A high specific strength high temperature resistant eutectic high entropy alloy and preparation method thereof
By designing Al-Cr-V-Ni eutectic high-entropy alloy, combining high melting point and low density elements, the problem of insufficient performance of existing materials in high temperature environments is solved, and high entropy eutectic with low density and excellent mechanical properties is achieved Alloys meet the lightweight and high-strength needs in the aerospace field.
Patent Information
- Application Number
- CN202411205285.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-08-30
AI Technical Summary
In the aerospace field, existing materials such as titanium alloys and nickel alloys are insufficient in high temperature environments, refractory high entropy alloys have high density and difficult preparation, making it difficult to meet the needs of lightweight, high strength and high temperature resistance.
An Al-Cr-V-Ni eutectic high-entropy alloy was designed, using high melting point elements Ni and Cr and low density elements Al and V, and designed sub-eutectic, complete eutectic and supereutectic structures by controlling the molar ratio. The vacuum arc smelting process is used to combine low density and excellent mechanical properties.
High specific strength eutectic high entropy alloys with low density, high room temperature and high yield strength are achieved, avoiding casting defects, and significantly improving the application potential of materials in the aerospace field.
Smart Images

Figure CN118703862B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of lightweight, high-temperature-resistant high-entropy alloy materials, and specifically relates to a high-specific-strength, high-temperature-resistant eutectic high-entropy alloy and a preparation method thereof. Background Art
[0002] In the aerospace field, lightweight materials with excellent performance are needed to promote the high-quality development of the aerospace industry. High performance and lightweight are two indispensable indicators. Titanium alloy is one of the most widely used materials in the aerospace field. It not only has a low density (about 4.5g·cm -3 ) also has high strength and good heat resistance. It is used as the cold end fan and compressor blades, skeletons, skins, fuselage bulkheads, landing gear and other structural parts of the engine. It is known as "space metal". However, some titanium alloys such as Ti-6Al-4V alloy are not resistant to high temperatures and are only suitable for structural parts in medium and low temperature environments. Although some titanium alloys such as TiAl alloys have good high temperature resistance, their toughness at room temperature is poor. Another material that is widely used in the aerospace field is nickel alloys. Nickel-based high-temperature alloys are key hot end component materials for aircraft engines, spacecraft and rocket engines, and the demand accounts for 80% of the proportion of high-temperature alloys. However, the density of nickel alloys is 8g·cm -3 As a result, its specific yield strength and specific hardness are not superior, only 150MPa·(g·cm -3 ) -1 and 550MPa·(g·cm -3 ) -1 , which limits its application to a certain extent.
[0003] The emergence of high entropy alloys has broken the composition and performance limitations of traditional single-principal alloys. The multi-component effect enables them to have better room and high temperature mechanical properties, wear resistance, corrosion resistance, and oxidation resistance than traditional alloys. Among them, refractory high entropy alloys have good mechanical properties and high temperature resistance, and are expected to be comparable to traditional alloys in the aerospace field. For example, the high entropy alloy TaHfNbZr has a hardness of 3.57GPa and a yield strength of 1315MPa under compression, showing excellent performance. However, the alloy contains too many heavy elements (such as Ta, Hf, and Nb), resulting in a high density (11.04g·cm -3 ), which seriously hinders its development and application in the aerospace field. The aerospace field requires not only materials with excellent mechanical properties, but also as light as possible. Moreover, refractory high-entropy alloys contain two or more refractory elements, and the preparation process is difficult to control, which is prone to casting defects. Summary of the invention
[0004] In view of the deficiencies of the above-mentioned technologies, the present invention provides a high-specific-strength, high-temperature-resistant eutectic high-entropy alloy and a preparation method thereof. With high-melting-point elements Ni and Cr, and low-density elements Al and V as main elements, an Al-Cr-V-Ni eutectic high-entropy alloy is designed. The eutectic high-entropy alloy has a relatively low density, and has both the high-temperature resistance required by the aerospace field and good room-temperature strength and plasticity, providing a new lightweight, high-temperature-resistant eutectic high-entropy alloy alternative material for the aerospace field.
[0005] In order to achieve the above object, the technical solution of the present invention is as follows:
[0006] On the one hand, the present invention provides a high specific strength and high temperature resistant eutectic high entropy alloy, the chemical formula of the eutectic high entropy alloy is Al x CrV y , wherein 0.75≤x≤1.5, 1.3≤y≤2.5, and x and y are molar percentages.
[0007] Another aspect of the present invention provides a method for preparing the above-mentioned high-specific-strength, high-temperature-resistant eutectic high-entropy alloy, the method comprising the following steps:
[0008] (1) preparing Ni, Al, Cr and V raw materials according to atomic percentage;
[0009] (2) placing the raw materials prepared in step (1) into a smelting furnace for smelting, protecting with high-purity argon gas, and obtaining the eutectic high entropy alloy after cooling.
[0010] In the above technical solution, further, in step (1), the purity of the Ni, Al, Cr, and V raw materials is ≥99.95%.
[0011] In the above technical solution, further, in step (2), the smelting method is: evacuating the smelting furnace to a vacuum of 6×10 -3 After reaching Pa, high-purity argon is backfilled to make the gas pressure in the furnace 0.05MPa. The current during smelting is 450-550A and the smelting time is 2-4min.
[0012] In the above technical solution, further, in step (2), during smelting, the alloy ingot is turned over and smelted repeatedly for 5 times to ensure uniform composition.
[0013] In the above technical solution, further, in step (2), Al, Ni, Cr, and V raw materials are placed in the smelting furnace from bottom to top in order according to the melting points of the elements from low to high.
[0014] The beneficial effects of the present invention are:
[0015] 1. The present invention provides a high-specific strength and high-temperature resistant eutectic high-entropy alloy. The elements Al, Cr, and V that have a binary eutectic point with Ni are selected, and an Al-Cr-V-Ni high-entropy alloy system with hypoeutectic, complete eutectic, and hypereutectic structures is designed by controlling the molar ratio.
[0016] 2. The eutectic high entropy alloy of the present invention has a relatively low density (5.60-6.50 g·cm -3 ), which is higher than the existing traditional alloys and refractory high entropy alloys (density of 8.00 g·cm -3 The prepared Al-V-Cr-Ni high entropy alloy has an excellent room temperature specific yield strength of 271-348 MPa·(g·cm -3 ) -1 (Currently, the room temperature specific yield strength of lightweight high entropy alloys and eutectic high entropy alloys is 55-246.29MPa·(g·cm -3 ) -1 ), and excellent high temperature specific yield strength, reaching 158-174MPa·(g·cm -3 ) -1 (Currently, the high temperature specific yield strength of lightweight high entropy alloys and eutectic high entropy alloys is between 45-150MPa·(g·cm -3 ) -1 ).
[0017] In summary, the present invention provides a high-specific-strength, high-temperature-resistant eutectic high-entropy alloy and a preparation method thereof. The alloy not only has the excellent yield strength and hardness of refractory high-entropy alloys, but also has the advantages of eutectic high-entropy alloys. Due to good fluidity during the synthesis process, casting defects are not prone to occur. Therefore, the alloy combines the advantages of lightweight with the advantages of eutectic and refractory high-entropy alloys, and shows great application potential in the field of aerospace. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 XRD patterns of high entropy alloys prepared in Examples 1, 2, 5, and 6;
[0019] Figure 2 XRD patterns of high entropy alloys prepared in Examples 3, 4, and 7;
[0020] Figure 3 This is a metallographic image of the high entropy alloy prepared in Example 1;
[0021] Figure 4 A metallographic image of the high entropy alloy prepared in Example 4;
[0022] Figure 5 The SEM and EDS element distribution results of the entropy alloy prepared in Example 2;
[0023] Figure 6 The SEM and EDS element distribution results of the high entropy alloy prepared in Example 3;
[0024] Figure 7 TEM images of the high entropy alloy prepared in Example 2, a is a TEM image, b is a selected electron diffraction pattern of the area marked with "1", and c is a selected electron diffraction pattern of the area marked with "2";
[0025] Figure 8 TEM images of the high entropy alloy prepared in Example 3, a is a TEM image, b is a selected electron diffraction pattern of the area marked with "1", and c is a selected electron diffraction pattern of the area marked with "2";
[0026] Fig. 9 DSC curve of the high entropy alloy prepared in Example 2;
[0027] Fig.10 DSC curve of the high entropy alloy prepared in Example 3;
[0028] Fig.11 The compressive engineering stress-strain curves of the high entropy alloys prepared in Examples 1-7;
[0029] Fig.12 A comparison chart of the specific yield strength of Examples 1-7 and other representative high entropy alloys and traditional alloys at room temperature;
[0030] Fig.13 The compressive engineering stress-strain curve of the high entropy alloy prepared in Example 3 at a high temperature of 800°C;
[0031] Fig.14 800°C high temperature compression engineering stress-strain curve of the high entropy alloy prepared in Example 4;
[0032] Fig.15 The compressive engineering stress-strain curve of the high entropy alloy prepared in Example 3 at a high temperature of 1000°C;
[0033] Fig.16 The compressive engineering stress-strain curve of the high entropy alloy prepared in Example 4 at a high temperature of 1000°C;
[0034] Fig.17 This is a comparison chart of the specific yield strength of the high entropy alloy prepared in Example 3-4 and other lightweight high entropy alloys, eutectic high entropy alloys and traditional alloys at high temperatures. DETAILED DESCRIPTION
[0035] The following examples may enable those skilled in the art to more fully understand the present invention, but are not intended to limit the present invention in any way.
[0036] Example 1
[0037] A high specific strength and high temperature resistant hypoeutectic high entropy alloy, the chemical formula of which is AlCrVNi 1.5 .
[0038] The above AlCrVNi 1.5 The method for preparing the alloy comprises the following steps:
[0039] (1) Ni, Al, Cr, and V raw materials are prepared according to atomic percentage, and the shapes are all small particles or flakes that are easy to proportion and weigh, and the purity of each element is ≥99.95%;
[0040] (2) The raw materials prepared in step (1) were placed into a water-cooled copper crucible in the order of Al, Ni, Cr, and V from bottom to top in a vacuum arc melting furnace, and the vacuum was evacuated to 6×10 -3 After Pa, high-purity argon gas is backfilled to make the gas pressure in the furnace 0.05MPa, and smelting is carried out under the Ar gas protection atmosphere. The current during smelting is 450-550A, and the smelting time is 2-4min. During smelting, the alloy ingot is turned over after each smelting, and the smelting is continued. The smelting is repeated 5 times to ensure that the composition of the cast alloy is uniform. AlCrVNi is obtained after cooling. 1.5 Hypoeutectic high entropy alloy.
[0041] Example 2
[0042] A high-specific-strength, high-temperature-resistant, fully eutectic high-entropy alloy with the chemical formula AlCrVNi 1.7 .
[0043] The above AlCrVNi 1.7 The method for preparing the alloy comprises the following steps:
[0044] (1) Ni, Al, Cr, and V raw materials are prepared according to atomic percentage, and the shapes are all small particles or flakes that are easy to proportion and weigh, and the purity of each element is ≥99.95%;
[0045] (2) The raw materials prepared in step (1) were placed into a water-cooled copper crucible in the order of Al, Ni, Cr, and V from bottom to top in a vacuum arc melting furnace, and the vacuum was evacuated to 6×10 -3 After Pa, high-purity argon gas is backfilled to make the gas pressure in the furnace 0.05MPa, and smelting is carried out under the Ar gas protection atmosphere. The current during smelting is 450-550A, and the smelting time is 2-4min. During smelting, the alloy ingot is turned over after each smelting, and the smelting is continued. The smelting is repeated 5 times to ensure that the composition of the cast alloy is uniform. AlCrVNi is obtained after cooling. 1.7 Eutectic high entropy alloy.
[0046] Example 3
[0047] A high-specific-strength, high-temperature-resistant, fully eutectic high-entropy alloy, whose chemical formula is Al 1.37 CrV 1.5 .
[0048] The above Al 1.37 CrV 1.5 The method for preparing the alloy comprises the following steps:
[0049] (1) Ni, Al, Cr, and V raw materials are prepared according to atomic percentage, and the shapes are all small particles or flakes that are easy to proportion and weigh, and the purity of each element is ≥99.95%;
[0050] (2) The raw materials prepared in step (1) were placed into a water-cooled copper crucible in the order of Al, Ni, Cr, and V from bottom to top in a vacuum arc melting furnace, and the vacuum was evacuated to 6×10 -3 After 3000 Pa, high-purity argon gas was backfilled to make the gas pressure in the furnace 0.05MPa. Smelting was carried out under the Ar gas protection atmosphere. The current during smelting was 450-550A and the smelting time was 2-4min. During smelting, the alloy ingot was turned over after each smelting and smelting was continued. The smelting was repeated 5 times to ensure that the composition of the cast alloy was uniform. Al 1.37 CrV 1.5 Completely eutectic high entropy alloy.
[0051] Example 4
[0052] A high specific strength and high temperature resistant hypereutectic high entropy alloy, whose chemical formula is Al 1.5 CrV 1.5 .
[0053] The above Al 1.5 CrV 1.5 The method for preparing the alloy comprises the following steps:
[0054] (1) Ni, Al, Cr, and V raw materials are prepared according to atomic percentage, and the shapes are all small particles or flakes that are easy to proportion and weigh, and the purity of each element is ≥99.95%;
[0055] (2) The raw materials prepared in step (1) were placed into a water-cooled copper crucible in the order of Al, Ni, Cr, and V from bottom to top in a vacuum arc melting furnace, and the vacuum was evacuated to 6×10 -3 After 3000 Pa, high-purity argon gas was backfilled to make the gas pressure in the furnace 0.05MPa. Smelting was carried out under the Ar gas protection atmosphere. The current during smelting was 450-550A and the smelting time was 2-4min. During smelting, the alloy ingot was turned over after each smelting and smelting was continued. The smelting was repeated 5 times to ensure that the composition of the cast alloy was uniform. Al 1.5CrV 1.5 Hypereutectic high entropy alloy.
[0056] Example 5
[0057] A high specific strength and high temperature resistant hypoeutectic high entropy alloy, the chemical formula of which is AlCrVNi 1.3 .
[0058] The above AlCrVNi 1.3 The method for preparing the alloy comprises the following steps:
[0059] (1) Ni, Al, Cr, and V raw materials are prepared according to atomic percentage, and the shapes are all small particles or flakes that are easy to proportion and weigh, and the purity of each element is ≥99.95%;
[0060] (2) The raw materials prepared in step (1) were placed into a water-cooled copper crucible in the order of Al, Ni, Cr, and V from bottom to top in a vacuum arc melting furnace, and the vacuum was evacuated to 6×10 -3 After Pa, high-purity argon gas is backfilled to make the gas pressure in the furnace 0.05MPa, and smelting is carried out under the Ar gas protection atmosphere. The current during smelting is 450-550A, and the smelting time is 2-4min. During smelting, the alloy ingot is turned over after each smelting, and the smelting is continued. The smelting is repeated 5 times to ensure that the composition of the cast alloy is uniform. AlCrVNi is obtained after cooling. 1.3 Hypoeutectic high entropy alloy.
[0061] Example 6
[0062] A high specific strength and high temperature resistant hypereutectic high entropy alloy, the chemical formula of which is AlCrVNi 2.5 .
[0063] The above AlCrVNi 2.5 The method for preparing the alloy comprises the following steps:
[0064] (1) Ni, Al, Cr, and V raw materials are prepared according to atomic percentage, and the shapes are all small particles or flakes that are easy to proportion and weigh, and the purity of each element is ≥99.95%;
[0065] (2) The raw materials prepared in step (1) were placed into a water-cooled copper crucible in the order of Al, Ni, Cr, and V from bottom to top in a vacuum arc melting furnace, and the vacuum was evacuated to 6×10 -3 After Pa, high-purity argon gas is backfilled to make the gas pressure in the furnace 0.05MPa, and smelting is carried out under the Ar gas protection atmosphere. The current during smelting is 450-550A, and the smelting time is 2-4min. During smelting, the alloy ingot is turned over after each smelting, and the smelting is continued. The smelting is repeated 5 times to ensure that the composition of the cast alloy is uniform. AlCrVNi is obtained after cooling. 2.5Hypereutectic high entropy alloy.
[0066] Example 7
[0067] A high specific strength and high temperature resistant hypoeutectic high entropy alloy, whose chemical formula is Al 0.75 CrV 1.5 .
[0068] The above Al 0.75 CrV 1.5 The method for preparing the alloy comprises the following steps:
[0069] (1) Ni, Al, Cr, and V raw materials are prepared according to atomic percentage, and the shapes are all small particles or flakes that are easy to proportion and weigh, and the purity of each element is ≥99.95%;
[0070] (2) The raw materials prepared in step (1) were placed into a water-cooled copper crucible in the order of Al, Ni, Cr, and V from bottom to top in a vacuum arc melting furnace, and the vacuum was evacuated to 6×10 -3 After 3000 Pa, high-purity argon gas was backfilled to make the gas pressure in the furnace 0.05MPa. Smelting was carried out under the Ar gas protection atmosphere. The current during smelting was 450-550A and the smelting time was 2-4min. During smelting, the alloy ingot was turned over after each smelting and smelting was continued. The smelting was repeated 5 times to ensure that the composition of the cast alloy was uniform. Al 0.75 CrV 1.5 Hypoeutectic high entropy alloy.
[0071] Test results:
[0072] (I) XRD test
[0073] The XRD test was conducted by cutting parallel blocks of about 5 mm thick from the smelted alloy using wire cutting, and the surface was carefully polished with sandpaper. The blocks were then placed in industrial ethanol and cleaned with ultrasonic vibration. The phase composition of the alloy was then analyzed using D8 Bruker X-ray diffraction, Cu Kα radiation, a scanning speed of 4° / min, and a scanning range of 20° to 100°.
[0074] The present invention takes the high entropy alloy prepared in Examples 1-4 as an example, and performs XRD tests on them respectively. The test results are as follows: Figure 1-2 shown.
[0075] in, Figure 1 From the XRD patterns of the high entropy alloys prepared in Examples 1, 2, 5, and 6, it can be seen that they are composed of an ordered L21 phase and a disordered BCC phase, and weak low-angle superlattice diffraction peaks appear at 2θ of 26.8° and 30.8°, indicating the formation of the L21 phase. Figure 2From the XRD patterns of the high entropy alloys prepared in Examples 3, 4 and 7, it can be seen that the high entropy alloys are composed of an ordered B2 phase and a disordered BCC phase, and the presence of a small (100) superlattice diffraction peak indicates the formation of an ordered B2 phase.
[0076] (II) Tissue characterization test
[0077] 1. Metallographic picture test
[0078] The microstructure of the alloy was analyzed by an optical microscope (OM, IMM 5000). The sample size was a rectangular sample with a length, width and height of 10×10×5mm. The test surface was carefully ground and polished with sandpaper, then placed in anhydrous ethanol and cleaned with ultrasonic vibration and blown dry. Before the test, the metallographic etching solution was used for corrosion, and the volume ratio of the etching solution was HF:HNO3:H2O=1:2:6. After corrosion for 5-10s, it was rinsed with anhydrous ethanol and blown dry.
[0079] The present invention takes the high entropy alloys prepared in Example 1 and Example 4 as examples, and performs metallographic tests on them respectively. The test results are as follows: Figure 3-4 shown.
[0080] Figure 3 The high entropy alloy AlCrVNi prepared in Example 1 1.5 The metallographic picture at the 10μm scale shows a hypoeutectic structure.
[0081] Figure 4 The high entropy alloy Al prepared in Example 4 1.5 CrV 1.5 From the metallographic image at 10μm scale, it can be seen that it is a hypereutectic structure.
[0082] 2. Scanning electron microscope test
[0083] The microstructure of the alloy was analyzed by scanning electron microscopy (SEM, Suparr 55). The sample processing was consistent with the sample processing in the above metallographic test.
[0084] The present invention takes the high entropy alloys prepared in Example 2 and Example 3 as examples, and performs SEM and EDS element distribution tests on them respectively. The test results are as follows: Figure 5-6 shown.
[0085] Figure 5 AlCrVNi prepared in Example 2 1.7 SEM image of high entropy alloy at 10μm scale. It can be seen that AlCrVNi 1.7The morphology of the high entropy alloy is a fine-grained center with a strip-shaped eutectic pattern extending from the inside to the outside, forming a eutectic structure with a sunflower or chrysanthemum pattern. The EDS distribution results show that Ni and Al elements are enriched in the L21 phase, and V and Cr elements are enriched in the BCC phase.
[0086] Figure 6 Al prepared in Example 3 1.37 CrV 1.5 SEM image of high entropy alloy at 10μm scale. It can be seen that Al 1.37 CrV 1.5 The high entropy alloy also presents a eutectic morphology, but it is slightly different from the eutectic morphology of Example 1. Example 3 is a dense coarse granular structure in the middle, and a divergent seaweed-like eutectic structure is formed from the inside to the outside. The EDS distribution results show that in the eutectic structure, Ni and Al elements are enriched in the B2 phase, and V and Cr elements are enriched in the BCC phase. The change from the dense and coarse seaweed-like eutectic structure composed of the L21 phase and the BCC phase in Example 1 to the sunflower or chrysanthemum pattern eutectic structure composed of the B2 phase and the BCC in Example 3 also illustrates that the present invention proposes that the alloy microstructure can be regulated by adjusting the content of the Al and Ni elements to obtain a high entropy alloy with excellent performance.
[0087] 3. Transmission electron microscopy test
[0088] The microstructure of the alloy was analyzed by transmission electron microscopy (TEM, JEM-F200). First, a block with a length, width and height of 5×5×0.3mm was cut from the smelted alloy by wire cutting, and it was carefully polished with sandpaper to a thickness of less than 50μm. Then, a small disc with a diameter of Φ3mm was punched out with a punching machine, and then a mixture of 90% ethanol and 10% perchloric acid (volume fraction) was used for electrolytic double spray thinning, and the obtained sample was used for TEM testing.
[0089] The present invention takes the high entropy alloys prepared in Example 2 and Example 3 as examples, and performs TEM tests on them respectively. The test results are as follows: Figure 7-8 shown.
[0090] Figure 7 AlCrVNi prepared in Example 2 1.7 TEM image of a high entropy alloy, Figure 7 a It can be seen that the sunflower-shaped eutectic structure in Example 1 is composed of regular stripes, and many nano-precipitated phases appear in the black stripes. Figure 7 b is Figure 7 The selected electron diffraction pattern of the area marked with “1” in a, that is, the black stripe area, indicates that the black stripes are a BCC structure. Figure 7 c is Figure 7The selected electron diffraction pattern of the area marked with "2" in a, that is, the white stripe area, indicates that the white stripes are L21 structures.
[0091] Figure 8 Al prepared in Example 3 1.37 CrV 1.5 TEM image of a high entropy alloy, Figure 8 a It can be seen that the seaweed-like eutectic structure in Example 3 is composed of regular wavy stripes, and many nano-precipitated phases appear in the white stripes. Figure 8 b is Figure 8 The selected electron diffraction pattern of the area marked with “1” in a, that is, the black stripe area, indicates that the black stripes are a BCC structure. Figure 8 c is Figure 8 The selected electron diffraction pattern of the area marked with "2" in a, that is, the white stripe area, indicates that the white stripes are B2 structures.
[0092] (III) DSC test
[0093] The thermal behavior of the sample was analyzed by using a NETZSCH differential scanning calorimeter (DSC 449F3) at a rate of 20 K / min in flowing argon.
[0094] The present invention takes the high entropy alloys prepared in Example 1 and Example 2 as examples, and performs DSC tests on them respectively. The test results are as follows: Figure 9-10 shown.
[0095] Fig. 9 This is the DSC curve of Example 2. It can be seen that only one obvious exothermic peak is observed in the heating process, and only one endothermic peak is observed in the cooling process, which is consistent with the characteristics of eutectic solidification.
[0096] Fig.10 This is the DSC curve of Example 3. In the curve, only one obvious exothermic peak is observed during the heating process, and only one endothermic peak is observed during the cooling process, which is consistent with the characteristics of eutectic solidification.
[0097] (IV) Mechanical properties test
[0098] 1. Mechanical properties at room temperature
[0099] The compression test at room temperature was performed by an Instron 5982 testing machine at 1×10 -3 s -1 The samples were obtained from alloy ingots by wire electrospark cutting and were made into bars with a size of Φ5×10 mm. In order to obtain reliable results, all compression tests were carried out 4 times.
[0100] The present invention takes the high entropy alloy prepared in Examples 1-7 as an example, and performs compression test on them respectively. The test results are as follows: Fig.11 shown.
[0101] Fig.11 The room temperature compression engineering stress-strain curves of the high entropy alloys prepared in Examples 1-7 are shown in Figure 1. 1.5 The compressive yield strength of the hypoeutectic high entropy alloy is 1695 MPa, the compressive strength is as high as 3564 MPa, and the plasticity is maintained at 33%. 1.7 The fully eutectic high entropy alloy has a room temperature compressive yield strength of up to 1932MPa, a compressive strength of up to 3745MPa, and maintains 30% of its plasticity. Its mechanical properties are relatively excellent, probably because AlCrVNi 1.7 The semi-coherent strong bonding interface composed of L21 phase and BCC will reduce the cracking tendency of the interface during deformation. Moreover, the nano-precipitated phase in the two-phase eutectic may be hardened through the Orowan dislocation mechanism to achieve the effect of precipitation strengthening. The hypoeutectic high entropy alloy is composed of a small amount of eutectic structure and primary phase, and the primary phase dendrite accounts for a high proportion, resulting in performance that is not as good as that of the eutectic structure. Al prepared in Example 3 1.37 CrV 1.5 The fully eutectic high entropy alloy has a room temperature compressive yield strength of up to 1586MPa, a compressive strength of up to 3604MPa, and maintains 35% of its plasticity. 1.37 CrV 1.5 The high entropy alloy has a completely eutectic structure, with a semi-coherent interface composed of the B2 phase and the BCC phase, and many nanophases are found in the TEM image. These nanophases may interact with dislocations during the compression deformation process to play a reinforcing role, thereby achieving excellent mechanical properties. 1.5 CrV 1.5 High entropy alloy, its room temperature compressive yield strength is as high as 1521MPa, compressive strength is as high as 3522MPa, and maintains 36% plasticity. 1.5 CrV 1.5 The high entropy alloy is a hypereutectic structure, which is composed of many brittle B2 primary phases, resulting in performance that is not as good as that of a complete eutectic structure. 1.3 The high entropy alloy has a room temperature compressive yield strength of up to 1795 MPa, a compressive strength of up to 3103 MPa, and maintains 24% of its plasticity. 2.5 The high entropy alloy has a room temperature compressive yield strength of up to 2286 MPa, a compressive strength of up to 3050 MPa, and maintains 13% plasticity. 0.75 CrV1.5 High entropy alloy, with room temperature compressive yield strength up to 2141MPa, compressive strength up to 2953MPa, and maintains 17% plasticity. Fig.12 The specific yield strength-plasticity of Examples 1-7 at room temperature is compared with other representative high entropy alloys and traditional alloys. It can be seen that the specific yield strength of Examples 1-7 of the present invention is 24%-44% higher than that of traditional titanium alloys, 83%-108% higher than that of nickel alloys, and is better than most reported high entropy alloys, and is expected to become an alternative material in the aerospace field.
[0102] 2. Mechanical properties at high temperature
[0103] The compression test at high temperature was performed by Gleeble-3800 testing machine at 1×10 -3 s -1 The samples were obtained from alloy ingots by wire-cutting with a size of Φ8×12mm. The high temperature mechanical properties were tested at 800 and 1000℃ respectively.
[0104] The present invention takes the high entropy alloy prepared in Example 3-4 as an example, and performs compression test on it respectively. The test results are as follows: Figure 13-17 shown.
[0105] Fig.13 Al prepared in Example 3 1.37 CrV 1.5 Engineering stress-strain curve of high entropy alloy under high temperature compression at 800℃. It can be seen that the compressive yield strength of high entropy alloy at 800℃ is as high as 1010MPa, and the plasticity exceeds 50%. It has good high temperature mechanical properties.
[0106] Fig.14 Al prepared in Example 4 1.5 CrV 1.5 Engineering stress-strain curve of high entropy alloy under high temperature compression at 800°C. It can be seen that the compressive yield strength of high entropy alloy at 800°C is as high as 902MPa, and the plasticity exceeds 50%.
[0107] Fig.15 This is the engineering stress-strain curve of the high entropy alloy prepared in Example 3 under high temperature compression at 1000°C. It can be seen that Al 1.37 CrV 1.5 The compressive yield strength of high entropy alloys at 1000°C is as high as 520MPa, and the plasticity exceeds 50%. It has good high-temperature mechanical properties.
[0108] Fig.16 This is the engineering stress-strain curve of the high entropy alloy prepared in Example 4 under high temperature compression at 1000°C. It can be seen that Al 1.5CrV 1.5 The compressive yield strength of high entropy alloys at 1000°C is as high as 397MPa, and the plasticity exceeds 50%.
[0109] Fig.17 The following is a comparison chart of the specific yield strength of Example 3-4 at different temperatures and that of other similar alloys. It can be seen that the high-temperature specific yield strength of Example 3-4 exceeds that of similar alloys and traditional alloys reported so far, indicating that Example 3-4 has excellent high-temperature mechanical properties.
[0110] The above embodiments are only preferred embodiments of the present invention and are not intended to limit the implementation methods. The protection scope of the present invention shall be subject to the scope defined in the claims. Other different forms of changes or modifications may be made based on the above description. Obvious changes or modifications derived therefrom are still within the protection scope of the present invention.
Claims
1. A high specific strength high temperature resistant eutectic high entropy alloy, characterized in that: The chemical formula of the eutectic high entropy alloy is Al x CrV y , wherein 0.75≤x≤1.5, 1.3≤y≤2.5, x and y are mole percentages; The room temperature specific yield strength of the eutectic high entropy alloy is 271-348 MPa·(g·cm -3 ) -1 , high temperature specific yield strength is 158-174MPa·(g·cm -3 ) -1 .
2. A method for preparing the high specific strength high temperature resistant eutectic high entropy alloy according to claim 1, characterized in that: The method comprises the following steps: (1) preparing Ni, Al, Cr and V raw materials according to atomic percentage; (2) placing the raw materials prepared in step (1) into a smelting furnace for smelting, protecting with high-purity argon gas, and obtaining the eutectic high entropy alloy after cooling.
3. The preparation method according to claim 2, characterized in that: In step (1), the purity of the Ni, Al, Cr and V raw materials is ≥99.95%.
4. The preparation method according to claim 2, characterized in that: In step (2), the smelting method is: evacuate the smelting furnace to a vacuum of 6×10 -3 After reaching Pa, high-purity argon is backfilled to make the gas pressure in the furnace 0.05MPa. The current during smelting is 450-550A and the smelting time is 2-4min.
5. The preparation method according to claim 2, characterized in that: In step (2), during smelting, the alloy ingot is turned over and smelted repeatedly for 5 times.
6. The preparation method according to claim 2, characterized in that: In step (2), Al, Ni, Cr, and V raw materials are placed into the smelting furnace from bottom to top in order according to the melting points of the elements from low to high.