first mixture and the array carbon nanotubes are evenly mixed by a vibration device. Compared with 100 parts by mass of the first mixture, the amount of the array carbon nanotubes used is 32 parts by mass.

[0094] (4) The product obtained by uniformly mixing the first mixture with the array carbon nanotubes is subjected to molding treatment. The molding treatment conditions are a temperature of 80° C., a pressure of 0.8 MPa, and molding in a mold for 10 hours. The product is then subjected to microwave treatment. The microwave treatment temperature is 1100° C., the power is 1000 W, and the time is 200 minutes. After microwave treatment, the composite material is obtained. The glassy carbon content of the composite material is 75.5wt%, the array carbon nanotube content is 22wt%, and the graphite content is 2.5wt%. The product after the molding treatment is microwave cured and the base is removed to obtain a composite material containing glassy carbon.

[0095] The thermal conductivity of the composite material is 176 W / mK, the flexural strength of the composite material is 72 MPa, and the thermal expansion coefficient of the composite material is 3.6×10 -6 / ℃, the resistivity of the composite material is 14µΩ·m, the compressive strength of the composite material is 161MPa, the shear strength of the composite material is 68MPa, the elastic modulus of the composite material is 18GPa, and the hardness of the composite material is 67HSD.

[0096] Example 2

[0097] (1) A graphite substrate was immersed in a solution of triacetylcyclopentadienyl iron with a concentration of 0.5 wt% and placed in a CVD reaction chamber. A negative electrode was placed at the bottom and a positive electrode was placed at the top in a direction perpendicular to the substrate. The distance between the electrodes was 8 μm and the electric field strength was 0.2 MV / m.

[0098] Ethylene gas and H2 are introduced into the CVD reaction chamber, and the dilution gas is argon. During the deposition process of the array carbon nanotubes, force is applied simultaneously in the growth direction and shear direction of the array carbon nanotubes. The pressure in the growth direction is 10.1 MPa, and the pressure in the shear direction is 1.2 MPa.

[0099] Among them, the flow ratio of ethylene gas and H2 is 1:6, the flow rate of dilution gas is 70% of the total flow rate of the gas system used in the deposition process, and the deposition process parameters are set: deposition temperature is 950℃, deposition pressure is 7KPa, deposition time is 5.5h, after the chemical vapor deposition is completed, stop the introduction of reaction gas, and continue to introduce protective gas argon to cool down the process to obtain array carbon nanotubes. The density of array carbon nanotubes is 0.7g / cm 3The diameter of a single carbon nanotube is 112nm and the length of the carbon nanotube is 216μm.

[0100] (2) Graphite with an average particle size of 30 μm, linear furfural resin, a curing agent (potassium dihydrogen phosphate), glass fiber and viscose fiber are mixed to obtain 100 parts by mass of a first mixture, wherein the amount of graphite is 10 parts by mass, the amount of linear furfural resin is 80.5 parts by mass, the amount of potassium dihydrogen phosphate is 3.5 parts by mass, the amount of glass fiber is 4 parts by mass, and the amount of viscose fiber is 2 parts by mass. The epoxy value of the linear furfural resin is 0.1 mol / 100 g, the free phenol of the linear furfural resin is 0.5%, and the solid content of the linear furfural resin is 80%.

[0101] (3) placing the array carbon nanotubes containing the base in a mold with the base in contact with the bottom of the mold, pouring the first mixture into the mold so that the first mixture covers the array carbon nanotubes and uniformly mixing the first mixture and the array carbon nanotubes through a vibration device, and mixing the first mixture and the array carbon nanotubes to obtain a molded product, wherein the amount of the first mixture is 100 parts by mass, and the amount of the array carbon nanotubes is 36 parts by mass.

[0102] (4) The molded product is compressed in a mold at 50° C. and 0.5 MPa for 5 h, and then subjected to microwave treatment at a temperature of 1000° C., a power of 700 W, and a time of 100 min to obtain the composite material.

[0103] Example 3

[0104] (1) A graphite substrate was immersed in a solution of triacetylcyclopentadienyl iron with a concentration of 0.5 wt% and placed in a CVD reaction chamber. A negative electrode was placed at the bottom and a positive electrode was placed at the top in a direction perpendicular to the substrate. The distance between the electrodes was 20 μm and the electric field strength was 3 MV / m.

[0105] Ethylene gas and H2 are introduced into the CVD reaction chamber, and the dilution gas is argon. During the deposition process of the array carbon nanotubes, force is applied in the growth direction and shear direction of the array carbon nanotubes at the same time. The pressure in the growth direction is 28.7MPa, and the pressure in the shear direction is 4.9MPa.

[0106] The flow ratio of ethylene gas to H2 is 1:6, the flow rate of the dilution gas is 70% of the total flow rate of the gas system used in the deposition process, and the deposition process parameters are set as follows: the deposition temperature is 950°C, the deposition pressure is 7KPa, and the deposition time is 5.5h. After the chemical vapor deposition is completed, the reaction gas is stopped, and the protective gas argon is continuously introduced for cooling treatment to obtain array carbon nanotubes. The density of the array carbon nanotubes is 1.4g / cm 3, the diameter of a single carbon nanotube is 147nm, and the length of the carbon nanotube is 120μm. Figure 2 shown.

[0107] (2) Graphite with an average particle size of 55 μm, linear phenolic resin, phenolic resin self-condensation agent, glass fiber and viscose fiber are mixed to obtain 100 parts by mass of a first mixture, wherein the amount of graphite is 19.5 parts by mass, the amount of linear phenolic resin is 71 parts by mass, the amount of phenolic resin self-condensation agent is 3.5 parts by mass, the amount of glass fiber is 4 parts by mass, and the amount of viscose fiber is 2 parts by mass. The epoxy value of the linear phenolic resin is 0.27 mol / 100 g, the free phenol of the linear phenolic resin is 0.2%, and the solid content of the linear phenolic resin is 90%.

[0108] (3) placing the array carbon nanotubes containing the base in a mold with the base in contact with the bottom of the mold, pouring the first mixture into the mold so that the first mixture covers the array carbon nanotubes and uniformly mixing the first mixture and the array carbon nanotubes through a vibration device, and mixing the first mixture and the array carbon nanotubes to obtain a molded product, wherein the amount of the first mixture is 100 parts by mass, and the amount of the array carbon nanotubes is 25 parts by mass.

[0109] (4) The molded product is compressed in a mold at 100°C and 2MPa for 15h, and then subjected to microwave treatment at a temperature of 1200°C, a power of 1400W, and a time of 320min to obtain the composite material. Figure 1 The figure shows the SEM image of the surface of the composite material in Example 3. The interface of the composite material in the figure is tightly connected and has no obvious fractures, that is, the composite material is not easy to break and has good mechanical properties. The curled graphite fragments in the figure are in a disordered state, that is, the thermal conductivity and thermal expansion properties of the obtained composite material are good.

[0110] Example 4

[0111] This example is used to illustrate the preparation of a composite material when the ratio of the average particle size A of graphite to the density B of the array carbon nanotubes is different.

[0112] Example 4-1

[0113] The operation was carried out according to the method described in Example 1, except that the average particle size of graphite was 22 μm, and the density of the array carbon nanotubes was 1.1 g / cm 3 , the diameter of a single carbon nanotube in step (1) is 51 nm.

[0114] Example 4-2

[0115] The operation was carried out according to the method described in Example 1, except that the average particle size of graphite was 70 μm, and the density of the array carbon nanotubes was 0.7 g / cm 3 , the diameter of a single carbon nanotube in step (1) is 197 nm.

[0116] Example 5

[0117] This example is used to illustrate the preparation of a composite material when the amount of the array carbon nanotubes used is different when the first mixture is mixed with the array carbon nanotubes.

[0118] Example 5-1

[0119] The operation was carried out in accordance with the method described in Example 1, except that in step (3), when the amount of the first mixture was 100 parts by mass, the amount of the array carbon nanotubes was 40 parts by mass.

[0120] Example 5-2

[0121] The operation was carried out in accordance with the method described in Example 1, except that in step (3), when the amount of the first mixture was 100 parts by mass, the amount of the array carbon nanotubes was 18 parts by mass.

[0122] Example 5-3

[0123] The operation was carried out in accordance with the method described in Example 1, except that in step (3), when the amount of the first mixture was 100 parts by mass, the amount of the array carbon nanotubes was 10 parts by mass.

[0124] Example 6

[0125] This example is used to illustrate the preparation of composite materials under different microwave treatment conditions.

[0126] Example 6-1

[0127] The method described in Example 1 was followed, except that the temperature of the microwave treatment in step (4) was 1000°C.

[0128] Example 6-2

[0129] The method described in Example 1 was followed, except that the temperature of the microwave treatment in step (4) was 1500°C.

[0130] Example 7

[0131] This example is used to illustrate the preparation of a composite material with different amounts of graphite and linear resin.

[0132] Example 7-1

[0133] The method described in Example 1 was followed, except that the amount of graphite used in step (2) was 5 parts by mass, and the portion of the graphite that was changed was replaced by a linear resin.

[0134] Example 7-2

[0135] The method described in Example 1 was followed, except that the amount of graphite used in step (2) was 30 parts by weight, and the amounts of linear resin, curing agent, and coupling agent were varied in equal proportions.

[0136] Example 7-3

[0137] The method described in Example 1 was followed, except that in step (2), the amount of graphite was 75.5 parts by weight, the amount of linear resin was 15 parts by weight, and the amounts of curing agent and coupling agent were changed in equal proportions.

[0138] Example 8

[0139] This example is used to illustrate the preparation of composite materials with different epoxy values ​​of linear resins.

[0140] The method described in Example 1 was followed, except that the epoxy value of the linear phenolic resin in step (2) was 0.51 mol / 100 g.

[0141] Comparative Example 1

[0142] This comparative example is used to illustrate the preparation of a composite material when the first mixture is mixed with non-array carbon nanotubes.

[0143] The method described in Example 1 was followed, except that no electric field was applied during the preparation of the array carbon nanotubes in step (1), and no pressure was applied in the growth direction and shear direction of the carbon nanotubes. The density of the array carbon nanotubes was 0.6 g / cm 3 .

[0144] Comparative Example 2

[0145] This comparative example is used to illustrate the preparation of a composite material when the resin is not a linear resin.

[0146] The operation was carried out in accordance with the method described in Example 1, except that the linear phenolic resin PF-8216 was replaced by the common resin BR2123.

[0147] Comparative Example 3

[0148] This comparative example is used to illustrate the preparation of a composite material when ordinary heating is used instead of microwave treatment.

[0149] The operation was carried out in accordance with the method described in Example 1, except that after the molded product was obtained, it was not subjected to microwave treatment but was heated by ordinary resistance.

[0150] Comparative Example 4

[0151] The method described in Example 1 was followed, except that the microwave treatment in step (4) was performed at a temperature of 613° C., a power of 300 W, and a time of 200 min.

[0152] Comparative Example 5

[0153] The operation was carried out according to the method described in Example 1, except that the average particle size of graphite was 100 μm, and the density of the array carbon nanotubes was 0.7 g / cm 3 .

[0154] Test Case

[0155] The composite materials prepared in the examples and comparative examples were tested.

[0156] (1) Thermal conductivity:

[0157] The thermal conductivity was tested at 100°C according to “GB_T 22588-2008 Flash method for measuring thermal diffusion coefficient or thermal conductivity”. The results are shown in Table 1.

[0158] (2) Bending strength:

[0159] The test was carried out according to “GB_T 6569-2006 Fine Ceramics Bending Strength Test Method”, and the results are shown in Table 1.

[0160] (3) Thermal expansion coefficient:

[0161] The temperature test procedure of "GB_T 16535-2008 Fine Ceramics Linear Thermal Expansion Coefficient Test Method Ejector Method" is to increase the temperature from room temperature to 1200℃, and record the value at 500℃ to illustrate the thermal properties. The results are shown in Table 1.

[0162]

[0163] The composite materials obtained in Examples 1 to 3 in Table 1 have higher thermal conductivity and thermal expansion coefficient, that is, the composite materials have better thermal conductivity. The flexural strength of Examples 1 to 3 is higher, that is, the composite materials also have better mechanical properties.

[0164] Example 4 is used to illustrate the preparation of a composite material when the ratio of the average particle size A of graphite to the density B of the array carbon nanotubes is different, that is, when the average particle size of graphite and the density of the array carbon nanotubes satisfy the relationship: 10≤A / B≤120, the composite material has good thermal and mechanical properties. Comparative Example 5 is used to illustrate the preparation of a composite material when the ratio of the average particle size A of graphite to the density B of the array carbon nanotubes is not within the protection scope of the present invention. The thermal conductivity and mechanical properties of the composite material of Comparative Example 5 are far lower than the protection scope of the embodiments of the present invention.

[0165] Example 5 is used to illustrate the preparation of a composite material when the amount of array carbon nanotubes used when the first mixture is mixed with the array carbon nanotubes is different, and illustrates that when the amount of the first mixture and the array carbon nanotubes used when mixed is within the range of the present invention, the composite material has better mechanical and thermal properties.

[0166] Example 6 is used to illustrate the preparation of composite materials under different microwave treatment conditions. When the microwave treatment conditions are within the scope of the present invention, the composite material has good thermal conductivity and mechanical properties. Comparative Example 3 is used to illustrate the preparation of composite materials when ordinary heating methods are used instead of microwave treatment. Microwave heating is more conducive to uniform heating inside the composite material compared to ordinary heating methods, so that the composite material has higher thermal conductivity and electrical conductivity. The microwave treatment temperature of Comparative Example 4 is relatively low, which is lower than the protection range of the microwave treatment of the present invention, and the thermal conductivity and electrical conductivity of the obtained composite material are also relatively low.

[0167] Example 7 is used to illustrate the preparation of composite materials when the amount of graphite and the amount of linear resin are different. When the amount of graphite and the amount of linear resin are within the range of the present invention, the composite material has good mechanical properties and thermal properties.

[0168] Example 8 is used to illustrate the preparation of composite materials when the epoxy values ​​of linear resins are different. When the epoxy value of the linear resin is within the range of the present invention, the composite material has good thermal and mechanical properties. Comparative Example 2 is used to illustrate the preparation of composite materials when the resin is not a linear resin. When the resin is not a linear resin but a common resin, the composite material does not have a high degree of density and consistency, and thus the thermal conductivity and mechanical properties of the composite material are poor.

[0169] Comparative Example 1 is used to illustrate the preparation of a composite material when the first mixture is mixed with non-array carbon nanotubes. When the carbon nanotubes are non-array carbon nanotubes, the density of the array carbon nanotubes is relatively low, and thus the thermal conductivity and mechanical properties of the composite material are relatively low.

[0170] It should be noted that, in this article, the terms "comprise", "include" or any other variant thereof are intended to cover non-exclusive inclusion, so that the process, method, article or device including a series of elements includes not only those elements, but also includes other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise one..." do not exclude the presence of other identical elements in the process, method, article or device including the element. In addition, it should be pointed out that the scope of the methods and devices in the embodiments of the present application is not limited to performing functions in the order shown or discussed, and may also include performing functions in a substantially simultaneous manner or in reverse order according to the functions involved, for example, the described method may be performed in an order different from that described, and various steps may also be added, omitted, or combined. In addition, the features described with reference to certain examples may be combined in other examples.

[0171] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a composite material, characterized in that: The method includes: (1) Depositing array carbon nanotubes on a substrate containing a catalyst by CVD method; (2) mixing graphite, linear resin, curing agent and coupling agent to obtain a first mixture; (3) applying the first mixture to the surface of the array carbon nanotubes and performing a molding process, wherein the molding process conditions include: a temperature of 50° C. to 100° C., a pressure of 0.5 MPa to 2 MPa, and a time of 5 h to 15 h; (4) subjecting the molded product to microwave treatment to obtain a composite material containing glassy carbon; the microwave treatment conditions include: a temperature of 900° C. to 1600° C. and a power of 700 W to 1400 W; The average particle size of the graphite and the density of the array carbon nanotubes satisfy the relationship: 10≤A / B≤120, wherein A is the average particle size of the graphite, which is 20 μm-100 μm; B is the density of the array carbon nanotubes, which is 0.7 g / cm 3 -1.4g / cm 3 ; The diameter of a single carbon nanotube in the carbon nanotube array is 50nm-200nm, and the length is 100μm-500μm; Compared with 100 parts by mass of the first mixture, the amount of the graphite is 5-30 parts by mass, the amount of the linear resin is 55-93 parts by mass, the amount of the curing agent is 1-5 parts by mass, the amount of the coupling agent is 1-10 parts by mass, and the amount of the array carbon nanotube is 16-50 parts by mass.

2. The method according to claim 1, characterized in that The epoxy value of the linear resin is 0.1-0.3 mol / 100g.

3. The method according to claim 1, characterized in that The linear resin comprises a linear phenolic resin and / or a linear furfural resin; and / or, The curing agent includes at least one of ammonium persulfate, potassium dihydrogen phosphate and a phenolic resin self-condensation agent; and / or, The coupling agent includes glass fiber and / or viscose fiber.

4. The method according to claim 1, characterized in that The method for preparing the array carbon nanotubes comprises: depositing the array carbon nanotubes by a CVD method under the condition of applying an external electric field and pressure; wherein the direction of the external electric field is perpendicular to the substrate.

5. The method according to claim 4, characterized in that The conditions for applying the external electric field include: the electric field strength is 0.2MV / m-3MV / m, the distance between electrodes is 8μm-20μm; and / or, The pressure applied in the growth direction of the array carbon nanotubes is 10-30 MPa; and / or, The pressure applied in the shear direction of the arrayed carbon nanotubes is 1-5 MPa.

6. The method according to claim 4, characterized in that The substrate is graphite, quartz or silicon; and / or, The catalyst is an iron-containing catalyst; and / or, The gas system for depositing the array carbon nanotubes includes a carbon source gas, and the carbon source gas includes at least one of C1-C4 alkanes and C2-C4 alkenes.

7. A composite material prepared by the method according to any one of claims 1 to 6.

8. The composite material according to claim 7, characterized in that The composite material comprises arrayed carbon nanotubes, graphite and glassy carbon dispersed in the arrayed carbon nanotubes.

9. The composite material according to claim 8, characterized in that The content of array carbon nanotubes in the composite material is 10wt%-25wt%, the content of graphite is ≤5wt%, and the content of glassy carbon is 70wt%-85wt%.

10. The composite material according to claim 9, characterized in that The thermal conductivity of the composite material is 120W / mK-200W / mK; and / or, The thermal expansion coefficient of the composite material is 3×10 -6 / ℃-5×10 -6 / ℃; and / or, The resistivity of the composite material is 8µΩ·m-30µΩ·m; and / or, The flexural strength of the composite material is 55 MPa-80 MPa; and / or, The compressive strength of the composite material is 120MPa-180MPa; and / or, The shear strength of the composite material is 60MPa-90MPa; and / or, The elastic modulus of the composite material is 12 GPa-25 GPa; and / or, The hardness of the composite material is 60HSD-80HSD.