A preparation device and method for aviation-grade vanadium-aluminum master alloy

By using a combination technology of vacuum pump, foam ceramic filter and ultrasonic vibrating rod in the vanadium aluminum intermediate alloy preparation device, the problem of high inclusion content in vanadium aluminum intermediate alloy is solved, and its purity and performance are significantly improved, ensuring the titanium alloy Reliability and durability.

CN118705874BActive Publication Date: 2024-11-26XIAN RARE METAL MATERIALS RES INST CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411178026.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-11-26
Estimated Expiration
2044-08-27

AI Technical Summary

Technical Problem

The prior art is difficult to effectively reduce the inclusion content in vanadium-aluminum intermediate alloys, especially carbide residue problems, which affects the performance of titanium alloys.

Method used

The air in the furnace is extracted by a vacuum pump, combined with a foam ceramic filter and an ultrasonic vibrating rod, to remove inclusions in the melt, reduce gas solubility, and synergistically reduce the content of oxygen, nitrogen and inclusions through the vacuum environment and ultrasonic action.

Benefits of technology

Effectively improve the purity and structure uniformity of vanadium aluminum intermediate alloy, enhance its performance, and ensure the reliability and durability of titanium alloy.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118705874B_ABST
    Figure CN118705874B_ABST
Patent Text Reader

Abstract

The present invention discloses a preparation device for aviation-grade vanadium-aluminum intermediate alloy, comprising a furnace body, a metal thermal reduction reaction mechanism and a melt filtering and collecting mechanism arranged in the furnace body, the furnace body is connected with a vacuum pump, the melt filtering and collecting mechanism comprises a foam ceramic filter screen and an ultrasonic vibration rod penetrating the foam ceramic filter screen, and an electric dumping device is arranged at the bottom of the metal thermal reduction reaction mechanism; the present invention also discloses a preparation method for vanadium-aluminum intermediate alloy, comprising the following steps: step one, raw material pretreatment; step two, preparation of alumina crucible; step three, metal thermal reduction process; step four, impurity removal. The preparation device of the present invention is used to remove gas and inclusions in the melt by arranging a vacuum pump, a foam ceramic filter screen and an ultrasonic vibration rod to obtain a high-purity, highly homogenized vanadium-aluminum intermediate alloy, and the preparation device of the present invention is suitable for preparing intermediate alloys.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of intermediate alloy preparation, and in particular relates to a preparation device and method for an aviation-grade vanadium-aluminum intermediate alloy. Background Art

[0002] Vanadium aluminum master alloy is an important industrial material, mainly used to manufacture aviation-grade high-quality vanadium-containing titanium alloy. With the increasing market requirements for the performance of titanium alloys and high-temperature alloys, the performance indicators of vanadium aluminum master alloys have also increased, especially the control of the content of impurity elements and inclusions such as oxygen, nitrogen, and carbon in the alloy. Reducing the content of these impurity elements and inclusions is crucial to prevent them from having a negative impact on the performance of the final titanium alloy during the preparation process.

[0003] Specifically, although oxygen and nitrogen, as interstitial solid solution forming elements, can improve the hardness of titanium alloys, their excessive presence will reduce the plasticity and toughness of titanium alloys. In addition, although the increase in carbon content helps to improve the strength of titanium alloys, excessive carbon will increase the brittleness of titanium alloys and increase their corrosion sensitivity. At the same time, the presence of inclusions will cause stress concentration, reduce the properties of titanium alloys including strength, toughness and fatigue life, and thus affect the reliability and durability of titanium alloys. Therefore, precise control of the content of impurity elements and inclusions is not only a necessary condition for improving the quality of vanadium-aluminum master alloys, but also a key step towards the development of high-performance titanium alloy materials.

[0004] At present, in order to reduce the content of impurity elements and inclusions in vanadium-aluminum master alloys, the preparation equipment is improved. For example, the Chinese invention patent "Smelting process and vacuum device for reducing oxygen and nitrogen in aerospace-grade high-vanadium aluminum alloy" (publication number CN111733340A) adds a vacuum device to the upper part of the crucible, and extracts the gas in the crucible at the end of the furnace loading reaction, which can effectively reduce the content of impurity elements such as oxygen and nitrogen brought in by the presence of air during the vanadium-aluminum alloy smelting process, but the problem of residual inclusions mainly composed of carbides cannot be solved. Summary of the invention

[0005] The purpose of the present invention is to overcome the deficiencies in the above-mentioned prior art and provide a preparation device for aviation-grade vanadium-aluminum master alloy. The preparation device extracts air from the furnace by setting a vacuum pump, and removes inclusions in the melt by setting a foam ceramic filter and an ultrasonic vibrating rod in direct contact with the melt. The vibration of the ultrasonic vibrating rod and the vacuum pump reduce the solubility of the gas in the melt, which together promote the precipitation of the gas, solving the problem that the prior art device can only reduce the oxygen and nitrogen content in the vanadium-aluminum master alloy, but cannot effectively remove inclusions.

[0006] To achieve the above-mentioned purpose, the technical solution adopted by the present invention is: a preparation device of aviation-grade vanadium-aluminum intermediate alloy, characterized in that it includes a furnace body, a metal thermal reduction reaction mechanism and a melt filtration and collection mechanism arranged in the furnace body, the furnace body is connected to a vacuum pump, the melt filtration and collection mechanism includes a foam ceramic filter screen and an ultrasonic vibration rod penetrating the foam ceramic filter screen, and an electric dumping device is provided at the bottom of the metal thermal reduction reaction mechanism.

[0007] The above-mentioned preparation device of aviation-grade vanadium-aluminum intermediate alloy is characterized in that the melt filtration and collection mechanism also includes a second alumina crucible, the foam ceramic filter is arranged at the upper end inside the second alumina crucible, and the ultrasonic tool head of the ultrasonic vibration rod is made of ceramic material.

[0008] The above-mentioned device for preparing aviation-grade vanadium-aluminum master alloy is characterized in that the metal thermal reduction reaction mechanism includes a first alumina crucible and a heating and ignition device extending into the first alumina crucible.

[0009] The above-mentioned preparation device of aviation-grade vanadium-aluminum intermediate alloy is characterized in that a guide groove is provided between the first alumina crucible and the melt filtration and collection mechanism, which is used to guide the melt in the first alumina crucible into the melt filtration and collection mechanism, and the guide groove includes a steel shell layer, a refractory brick layer arranged above the steel shell layer, and an alumina layer arranged above the refractory brick layer, and the alumina layer is also filled in the gap of the refractory brick layer, and the alumina layer is composed of alumina and an adhesive.

[0010] The above-mentioned device for preparing aviation-grade vanadium-aluminum intermediate alloy is characterized in that the furnace body is a double-layer water-cooled jacket structure consisting of the inner wall of the furnace body and a jacket fixedly installed outside the inner wall of the furnace body, and circulating water is passed into the jacket.

[0011] The present invention also discloses a method for preparing aviation-grade vanadium-aluminum master alloy by using the above device, characterized in that the method comprises the following steps:

[0012] Step 1: Raw material pretreatment: drying vanadium pentoxide powder, aluminum particles, calcium fluoride and calcium oxide in an oven, and then mixing them in a mixer to obtain raw materials;

[0013] Step 2, preparing an alumina crucible: mixing aluminum oxide and sodium carbonate evenly, shaping them into a shape, and then sintering them to obtain an alumina crucible; the alumina crucible includes a first alumina crucible and a second alumina crucible;

[0014] Step 3, metal thermal reduction process: put the raw materials mixed in step 1 into the first alumina crucible obtained in step 2, contact the heating ignition device with the raw materials, start the vacuum pump to evacuate to below -0.1MPa and turn off the vacuum pump, then start the heating ignition device to induce metal thermal reduction reaction to obtain a melt;

[0015] Step 4, impurity removal: start the vacuum pump and control the electric dumping equipment, pour the melt obtained in step 3 into the second alumina crucible through the foam ceramic filter, start the ultrasonic vibrator to remove impurities, and turn off the ultrasonic vibrator and vacuum pump after the melt is cooled to obtain a vanadium aluminum intermediate alloy.

[0016] The present invention is used to completely remove moisture in the raw materials by drying the raw materials, thereby avoiding adverse effects caused by the presence of moisture in the subsequent metal thermal reduction reaction, such as reducing the reaction rate, introducing impurities, etc.

[0017] During the melt cooling process of the present invention, a part of the melt will adhere to the ultrasonic tool head. However, the chemical reaction between the melt and the ultrasonic tool head made of ceramic material is limited, and the bonding force of the contact surface between the two is relatively weak. In addition, due to the significant difference in thermal expansion coefficients between the vanadium-aluminum master alloy and the ceramic, the shrinkage speed and degree of the vanadium-aluminum master alloy during solidification are not synchronized with the ultrasonic tool head, resulting in thermal stress at the interface between the vanadium-aluminum master alloy and the ceramic, thereby inducing the generation of cracks inside the vanadium-aluminum master alloy, and even breaking it, so that the vanadium-aluminum master alloy can easily fall off from the surface of the tool head.

[0018] The above-mentioned method for preparing an aviation-grade vanadium-aluminum master alloy is characterized in that the mass purity of the vanadium pentoxide powder in step one is not less than 99.9%, the mass purity of the aluminum particles is not less than 99.9%, the D50 particle size ratio of the vanadium pentoxide powder to the aluminum particles is 1:1~1:2, and the calcium fluoride and calcium oxide are both analytically pure.

[0019] The present invention controls the D50 particle size ratio of vanadium pentoxide powder to aluminum particles to be 1:1-1:2. Under the condition of the particle size ratio, the stacking effect of the powder is optimal, which is beneficial to improving the ignition success rate. In addition, since aluminum has a low melting point, it can be melted first and fully contacted with the vanadium pentoxide powder, thereby improving the reaction efficiency and success rate.

[0020] The above-mentioned method for preparing an aviation-grade vanadium-aluminum intermediate alloy is characterized in that the aluminum oxide described in step 2 is composed of aluminum oxide with a particle size of 3mm~5mm, 1mm~3mm, 0.3mm~1mm and less than 0.3mm in a mass ratio of 1:2:3:4; the sintering system is: heating to 20℃~25℃ and keeping warm for 25min, then heating to 200℃ and keeping warm for 25min, heating to 200℃~700℃ and keeping warm for 100min, heating to 700℃~900℃ and keeping warm for 60min, and then turning off the furnace and cooling for 60min.

[0021] The present invention sets the mixing ratio of alumina with different particle sizes so that the alumina reaches the maximum packing density, thereby making the alumina crucible have better thermal insulation performance, reducing heat loss during the thermal reduction reaction, and improving the efficiency of the thermal reduction reaction; by adopting a multi-stage sintering process to prepare the alumina crucible, it is possible to prevent the crucible blank from cracking due to thermal stress during the rapid heating process, improve the density and mechanical properties of the alumina crucible, and make the internal grains more uniform.

[0022] The specific functions of the temperature and insulation time settings in each stage are as follows: heating to 20℃~25℃ and insulation for 25 minutes can make the temperature of the entire blank uniform and avoid the temperature gradient and stress formation in various parts of the crucible blank in the initial stage; heating to 200℃ and insulation for 25 minutes is used to decompose and volatilize the organic matter in the blank. The insulation process helps to ensure that the organic matter is completely volatilized and prevent the sudden decomposition of the organic matter during subsequent heating to cause the blank to crack; heating to 200℃~700℃ and insulation for 100 minutes is used to further remove organic matter and other volatile impurities, reduce internal defects of the crucible blank, and make the aluminum oxide particles initially melt and begin to form preliminary connections between the aluminum oxide particles; heating to 700℃~900℃ and insulation for 60 minutes is used to further sinter the aluminum oxide particles to form a dense structure. At the same time, the insulation time is short to prevent excessive growth of grains; furnace cooling for 60 minutes, slow cooling in the furnace helps to reduce the thermal stress inside the crucible and eventually form a stable structure.

[0023] The above-mentioned method for preparing an aviation-grade vanadium-aluminum master alloy is characterized in that the vanadium-aluminum master alloy in step 4 is composed of the following elements in percentage by mass: V 55%~88%, Fe not more than 0.20%, Si not more than 0.20%, C not more than 0.02%, O not more than 0.02%, N not more than 0.01%, and the balance is Al.

[0024] The above-mentioned method for preparing aviation-grade vanadium-aluminum master alloy is characterized in that the vanadium-aluminum master alloy in step 4 is sandblasted and finished, and then crushed and screened in sequence to obtain vanadium-aluminum master alloy particles, and the vanadium-aluminum master alloy particles are stored after manual selection and sampling inspection.

[0025] Compared with the prior art, the present invention has the following advantages:

[0026] 1. The present invention adopts a foam ceramic filter and an ultrasonic vibrator to remove inclusions in the melt. The foam ceramic filter has a unique porous structure to filter out larger inclusions. Then, the ultrasonic vibrator is in direct contact with the melt, and the cavitation effect, stirring and dispersing effect, degassing effect and cleaning effect of the ultrasonic wave are utilized to further reduce the content of inclusions and gas, thereby improving the purity of the melt. While the ultrasonic wave is acting, the vacuum pump has already extracted the air in the furnace, so that the removal of inclusions is carried out in a vacuum environment, which can effectively reduce the solubility of the gas in the melt, and cooperate with the ultrasonic wave to promote the precipitation of the gas. Combining vacuum degassing, foam ceramic filter and ultrasonic technology, the oxygen, nitrogen and inclusion contents in the vanadium-aluminum alloy are synergistically reduced, and the purity and structural uniformity of the vanadium-aluminum master alloy are effectively improved.

[0027] 2. The present invention adopts a crucible made of alumina as a container for thermal reduction reaction and melt filtering and solidification, thereby ensuring that no reaction occurs between the melt and the container, thereby improving the purity of the vanadium-aluminum master alloy; since alumina has low thermal conductivity and good thermal insulation properties, it helps to prolong the duration of the high-temperature molten state of the melt, improve the fluidity of the slag in the melt to improve the separation efficiency of the slag and the melt, thereby ensuring the purity of the vanadium-aluminum master alloy.

[0028] 3. The present invention helps to improve the efficiency and success rate of the thermal reduction reaction by controlling the particle size ratio of vanadium pentoxide powder to aluminum particles.

[0029] 4. The present invention controls the mixing ratio of alumina with different particle sizes and adopts a multi-stage sintering process to prepare an alumina crucible, thereby preventing the crucible from cracking due to thermal stress during rapid heating, ensuring the integrity of the alumina crucible during the high-temperature reaction of preparing a vanadium-aluminum intermediate alloy, reducing the contact area between the melt and the crucible, and reducing the probability of impurities being introduced; at the same time, the density and mechanical properties of the alumina crucible are improved, and the internal grains are made more uniform, so that the alumina crucible has better thermal insulation performance, thereby improving the efficiency of thermal reduction reaction and impurity removal. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 It is a schematic diagram of the structure of the preparation device of the present invention.

[0031] Figure 2 This is a scanning electron microscope image of the Al-55wt.%V master alloy prepared in Example 2 of the present invention.

[0032] Figure 3 This is a scanning diagram of the aluminum element energy spectrum of the Al-55wt.%V master alloy prepared in Example 2 of the present invention.

[0033] Figure 4 This is a scanning diagram of the vanadium element energy spectrum of the Al-55wt.%V master alloy prepared in Example 2 of the present invention.

[0034] Figure 5 This is a scanning electron microscope image of the Al-65wt.%V intermediate alloy prepared in Example 3 of the present invention.

[0035] Description of reference numerals:

[0036] 1—vacuum pump; 2—furnace body; 3—foam ceramic filter; 4—ultrasonic vibration rod; 5—electric dumping equipment; 6—first alumina crucible; 7—heating and ignition device; 8—second alumina crucible. DETAILED DESCRIPTION

[0037] The preparation device of the aviation-grade vanadium-aluminum master alloy of the present invention is described in detail through Example 1.

[0038] Example 1

[0039] like Figure 1 As shown, the preparation device of this embodiment includes a furnace body 2, a metal thermal reduction reaction mechanism and a melt filtration and collection mechanism arranged in the furnace body 2, the furnace body 2 is connected to a vacuum pump 1, the melt filtration and collection mechanism includes a foam ceramic filter screen 3 and an ultrasonic vibration rod 4 penetrating the foam ceramic filter screen 3, and an electric dumping device 5 is provided at the bottom of the metal thermal reduction reaction mechanism.

[0040] In actual use, in this embodiment, a furnace body 2 and a vacuum pump 1 are provided to carry out the thermal reduction and melt collection processes under vacuum conditions, thereby reducing the content of oxygen and nitrogen elements in the melt; a foam ceramic filter screen 3 and an ultrasonic vibration rod 4 are provided in the melt filtration and collection mechanism to separate inclusions in the melt; the ultrasonic tool head is brought into direct contact with the melt to enhance the effect of ultrasonic waves on the melt, thereby improving the purity and uniformity of the melt; an electric dumping device 5 is provided at the bottom of the metal thermal reduction reaction mechanism to enable the melt prepared in the metal thermal reduction reaction mechanism to be transferred to the melt filtration and collection mechanism.

[0041] Preferably, in this embodiment, the power of the ultrasonic vibration rod 4 is 3 kW and the operating frequency is 20 kHz. The power and operating frequency of the ultrasonic vibration rod 4 are relatively large, which can improve the efficiency of separating slag materials.

[0042] It should be noted that in this embodiment, the electric dumping device 5 is controlled by an experienced and skilled operator to accurately control the dumping angle and speed so that the melt prepared by the metal thermal reduction reaction mechanism is completely transferred to the melt filtering and collecting mechanism.

[0043] Furthermore, if Figure 1 As shown, in this embodiment, the melt filtering and collecting mechanism further includes a second alumina crucible 8, the foam ceramic filter 3 is arranged at the upper end inside the second alumina crucible 8, and the ultrasonic tool head of the ultrasonic vibration rod 4 is made of ceramic material.

[0044] In actual use, in this embodiment, a second alumina crucible 8 is provided to collect the melt, and a foam ceramic filter screen 3 is provided at the upper end inside the second alumina crucible 8 to utilize the unique porous structure of the foam ceramic filter screen 3 to preliminarily filter the melt, filter out larger inclusions, and divide the larger pores inside the melt to facilitate subsequent exhaust. By setting the ultrasonic tool head of the ultrasonic vibrator 4 to be made of ceramic material, the ultrasonic tool head can maintain normal operation after contacting the melt. At the same time, the ceramic material hardly reacts with the melt and is easy to separate from the adhered vanadium-aluminum intermediate alloy.

[0045] Preferably, in this embodiment, the foam ceramic filter 3 is made of zirconia material, with a pore size greater than 30PPI, a porosity of 80%~90%, and a thickness of 20mm~40mm. By preferably selecting the foam ceramic filter 3 made of zirconia material, the foam ceramic filter 3 is more stable when filtering the melt, and the filtering performance of the foam ceramic filter 3 can be adjusted by controlling various dimensional indicators of the foam ceramic filter 3.

[0046] Preferably, the ultrasonic tool head in this embodiment is made of Sialon ceramic material, which can withstand high temperatures above 1500°C.

[0047] Furthermore, if Figure 1 As shown, in this embodiment, the metal thermal reduction reaction mechanism includes a first alumina crucible 6 and a heating and ignition device 7 extending into the first alumina crucible 6 .

[0048] In actual use, in this embodiment, a first alumina crucible 6 is used as a container for thermal reduction reaction and a second alumina crucible 8 is used to collect the melt. Since the alumina crucible has low thermal conductivity and good thermal insulation performance, this characteristic prolongs the duration of the high-temperature molten state of the melt. In the high-temperature state, both the melt and the slag have high fluidity, which can promote the complete separation of the melt and the slag.

[0049] Preferably, the heating and ignition device 7 in this embodiment uses a resistance wire made of nickel-chromium or tungsten. By setting a resistance wire made of nickel-chromium or tungsten that can withstand high temperatures above 1200° C., it is ensured that the metal thermal reduction reaction can be triggered.

[0050] Furthermore, if Figure 1As shown, in this embodiment, a guide groove is provided between the first alumina crucible 6 and the melt filtering and collecting mechanism, which is used to guide the melt in the first alumina crucible 6 into the melt filtering and collecting mechanism, and the guide groove includes a steel shell layer, a refractory brick layer arranged above the steel shell layer, and an alumina layer arranged above the refractory brick layer, and the alumina layer is also filled in the gap of the refractory brick layer, and the alumina layer is formed by a mixture of alumina and a binder.

[0051] In actual use, in this embodiment, a guide groove is provided to guide the melt to be transferred from the first alumina crucible 6 to the melt filtering and collecting mechanism to prevent the melt from being difficult to pour and difficult to enter the melt filtering and collecting mechanism when the viscosity is too high; by setting the guide groove to a structure consisting of a steel shell layer, a refractory brick layer and an alumina layer, and the gaps in the refractory brick layer are filled with an alumina layer, the guide groove has excellent thermal stability and can smoothly transfer the melt without being affected by high temperature.

[0052] It should be noted that, in this embodiment, the guide groove is subjected to a baking treatment at 200° C. for 48 hours to evaporate moisture to ensure the integrity of the guide groove structure and the reliability of its function.

[0053] Furthermore, if Figure 1 As shown, in this embodiment, the furnace body 2 is a double-layer water-cooled jacket structure consisting of an inner wall of the furnace body 2 and a jacket fixedly installed outside the inner wall of the furnace body 2, and circulating water is passed into the jacket.

[0054] In actual use, in this embodiment, the furnace body 2 is set as a double-layer water-cooled jacket structure to cool the preparation device; preferably, the circulating water in this embodiment uses cooling water that is not easy to produce scale layer to reduce the frequency of descaling.

[0055] The preparation method of the aviation-grade vanadium-aluminum master alloy of the present invention is described in detail through Examples 2 to 4.

[0056] Example 2

[0057] The preparation method of this embodiment comprises the following steps:

[0058] Step 1, raw material pretreatment: 42.71g of vanadium pentoxide powder with a mass purity of not less than 99.9% and a D50 particle size of 300μm, 40.21g of aluminum particles with a mass purity of not less than 99.9% and a D50 particle size of 500μm, 3.14g of analytically pure calcium fluoride and 13.94g of analytically pure calcium oxide are placed in an oven at 120°C for 24h, and then placed in a mixer for mixing for 4h to obtain a raw material;

[0059] Step 2, preparing an alumina crucible: mixing aluminum oxide and sodium carbonate with a mass concentration of 15% evenly, shaping and then sintering: heating to 20°C and keeping warm for 25 minutes, then heating to 200°C and keeping warm for 25 minutes, heating to 200°C and keeping warm for 100 minutes, heating to 700°C and keeping warm for 60 minutes, then turning off the flame and cooling in the furnace for 60 minutes, to obtain a first alumina crucible 6 and a second alumina crucible 8; the aluminum oxide is composed of aluminum oxide with a particle size of 3mm~5mm, 1mm~3mm, 0.3mm~1mm and less than 0.3mm in a mass ratio of 1:2:3:4;

[0060] Step 3, metal thermal reduction process: put the raw materials mixed in step 1 into the first alumina crucible 6 obtained in step 2, contact the heating ignition device 7 with the raw materials, start the vacuum pump 1 to evacuate to below -0.1 MPa, turn off the vacuum pump 1, and then start the heating ignition device 7 to induce metal thermal reduction reaction to obtain a melt;

[0061] Step 4, impurity removal: start the vacuum pump 1 and control the electric dumping device 5, pour the melt obtained in step 3 into the second alumina crucible 8 through the foam ceramic filter 3, start the ultrasonic vibrator 4 to remove impurities, and turn off the ultrasonic vibrator 4 and the vacuum pump 1 after the melt is cooled to obtain Al-55wt.%V alloy; sandblast and finish the Al-55wt.%V alloy, and then crush and screen it in turn to obtain Al-55wt.%V alloy particles, which are stored after manual selection and sampling inspection.

[0062] The Al-55wt.%V alloy prepared in this example was subjected to electron microscope scanning analysis and energy spectrum analysis. Figures 2 to 4 As shown, aluminum and vanadium elements are evenly distributed in the Al-55wt.%V alloy and no inclusions are observed; the Al-55wt.%V alloy prepared in this embodiment is analyzed for composition, and the Al-55wt.%V alloy is composed of the following elements in mass percentage: V 56.24%, Fe 0.016%, Si 0.010%, C 0.008%, O 0.011%, N 0.008%, and the balance is Al; the mass percentage of nitrogen element is less than 0.01%, and the mass percentages of impurity elements such as carbon and oxygen are all less than 0.02%, indicating that the use of vacuum degassing technology, foam ceramic filter 3 and ultrasonic technology can effectively reduce the content of impurity elements and inclusions and improve the purity of vanadium-aluminum intermediate alloy.

[0063] Example 3

[0064] The preparation method of this embodiment comprises the following steps:

[0065] Step 1, raw material pretreatment: 49.28g of vanadium pentoxide powder with a mass purity of not less than 99.9% and a D50 particle size of 300μm, 37.32g of aluminum particles with a mass purity of not less than 99.9% and a D50 particle size of 300μm, 2.46g of analytically pure calcium fluoride and 10.94g of analytically pure calcium oxide are placed in an oven at 120°C for 24h, and then placed in a mixer for mixing for 4h to obtain a raw material;

[0066] Step 2, preparing an alumina crucible: mixing aluminum oxide and sodium carbonate with a mass concentration of 15% uniformly, shaping and then sintering, heating to 22°C and keeping warm for 25 minutes, then heating to 200°C and keeping warm for 25 minutes, heating to 400°C and keeping warm for 100 minutes, heating to 800°C and keeping warm for 60 minutes, then turning off the furnace and cooling for 60 minutes to obtain a first alumina crucible 6 and a second alumina crucible 8; the aluminum oxide is composed of aluminum oxide with a particle size of 3mm~5mm, 1mm~3mm, 0.3mm~1mm and less than 0.3mm in a mass ratio of 1:2:3:4;

[0067] Step 3, metal thermal reduction process: put the raw materials mixed in step 1 into the first alumina crucible 6 obtained in step 2, contact the heating ignition device 7 with the raw materials, start the vacuum pump 1 to evacuate to below -0.1 MPa, turn off the vacuum pump 1, and then start the heating ignition device 7 to induce metal thermal reduction reaction to obtain a melt;

[0068] Step 4, impurity removal: start the vacuum pump 1 and control the electric dumping device 5, pour the melt obtained in step 3 into the second alumina crucible 8 through the foam ceramic filter 3, start the ultrasonic vibrator 4 to remove impurities, and turn off the ultrasonic vibrator 4 and the vacuum pump 1 after the melt is cooled to obtain Al-65wt.%V alloy; sandblast and finish the Al-65wt.%V alloy, and then crush and screen it in turn to obtain Al-65wt.%V alloy particles, which are stored after manual selection and sampling inspection.

[0069] The Al-65wt.%V alloy prepared in this example was subjected to electron microscope scanning analysis. Figure 5As shown, no inclusions were observed in the Al-65wt.%V alloy; the Al-65wt.%V alloy prepared in this embodiment was analyzed for composition, and the Al-65wt.%V alloy was composed of the following elements in mass percentage: V 66.82%, Fe 0.013%, Si 0.007%, C 0.010%, O 0.012%, N0.006%, and the balance was Al; the mass percentage of nitrogen element was less than 0.01%, and the mass percentages of impurity elements such as carbon and oxygen were all less than 0.02%, indicating that the use of vacuum degassing technology, foam ceramic filter 3 and ultrasonic technology can effectively reduce the content of impurity elements and inclusions and improve the purity of the vanadium-aluminum intermediate alloy.

[0070] Example 4

[0071] The preparation method of this embodiment comprises the following steps:

[0072] Step 1, raw material pretreatment: 45.84g of vanadium pentoxide powder with a mass purity of not less than 99.9% and a D50 particle size of 300μm, 25.87g of aluminum particles with a mass purity of not less than 99.9% and a D50 particle size of 600μm, 5.20g of analytically pure calcium fluoride and 23.09g of analytically pure calcium oxide are placed in an oven at 120°C for 24h, and then placed in a mixer for mixing for 4h to obtain a raw material;

[0073] Step 2, preparing an alumina crucible: mixing aluminum oxide and sodium carbonate with a mass concentration of 15% uniformly, shaping and sintering, heating to 25°C and keeping warm for 25 minutes, then heating to 200°C and keeping warm for 25 minutes, heating to 700°C and keeping warm for 100 minutes, heating to 900°C and keeping warm for 60 minutes, then turning off the flame and cooling in the furnace for 60 minutes to obtain a first alumina crucible 6 and a second alumina crucible 8; the aluminum oxide is composed of aluminum oxide with a particle size of 3mm~5mm, 1mm~3mm, 0.3mm~1mm and less than 0.3mm in a mass ratio of 1:2:3:4;

[0074] Step 3, metal thermal reduction process: put the raw materials mixed in step 1 into the first alumina crucible 6 obtained in step 2, contact the heating ignition device 7 with the raw materials, start the vacuum pump 1 to evacuate to below -0.1 MPa, turn off the vacuum pump 1, and then start the heating ignition device 7 to induce metal thermal reduction reaction to obtain a melt;

[0075] Step 4, impurity removal: start the vacuum pump 1 and control the electric dumping device 5, pour the melt obtained in step 3 into the second alumina crucible 8 through the foam ceramic filter 3, start the ultrasonic vibrator 4 to remove impurities, and turn off the ultrasonic vibrator 4 and the vacuum pump 1 after the melt is cooled to obtain Al-85wt.%V alloy; sandblast and finish the Al-85wt.%V alloy, and then crush and screen it in turn to obtain Al-85wt.%V alloy particles, which are stored after manual selection and sampling inspection.

[0076] The Al-85wt.%V alloy prepared in this embodiment was analyzed for its composition. The Al-85wt.%V alloy was composed of the following elements in mass percentage: V 87.69%, Fe 0.015%, Si 0.009%, C 0.007%, O 0.016%, N 0.009%, and the balance was Al; the mass percentage of nitrogen was less than 0.01%, and the mass percentages of impurity elements such as carbon and oxygen were all less than 0.02%, indicating that the use of vacuum degassing technology, foam ceramic filter 3 and ultrasonic technology can effectively reduce the content of impurity elements and inclusions, and improve the purity of the vanadium-aluminum intermediate alloy.

[0077] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent structural transformation made to the above embodiment based on the technical essence of the present invention still falls within the protection scope of the technical solution of the present invention.

Claims

1. A device for preparing aviation-grade vanadium-aluminum master alloy, characterized in that: The invention comprises a furnace body (2), a metal thermal reduction reaction mechanism and a melt filtering and collecting mechanism arranged in the furnace body (2), wherein the furnace body (2) is connected to a vacuum pump (1), the melt filtering and collecting mechanism comprises a foam ceramic filter screen (3) and an ultrasonic vibration rod (4) penetrating the foam ceramic filter screen (3), an electric dumping device (5) is arranged at the bottom of the metal thermal reduction reaction mechanism, the melt filtering and collecting mechanism also comprises a second alumina crucible (8), the foam ceramic filter screen (3) is arranged at the upper end of the second alumina crucible (8), the ultrasonic tool head of the ultrasonic vibration rod (4) is made of ceramic material, and the metal thermal reduction reaction mechanism comprises a first alumina crucible (6) and a heating and ignition device (7) extending into the first alumina crucible (6).

2. The device for preparing aviation-grade vanadium-aluminum master alloy according to claim 1, characterized in that: A guide groove is provided between the first alumina crucible (6) and the melt filtering and collecting mechanism, for guiding the melt in the first alumina crucible (6) into the melt filtering and collecting mechanism, the guide groove comprising a steel shell layer, a refractory brick layer arranged above the steel shell layer, and an alumina layer arranged above the refractory brick layer, the alumina layer also filling the gaps in the refractory brick layer, the alumina layer consisting of alumina and a binder.

3. The device for preparing aviation-grade vanadium-aluminum master alloy according to claim 1, characterized in that: The furnace body (2) is a double-layer water-cooled jacket structure consisting of an inner wall of the furnace body (2) and a jacket fixedly installed outside the inner wall of the furnace body (2), and circulating water is passed into the jacket.

4. A method for preparing an aviation-grade vanadium-aluminum master alloy, using the apparatus for preparing an aviation-grade vanadium-aluminum master alloy as claimed in any one of claims 1 to 3, characterized in that: The preparation method comprises the following steps: Step 1: Raw material pretreatment: drying vanadium pentoxide powder, aluminum particles, calcium fluoride and calcium oxide in an oven, and then mixing them in a mixer to obtain raw materials; Step 2, preparing an alumina crucible: mixing aluminum oxide and sodium carbonate evenly, shaping them into a shape, and then sintering them to obtain an alumina crucible; the alumina crucible comprises a first alumina crucible (6) and a second alumina crucible (8); Step 3, metal thermal reduction process: the raw materials mixed in step 1 are placed in the first alumina crucible (6) obtained in step 2, a heating ignition device (7) is brought into contact with the raw materials, a vacuum pump (1) is started to evacuate to below -0.1 MPa, the vacuum pump (1) is turned off, and then the heating ignition device (7) is started to initiate a metal thermal reduction reaction to obtain a melt; Step 4, impurity removal: start the vacuum pump (1) and control the electric dumping device (5), pour the melt obtained in step 3 into the second alumina crucible (8) through the foam ceramic filter (3), start the ultrasonic vibration rod (4) to remove impurities, and turn off the ultrasonic vibration rod (4) and the vacuum pump (1) after the melt is cooled to obtain a vanadium aluminum intermediate alloy.

5. The method for preparing an aviation-grade vanadium-aluminum master alloy according to claim 4, characterized in that: The mass purity of the vanadium pentoxide powder in step 1 is not less than 99.9%, the mass purity of the aluminum particles is not less than 99.9%, the D50 particle size ratio of the vanadium pentoxide powder to the aluminum particles is 1:1-1:2, and the calcium fluoride and calcium oxide are both analytically pure.

6. The method for preparing an aviation-grade vanadium-aluminum master alloy according to claim 4, characterized in that: The aluminum oxide in step 2 is composed of aluminum oxide with particle sizes of 3mm~5mm, 1mm~3mm, 0.3mm~1mm and less than 0.3mm in a mass ratio of 1:2:3:4; the sintering system is: heating to 20℃~25℃ and keeping warm for 25min, then heating to 200℃ and keeping warm for 25min, heating to 200℃~700℃ and keeping warm for 100min, heating to 700℃~900℃ and keeping warm for 60min, and then turning off the furnace and cooling for 60min.

7. The method for preparing an aviation-grade vanadium-aluminum master alloy according to claim 4, characterized in that: The vanadium-aluminum master alloy in step 4 is composed of the following elements in percentage by mass: V 55%-88%, Fe not more than 0.20%, Si not more than 0.20%, C not more than 0.02%, O not more than 0.02%, N not more than 0.01%, and the balance is Al.

8. The method for preparing an aviation-grade vanadium-aluminum master alloy according to claim 4, characterized in that: In step 4, the vanadium-aluminum master alloy is subjected to sandblasting and finishing treatment, and then crushed and screened in sequence to obtain vanadium-aluminum master alloy particles. The vanadium-aluminum master alloy particles are manually selected and sampled for inspection before being stored.