A kind of aging-resistant acrylic resin waterproof coating
By copolymerizing the sulfone-aminoacrylate monomer with methyl methacrylate and butyl acrylate in the acrylic resin, and adding KH550 modified zinc oxide and epoxy resin for curing and crosslinking, the water resistance and resistance of the acrylic resin are solved. The problem of insufficient UV aging performance has significantly improved the performance of the paint.
Patent Information
- Application Number
- CN202411208780.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-08-30
AI Technical Summary
Acrylic resin has poor water resistance and UV aging resistance.
Copolymerization reaction was carried out with sulfone-aminoacrylate monomer with methyl methacrylate and butyl acrylate, and KH550 modified zinc oxide and epoxy resin were added as curing crosslinking agents. Nano zinc oxide was chemically bonded through curing crosslinking reaction. Into the acrylic resin molecular chain, the interface bond strength and dispersion are enhanced, and the coating's ultraviolet and heat resistance are improved.
It significantly improves the tensile strength, elongation of break, UV resistance and heat resistance of acrylic resin, and reduces water absorption, enhancing the water resistance and water resistance of the paint.
Smart Images

Figure SMS_2 
Figure SMS_3 
Figure SMS_4
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of acrylic resins, and in particular relates to an aging-resistant acrylic resin waterproof coating. Background Art
[0002] Nano zinc oxide is cheap, easy to obtain, non-toxic and pollution-free, and has the advantages of high mechanical strength and strong UV resistance. It is widely used in coatings, inks, plastics, rubber and other materials. Surface modification of nano zinc oxide can improve its compatibility with polymer matrix, which can better improve material strength, UV resistance and other properties.
[0003] Acrylic resin coating has good color, gloss, chemical resistance and film-forming property, and is widely used in electronic appliances, mechanical equipment, wooden furniture and other aspects. At present, the methods for modifying acrylic resin mainly include copolymerization modification, filling modification, etc. When preparing acrylic resin, adding functional olefin monomers for copolymerization reaction can give acrylic resin unique properties. Adding high-performance inorganic nanomaterials to acrylic resin coating is also an effective method to improve the comprehensive performance of coatings. The patent of publication number CN116218278A discloses a modified luminescent nano zinc oxide for photocurable thick coating coating and its preparation and application. Nano zinc oxide, diisocyanate, and hydroxy acrylate are reacted to obtain modified luminescent nano zinc oxide, which improves its dispersibility in photocurable resin coating and enhances the performance of coating film. However, the patent does not improve the heat resistance and water resistance and waterproof properties of the coating film. Summary of the invention
[0004] Technical problem solved: The present invention solves the problem that acrylic resin has poor water resistance and poor UV aging resistance.
[0005] Technical solution: An aging-resistant acrylic resin waterproof coating comprises the following components in parts by weight: 100 parts of sulfone-amino acrylic resin solution, 0.5-3 parts of KH550 modified zinc oxide, 0.3-2 parts of epoxy resin, and 0.2-0.6 parts of defoaming agent.
[0006] The preparation method of sulfone-containing amino acrylic resin emulsion is:
[0007] Step A, adding polymerization monomer and sulfone-amino acrylate monomer to butyl acetate solvent, stirring to dissolve, and obtaining a monomer solution; adding butyl acetate solvent to a reaction bottle, introducing nitrogen, heating to 90-110° C., dripping the monomer solution, and controlling the dripping time to be 1.5-2.5 hours; simultaneously dripping a butyl acetate solution containing an initiator, and controlling the dripping time to be 2-3 hours; stirring to react for 6-8 hours, and cooling to obtain a sulfone-amino acrylic resin solution.
[0008] The sulfone-aminoacrylate monomer has the structural formula (I) as follows:
[0009] Formula (I).
[0010] Furthermore, the weight of the sulfone-amino acrylate monomer is 6-10% of the total weight of the polymerized monomers; the polymerized monomers are methyl methacrylate and butyl acrylate.
[0011] Furthermore, the initiator is dibenzoyl peroxide or azobisisobutyronitrile.
[0012] Further, the preparation method of sulfone-amino acrylate monomer is:
[0013] (1) Add toluene, 3-hydroxy-5-nitrobenzoic acid, pyridine and 4-benzenesulfonylbenzoyl chloride to a reaction flask, stir and react at 20-35°C for 6-9 hours, and then perform rotary evaporation and column chromatography separation. Use a gradient elution method with a solution of ethyl acetate and petroleum ether to obtain intermediate 1.
[0014] (2) Add toluene, intermediate 1, hydroxyethyl acrylate, and p-toluenesulfonic acid to a reaction flask, heat to 70-90°C, stir and react for 8-14 hours, rotary evaporate, separate by column chromatography, and gradient elute with a solution of ethyl acetate and petroleum ether to obtain intermediate 2.
[0015] (3) Add 3-5% by mass hydrochloric acid solution and iron powder to the reaction flask, stir, add intermediate 2 and ethanol at 0-5°C, react for 4-6 hours, extract with dichloromethane, rotary evaporate the organic phase, separate by column chromatography, and gradient elute with ethyl acetate and petroleum ether solution to obtain sulfone-amino acrylate monomer.
[0016] Furthermore, in (1), the masses of pyridine and 4-benzenesulfonylbenzoyl chloride are 62-70% and 150-165% of the mass of 3-hydroxy-5-nitrobenzoic acid, respectively.
[0017] Furthermore, in (2), the masses of hydroxyethyl acrylate and p-toluenesulfonic acid are 28-35% and 2.2-3% of the mass of intermediate 1, respectively.
[0018] Furthermore, in (3), the mass of the iron powder is 36-48% of the mass of the intermediate 2.
[0019] Furthermore, the preparation method of KH550 modified zinc oxide is as follows: add ethanol and nano zinc oxide into a reaction bottle, perform ultrasonic dispersion treatment, then add KH550, perform centrifugal separation after reaction, wash with ethanol, and dry to obtain KH550 modified zinc oxide.
[0020] (III) Technical effect: The present invention utilizes sulfone-amino acrylate monomer as a functional monomer, and copolymerizes it with methyl methacrylate and butyl acrylate to obtain an acrylic resin whose molecular chain contains an amino group and a heat-resistant diphenyl sulfone structure, and uses it as a film-forming substance for the coating. At the same time, KH550 modified zinc oxide and epoxy resin are added as curing cross-linking agents. During the high-temperature curing process, the amino group of the acrylic resin and the amino group on the surface of the modified zinc oxide react with the epoxy resin to undergo a curing cross-linking reaction. The three are cured and cross-linked, thereby chemically bonding the nano zinc oxide to the acrylic resin molecular chain, enhancing the interface bonding strength and dispersibility between the two, so that the nano zinc oxide plays a good reinforcing role and improves the tensile strength and elongation at break of the acrylic resin.
[0021] The KH550 modified nano zinc oxide of the present invention forms a chemical bond with acrylic resin and is uniformly dispersed in the acrylic resin matrix, which has a strong scattering effect on ultraviolet rays, thereby improving the shielding effect of the coating film on ultraviolet rays, thereby enhancing the anti-ultraviolet performance of the film. After ultraviolet aging experiments, the film still maintains very high tensile strength and elongation at break.
[0022] The invention utilizes sulfone-amino acrylate monomer as functional monomer, introduces heat-resistant diphenyl sulfone structure into acrylic resin molecular chain, significantly improves the heat resistance of coating film, and exhibits higher thermal decomposition temperature.
[0023] The present invention uses epoxy resin as a curing crosslinking agent to carry out curing crosslinking reaction on acrylic resin and KH550 modified zinc oxide, thereby increasing the crosslinking degree of the acrylic resin molecular chain and forming a tight crosslinking network in the film matrix, which is beneficial to reducing the water absorption rate of the film, thereby improving its water resistance and waterproof performance. DETAILED DESCRIPTION
[0024] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0025] Preparation of KH550 modified zinc oxide: add 60 mL of ethanol and 2 g of nano zinc oxide (average particle size 50 nm) into a reaction bottle, perform ultrasonic dispersion treatment, then add 0.4 g of KH550, heat to 60°C, stir and react for 24 hours, centrifuge, wash with ethanol, and dry to obtain KH550 modified zinc oxide.
[0026] Example 1
[0027] (1) Add 70 mL of toluene, 4 g of 3-hydroxy-5-nitrobenzoic acid (CAS registration number: 78238-14-9), 2.8 g of pyridine, and 6.6 g of 4-benzenesulfonylbenzoyl chloride (CAS registration number: 37991-83-6) to a reaction flask, stir and react at 20°C for 6 h, and after the reaction, perform rotary evaporation, separate by column chromatography, and use a gradient elution of a solution of ethyl acetate and petroleum ether to obtain intermediate 1. The reaction formula is as follows:
[0028]
[0029] (2) Add 50 mL of toluene, 4 g of intermediate 1, 1.12 g of hydroxyethyl acrylate, and 120 mg of p-toluenesulfonic acid to the reaction flask, heat to 90°C, stir and react for 8 h, rotary evaporate, separate by column chromatography, and gradient elute with a solution of ethyl acetate and petroleum ether to obtain intermediate 2. The reaction formula is as follows:
[0030]
[0031] (3) Add 6 mL of 5% hydrochloric acid solution and 1.8 g of iron powder to the reaction bottle, stir, then add 5 g of intermediate 2 and 40 mL of ethanol at 0 °C, react for 4 h, extract with dichloromethane, rotary evaporate the organic phase, separate by column chromatography, and gradient elute with ethyl acetate and petroleum ether to obtain sulfone-amino acrylate monomer. The reaction formula is as follows:
[0032]
[0033] (4) Add 15 g of methyl methacrylate, 35 g of butyl acrylate and 3 g of sulfone-amino acrylate monomer to 80 mL of butyl acetate solvent, stir to dissolve and obtain a monomer solution; add 20 mL of butyl acetate solvent to the reaction bottle, introduce nitrogen, heat to 100 °C, add the monomer solution dropwise, and control the dropping time to 1.5 h; at the same time, add butyl acetate solution (10 mL) containing 0.47 g of dibenzoyl peroxide dropwise, and control the dropping time to 2 h; stir to react for 8 h, cool to obtain a sulfone-amino acrylic resin solution.
[0034] (5) Add 0.5 g KH550 modified zinc oxide, 0.3 g epoxy resin E44 and 0.2 g defoamer (brand EFKA7250) to 100 g sulfone-amino acrylic resin solution, stir and disperse to obtain an aging-resistant acrylic resin waterproof coating.
[0035] Example 2
[0036] (1) Add 60 mL of toluene, 4 g of 3-hydroxy-5-nitrobenzoic acid, 2.48 g of pyridine, and 6 g of 4-benzenesulfonylbenzoyl chloride to a reaction flask, stir and react at 35°C for 9 h, and then perform rotary evaporation and column chromatography separation with a gradient elution of ethyl acetate and petroleum ether to obtain intermediate 1.
[0037] (2) Add 60 mL of toluene, 4 g of intermediate 1, 1.4 g of hydroxyethyl acrylate, and 88 mg of p-toluenesulfonic acid to the reaction flask, heat to 70°C, stir and react for 14 h, rotary evaporate, separate by column chromatography, and gradient elute with a solution of ethyl acetate and petroleum ether to obtain intermediate 2.
[0038] (3) Add 10 mL of 3% hydrochloric acid solution and 2.4 g of iron powder to the reaction bottle, stir, then add 5 g of intermediate 2 and 50 mL of ethanol at 5°C, react for 6 h, extract with dichloromethane, rotary evaporate the organic phase, separate by column chromatography, and gradient elute with ethyl acetate and petroleum ether solution to obtain sulfone-amino acrylate monomer.
[0039] (4) Add 18 g of methyl methacrylate, 32 g of butyl acrylate and 4.2 g of sulfone-amino acrylate monomer to 80 mL of butyl acetate solvent, stir to dissolve and obtain a monomer solution; add 20 mL of butyl acetate solvent to the reaction bottle, introduce nitrogen, heat to 110°C, add the monomer solution dropwise, and control the dropping time to 2.5 h; at the same time, add butyl acetate solution (10 mL) containing 0.42 g of azobisisobutyronitrile dropwise, and control the dropping time to 3 h; stir to react for 6 h, cool to obtain a sulfone-amino acrylic resin solution.
[0040] (5) Add 0.5 g KH550 modified zinc oxide, 0.3 g epoxy resin E44 and 0.6 g defoamer (brand EFKA7250) to 100 g sulfone-amino acrylic resin solution, stir and disperse to obtain an aging-resistant acrylic resin waterproof coating.
[0041] Example 3
[0042] (1) Prepare sulfone-amino acrylate monomer according to the method of Example 1.
[0043] (2) Add 15 g of methyl methacrylate, 35 g of butyl acrylate and 5 g of sulfone-amino acrylate monomer to 80 mL of butyl acetate solvent, stir and dissolve to obtain a monomer solution; add 20 mL of butyl acetate solvent to the reaction bottle, introduce nitrogen, heat to 90°C, add the monomer solution dropwise, and control the dropping time to 1.5 h; at the same time, add butyl acetate solution (10 mL) containing 0.47 g of dibenzoyl peroxide dropwise, and control the dropping time to 2 h; stir the reaction for 8 h, cool and obtain a sulfone-amino acrylic resin solution.
[0044] (3) Add 0.5 g KH550 modified zinc oxide, 0.3 g epoxy resin E44 and 0.4 g defoamer (brand EFKA7250) to 100 g sulfone-amino acrylic resin solution, stir and disperse to obtain an aging-resistant acrylic resin waterproof coating.
[0045] Example 4
[0046] (1) Prepare a sulfone-amino acrylic resin solution according to the method of Example 1.
[0047] (2) Add 1.8 g KH550 modified zinc oxide, 1 g epoxy resin E44, and 0.6 g defoamer (brand EFKA7250) to 100 g sulfone-amino acrylic resin solution, stir and disperse to obtain an aging-resistant acrylic resin waterproof coating.
[0048] Example 5
[0049] (1) Prepare a sulfone-amino acrylic resin solution according to the method of Example 1.
[0050] (2) Add 3g KH550 modified zinc oxide, 2g epoxy resin E44 and 0.6g defoamer (brand EFKA7250) to 100g sulfone-amino acrylic resin solution, stir and disperse to obtain an aging-resistant acrylic resin waterproof coating.
[0051] Comparative Example 1
[0052] (1) Prepare a sulfone-amino acrylic resin solution according to the method of Example 1.
[0053] (2) Add 0.2 g of defoamer (brand EFKA7250) to 100 g of sulfone-containing amino acrylic resin solution, stir and disperse to obtain acrylic resin coating.
[0054] Comparative Example 2
[0055] (1) Prepare a sulfone-amino acrylic resin solution according to the method of Example 1.
[0056] (2) Add 0.5 g KH550 modified zinc oxide and 0.2 g defoamer (brand EFKA7250) to 100 g sulfone-amino acrylic resin solution, stir and disperse to obtain an aging-resistant acrylic resin waterproof coating.
[0057] Comparative Example 3
[0058] (1) Prepare a sulfone-amino acrylic resin solution according to the method of Example 1.
[0059] (2) Add 0.3 g of epoxy resin E44 and 0.2 g of defoamer (brand EFKA7250) to 100 g of sulfone-amino acrylic resin solution, stir and disperse to obtain an aging-resistant acrylic resin waterproof coating.
[0060] Comparative Example 4
[0061] (1) Prepare a sulfone-amino acrylic resin solution according to the method of Example 1.
[0062] (2) Add 0.5 g of nano zinc oxide, 0.3 g of epoxy resin E44, and 0.2 g of defoamer (brand EFKA7250) to 100 g of sulfone-amino acrylic resin solution, stir and disperse, and obtain an aging-resistant acrylic resin waterproof coating.
[0063] Comparative Example 5
[0064] (1) Prepare intermediate 2 according to the method of Example 1. The structural formula is as follows:
[0065] .
[0066] (2) Add 15 g of methyl methacrylate, 35 g of butyl acrylate and 3 g of intermediate 2 to 80 mL of butyl acetate solvent, stir and dissolve to obtain a monomer solution; add 20 mL of butyl acetate solvent to the reaction bottle, introduce nitrogen, heat to 100°C, add the monomer solution dropwise, and control the dropping time to 1.5 h; at the same time, add butyl acetate solution (10 mL) containing 0.47 g of dibenzoyl peroxide dropwise, and control the dropping time to 2 h; stir the reaction for 8 h, cool and obtain a sulfone-containing acrylic resin solution.
[0067] (3) Add 0.5 g KH550 modified zinc oxide, 0.3 g epoxy resin E44 and 0.2 g defoamer (brand EFKA7250) to 100 g sulfone-containing acrylic resin solution, stir and disperse to obtain an aging-resistant acrylic resin waterproof coating.
[0068] Comparative Example 6
[0069] (1) Add 15 g of methyl methacrylate and 35 g of butyl acrylate to 80 mL of butyl acetate solvent, stir and dissolve to obtain a monomer solution; add 20 mL of butyl acetate solvent to a reaction bottle, introduce nitrogen, heat to 100°C, and drop the monomer solution, controlling the dropping time to 1.5 h; at the same time, drop a butyl acetate solution (10 mL) containing 0.47 g of dibenzoyl peroxide, controlling the dropping time to 2 h; stir and react for 8 h, cool, and obtain an acrylic resin solution.
[0070] (2) Add 0.5 g KH550 modified zinc oxide, 0.3 g epoxy resin E44, and 0.2 g defoamer (brand EFKA7250) to 100 g acrylic resin solution, stir and disperse to obtain an aging-resistant acrylic resin waterproof coating.
[0071] The acrylic resin waterproof coating was cured at 80°C for 3 hours, 120°C for 2 hours, and 140°C for 2 hours in sequence to form a cured film.
[0072] The tensile properties of the cured film are tested according to GB / T 1040.1-2018 standard.
[0073] The cured film was placed in a UV accelerated aging tester for 120 hours. The wavelength of the light source was 340nm and the irradiance was 0.76W / (m 2 ×nm), relative humidity is 65%. Then the tensile properties test is carried out.
[0074] Table 1 Test of tensile properties and UV aging resistance of cured film
[0075]
[0076] The cured film was made into a 8cm×8cm×0.5cm sample, weighed, and immersed in water for 48 hours. The film was taken out, the surface moisture was wiped dry, and weighed to calculate the water absorption rate.
[0077] Water absorption rate = (mass of the film after water absorption - mass of the film before water absorption) / mass of the film before water absorption × 100%.
[0078] 6 mg of the cured film was weighed and placed in a thermogravimetric analyzer to perform a thermal property test in a nitrogen atmosphere, with the temperature rising from room temperature to 700° C. at a heating rate of 10° C. / min.
[0079]
[0080] As can be seen from Table 1 and Table 2, Examples 1-5 use sulfone-amino acrylate monomer as a functional monomer, and copolymerize with methyl methacrylate and butyl acrylate to obtain an acrylic resin with an amino group and a heat-resistant diphenyl sulfone structure in the molecular chain, which is used as a film-forming substance for the coating, and KH550 modified zinc oxide and epoxy resin are added as curing cross-linking agents. During the high-temperature curing process, the amino group of the acrylic resin and the amino group on the surface of the modified zinc oxide react with the epoxy resin to undergo a curing cross-linking reaction, and the three are cured and cross-linked, thereby chemically bonding the nano zinc oxide to the acrylic resin molecular chain, enhancing the interface bonding strength and dispersibility between the two, so that the nano zinc oxide plays a good reinforcing role, and improves the tensile strength and elongation at break of the acrylic resin. The nano zinc oxide is evenly dispersed in the acrylic resin matrix, has a strong scattering effect on ultraviolet rays, improves the shielding effect of the coating film on ultraviolet rays, and thus enhances the anti-ultraviolet performance of the film. After the ultraviolet aging experiment, the film still maintains a very high tensile strength and elongation at break.
[0081] By using sulfone-amino acrylate monomer as a functional monomer, the heat-resistant diphenyl sulfone structure is introduced into the acrylic resin molecular chain, which significantly improves the heat resistance of the coating film and exhibits a higher thermal decomposition temperature.
[0082] Epoxy resin is used as a curing cross-linking agent to carry out curing and cross-linking reaction on acrylic resin and KH550 modified zinc oxide, which increases the cross-linking degree of the acrylic resin molecular chain and forms a tight cross-linking network in the film matrix, which is beneficial to reduce the water absorption rate of the film, thereby improving its water resistance and waterproof performance.
[0083] Compared with Example 1, Comparative Example 1 did not add KH550 modified zinc oxide, the tensile strength and elongation at break of the film were low, and the UV resistance was poor. After the UV aging test, the tensile strength and elongation at break of the film decreased significantly. No epoxy resin was added, and no curing and crosslinking reaction with the acrylic resin occurred, and the crosslinking degree of the acrylic resin molecular chain was not increased. The water absorption rate of the film was large, and its water resistance and waterproof performance were poor.
[0084] Comparative Example 2 did not add epoxy resin, the water absorption rate of the film was large, and the water resistance and waterproof performance were poor. However, KH550 modified zinc oxide was added, and the tensile strength and elongation at break were higher than those of Comparative Example 1, and after the UV aging test, the film still maintained a high tensile strength and elongation at break, and had good UV aging resistance.
[0085] Compared with comparative example 1, comparative example 3 did not add KH550 modified zinc oxide, and the tensile strength and elongation at break were lower, and the UV aging resistance was poor. However, epoxy resin was added to cross-link with acrylic resin, which improved the tensile strength to a certain extent, and the water absorption rate was significantly reduced.
[0086] Compared with Example 1, Comparative Example 4 added unmodified nano zinc oxide, which had poor compatibility with acrylic resin, could not be evenly dispersed in the coating film matrix, was easily agglomerated, had poor reinforcing effect on acrylic resin, and had tensile strength and elongation at break compared with Example 1. Moreover, after UV aging test, the decrease in tensile strength and elongation at break of the film was higher than that of Example 1, and the UV aging resistance was poor.
[0087] In Comparative Example 5, intermediate 2 is polymerized with methyl methacrylate and butyl acrylate. The obtained acrylic resin does not contain amino groups and cannot undergo curing and cross-linking reactions with KH550 modified zinc oxide and epoxy resin. The film has a large water absorption rate and poor water resistance and waterproof properties.
[0088] In Comparative Example 6, when preparing acrylic resin, no sulfone-amino acrylate monomer was added, and the obtained acrylic resin did not contain a heat-resistant sulfone structure, had the lowest thermal decomposition temperature, and had poor heat resistance. In addition, the acrylic resin did not contain an amino group and could not undergo a curing and cross-linking reaction with KH550 modified zinc oxide and epoxy resin. The water absorption rate of the film was large, and the water resistance and waterproofing properties were poor.
[0089] The above embodiments only express the preferred implementation modes of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for those of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. An aging-resistant acrylic resin waterproof coating, characterized in that: The aging-resistant acrylic resin waterproof coating comprises the following components in parts by weight: 100 parts of sulfone-amino acrylic resin solution, 0.5-3 parts of KH550 modified zinc oxide, 0.3-2 parts of epoxy resin, and 0.2-0.6 parts of defoaming agent; The preparation method of the sulfone-containing amino acrylic resin solution is: Step A, adding methyl methacrylate, butyl acrylate, and sulfone-amino acrylate monomers to butyl acetate solvent, stirring to dissolve, and obtaining a monomer solution; adding butyl acetate solvent to a reaction bottle, introducing nitrogen, heating to 90-110° C., dropping the monomer solution, dropping the butyl acetate solution containing an initiator, stirring to react for 6-8 hours, and cooling to obtain a sulfone-amino acrylic resin solution; The mass of the sulfone-amino acrylate monomer is 6-10% of the total weight of methyl methacrylate and butyl acrylate; The sulfone-amino acrylate monomer has the structural formula (I) as follows: Formula (I).
2. The aging-resistant acrylic resin waterproof coating according to claim 1, characterized in that: The monomer solution is added dropwise for 1.5-2.5 hours, and the initiator-containing butyl acetate solution is added dropwise for 2-3 hours.
3. The aging-resistant acrylic resin waterproof coating according to claim 2, characterized in that: The initiator is dibenzoyl peroxide or azobisisobutyronitrile.
4. The aging-resistant acrylic resin waterproof coating according to claim 1, characterized in that: The preparation method of the sulfone-amino acrylate monomer is: (1) Add toluene, 3-hydroxy-5-nitrobenzoic acid, pyridine, and 4-benzenesulfonylbenzoyl chloride to a reaction flask, stir and react at 20-35° C. for 6-9 hours, and after the reaction, perform rotary evaporation and separate by column chromatography to obtain intermediate 1; (2) Add toluene, intermediate 1, hydroxyethyl acrylate, and p-toluenesulfonic acid to the reaction flask, heat to 70-90°C, stir and react for 8-14 hours, rotary evaporate, and separate by column chromatography to obtain intermediate 2; (3) Add hydrochloric acid solution and iron powder to the reaction bottle, stir, add intermediate 2 and ethanol at 0-5°C, react for 4-6 hours, extract, and separate by column chromatography to obtain sulfone-amino acrylate monomer.
5. The aging-resistant acrylic resin waterproof coating according to claim 4, characterized in that: In the above (1), the mass of pyridine and 4-benzenesulfonylbenzoyl chloride are 62-70% and 150-165% of the mass of 3-hydroxy-5-nitrobenzoic acid, respectively.
6. The aging-resistant acrylic resin waterproof coating according to claim 4, characterized in that: In the above (2), the mass of hydroxyethyl acrylate and p-toluenesulfonic acid are 28-35% and 2.2-3% of the mass of intermediate 1, respectively.
7. The aging-resistant acrylic resin waterproof coating according to claim 4, characterized in that: In the above (3), the mass fraction of the hydrochloric acid solution is 3-5%.
8. The aging-resistant acrylic resin waterproof coating according to claim 4, characterized in that: In (3), the mass of the iron powder is 36-48% of the mass of the intermediate 2.
9. The aging-resistant acrylic resin waterproof coating according to claim 1, characterized in that: The preparation method of the KH550 modified zinc oxide is as follows: adding ethanol and nano zinc oxide into a reaction bottle, performing ultrasonic dispersion treatment, and then adding KH550, performing centrifugal separation after reaction, washing, and drying to obtain the KH550 modified zinc oxide.