Micro-LED epitaxial wafer and preparation method thereof, Micro-LED
By designing two P-type hole injection layers and semiconductor layers in Micro-LED epitaxial sheets, the problem of low efficiency at low current density is solved, hole injection efficiency and electron hole matching are improved, and Micro-LED is improved light effect and material quality.
Patent Information
- Application Number
- CN202411204418.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-08-30
AI Technical Summary
Micro LEDs are inefficient at low operating current density. Traditional epitaxial structure design cannot meet the application requirements of small size, low current and low power. The electronic barrier layer structure blocks hole injection, reducing quantum efficiency.
Design a Micro-LED epitaxial sheet, including an N-type semiconductor layer, a stress relief layer, a multi-quantum well luminescent layer, two P-type hole injection layers and two P-type semiconductor layers, a second P-type hole injection layer and The growth temperature of the semiconductor layer is higher than that of the first layer, which eliminates the blocking effect of the electron barrier layer on hole injection, and improves the matching degree of hole injection efficiency and electron hole concentration.
It improves the light efficiency of Micro-LED at low operating current density, enhances the quality of epitaxial layer materials, and improves the brightness and yield of Micro-LED chips.
Smart Images

Figure CN118712302B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of optoelectronic technology, and in particular to a Micro-LED epitaxial wafer and a preparation method thereof, and a Micro-LED. Background Art
[0002] With the booming development of emerging wearable and portable technologies, micron-sized LED chips (Micro LED) have received great attention and research from scientific research institutions and enterprises due to their application prospects in display, visible light communication, biomedicine and other fields. In addition, Micro LED display has excellent performance such as nanosecond-level high-speed response performance, stable characteristics of inorganic materials, high light efficiency, high reliability, high color purity and contrast, and transparency. The combination of these characteristics is unattainable by liquid crystal display and organic LED.
[0003] Although Micro LED has many excellent characteristics, it also faces challenges in manufacturing technology and material device physics. For example, the problem of the decrease in device peak EQE (External Quantum Efficiency) and the corresponding increase in current density as the chip size decreases has not been completely solved. The efficiency of Micro LED with an operating current density in the range of 0.01~0.5A / cm² is still obviously insufficient. In fact, even conventional-sized chips for general lighting and backlight display applications have relatively low efficiency at this current density. The reason is that in order to balance efficiency and cost factors, the operating current density of conventional-sized chips is 20A / cm². 2 Up to 40A / cm 2The goal of the corresponding epitaxial structure design and material growth is to improve the efficiency under high current density, and its peak EQE is usually in the current density range of 1~4A / cm², without paying attention to the device efficiency under low current density. Under different current densities, the dominant reasons for the light-emitting mechanism of LED devices are different, and the corresponding epitaxial layer structure should also change. For example, under the low current density of 0.01~0.5A / cm² in the Micro LED working range, the carrier concentration in the quantum well is relatively low, the proportion of Auger recombination is small, and the corresponding quantum well recombination volume can be reduced, that is, the number of quantum wells can be reduced, the number of defects can be reduced, and the EQE of the device under low current density can be improved; at the same time, electron leakage has not occurred or the proportion is very low under low current density, and the electron blocking layer structure not only has no effect of blocking electrons, but will block the injection of holes, reducing the quantum efficiency of the device. Therefore, in-depth mechanism research, design and growth of LED epitaxial layer structure under low current density working conditions of Micro LED is a necessary key technology for the research and development of high-efficiency Micro LED devices driven by low working current density. The epitaxial structure design of traditional visible light LEDs is based on traditional application scenarios of large chips, high currents, and high powers, while the display applications of Micro LEDs require small size, low current, and low power. LEDs designed with traditional epitaxial structures can no longer meet the application requirements of Micro LEDs. Therefore, redesigning the epitaxial structure of Micro LEDs suitable for small size, low current, and low power, and improving their electro-optical conversion efficiency, is an important challenge currently faced by both academia and industry. Summary of the invention
[0004] The technical problem to be solved by the present invention is to provide a Micro-LED epitaxial wafer, which improves the hole injection efficiency of the P-type semiconductor layer and improves the matching degree of the electron hole concentration in the multi-quantum well light-emitting layer region, thereby improving the luminous efficiency of the Micro-LED chip at low operating current density.
[0005] The technical problem to be solved by the present invention is also to provide a method for preparing a Micro-LED epitaxial wafer, which has a simple process and can stably produce a Micro-LED epitaxial wafer with good luminous efficiency.
[0006] In order to solve the above technical problems, the present invention provides a Micro-LED epitaxial wafer, comprising a substrate, on which an N-type semiconductor layer, a stress release layer, a multi-quantum well light-emitting layer, a first P-type hole injection layer, a first P-type semiconductor layer, a second P-type hole injection layer, a second P-type semiconductor layer, and a P-type ohmic contact layer are sequentially arranged;
[0007] The growth temperature of the second P-type hole injection layer is higher than the growth temperature of the first P-type hole injection layer;
[0008] A growth temperature of the second P-type semiconductor layer is higher than a growth temperature of the first P-type semiconductor layer.
[0009] In some embodiments, the first P-type hole injection layer includes a first AlGaN layer, an AlN layer, a first AlInGaN layer, a second AlInGaN layer, a second AlGaN layer, and a GaN layer stacked in sequence;
[0010] In some embodiments, the thickness of the first AlGaN layer is 1 nm to 16 nm;
[0011] The Al composition of the first AlGaN layer is 0.25-0.75;
[0012] The thickness of the AlN layer is 1 nm to 16 nm;
[0013] The thickness of the first AlInGaN layer is 2nm~36nm;
[0014] The Al composition of the first AlInGaN layer is 0.25-0.75;
[0015] The In composition of the first AlInGaN layer is 0.01-0.06;
[0016] The thickness of the second AlInGaN layer is 2nm~36nm;
[0017] The Al composition of the second AlInGaN layer is 0.16-0.6;
[0018] The In composition of the second AlInGaN layer is 0.02-0.08;
[0019] The first AlInGaN layer is not intentionally doped, and the Mg doping concentration of the second AlInGaN layer is 2.8×10 18 atoms / cm 3 ~1.6×10 19 atoms / cm 3 ;
[0020] The thickness of the second AlGaN layer is 1 nm to 16 nm;
[0021] The Al composition of the second AlGaN layer is 0.25-0.75;
[0022] The GaN layer is not intentionally doped, and the thickness of the GaN layer is 1 nm to 16 nm.
[0023] In some embodiments, the Al composition of the first AlInGaN layer is greater than the Al composition of the second AlInGaN layer;
[0024] The In composition of the first AlInGaN layer is smaller than the In composition of the second AlInGaN layer.
[0025] In some embodiments, the first P-type semiconductor layer is a Mg-doped AlInGaN layer;
[0026] The Mg doping concentration of the first P-type semiconductor layer is 1.5×10 19 atoms / cm 3 ~3.6×10 20 atoms / cm 3 ;
[0027] The thickness of the first P-type semiconductor layer is 8nm-250nm;
[0028] The Al component in the first P-type semiconductor layer decreases along the growth direction;
[0029] The Mg doping concentration in the first P-type semiconductor layer decreases along the growth direction.
[0030] In some embodiments, the second P-type hole injection layer is an AlGaN / InGaN superlattice layer;
[0031] The AlGaN / InGaN superlattice layer includes an AlGaN layer and a Mg-doped InGaN layer alternately stacked, and the number of alternating periods is 3 to 25;
[0032] The thickness of the AlGaN layer is 1.2nm~7.5nm;
[0033] The Al composition of the AlGaN layer is 0.25-0.6;
[0034] The thickness of the Mg-doped InGaN layer is 1.2 nm to 7.5 nm;
[0035] The In component of the Mg-doped InGaN layer is 0.02-0.1;
[0036] The Mg doping concentration of the Mg-doped InGaN layer is 3.2×10 18 atoms / cm 3 ~2.5×10 19 atoms / cm 3 .
[0037] In some embodiments, the second P-type semiconductor layer is a Mg-doped GaN layer;
[0038] The Mg doping concentration of the second P-type semiconductor layer is 1.2×10 19 atoms / cm3 ~2.5×10 20 atoms / cm 3 ;
[0039] The thickness of the second P-type semiconductor layer is 6nm-200nm;
[0040] The Mg doping concentration in the second P-type semiconductor layer decreases along the growth direction.
[0041] In some embodiments, the P-type ohmic contact layer is an AlInGaN layer heavily doped with Mg;
[0042] The Mg doping concentration of the P-type ohmic contact layer is 3.2×10 19 atoms / cm 3 ~8.5×10 20 atoms / cm 3 ;
[0043] The thickness of the P-type ohmic contact layer is 1nm~30nm;
[0044] The In component in the heavily Mg-doped AlInGaN layer increases gradually along the growth direction.
[0045] To solve the above problems, the present invention also provides a method for preparing a Micro-LED epitaxial wafer, comprising the following steps:
[0046] S1. Prepare substrate;
[0047] S2, depositing an N-type semiconductor layer, a stress release layer, a multi-quantum well light-emitting layer, a first P-type hole injection layer, a first P-type semiconductor layer, a second P-type hole injection layer, a second P-type semiconductor layer, and a P-type ohmic contact layer on the substrate in sequence;
[0048] The growth temperature of the second P-type hole injection layer is higher than the growth temperature of the first P-type hole injection layer;
[0049] A growth temperature of the second P-type semiconductor layer is higher than a growth temperature of the first P-type semiconductor layer.
[0050] Correspondingly, the present invention also provides a Micro-LED, which includes the above-mentioned Micro-LED epitaxial wafer.
[0051] The implementation of the present invention has the following beneficial effects:
[0052] In the Micro-LED of the present invention, no electron blocking layer is provided on the multi-quantum well light-emitting layer. Under the low operating current density of the Micro-LED, electron leakage has not occurred or the proportion is very low. The electron blocking layer structure not only does not block electrons, but blocks the injection of holes, thereby reducing the quantum efficiency of the device. The present invention is provided with two P-type hole injection layers and two P-type semiconductor layers, that is, a first P-type hole injection layer, a first P-type semiconductor layer, a second P-type hole injection layer, and a second P-type semiconductor layer are sequentially stacked and grown from bottom to top. The present invention can eliminate the blocking effect of the electron blocking layer structure on hole injection, improve the hole injection efficiency of the P-type material, and improve the matching degree of the electron hole concentration in the multi-quantum well light-emitting layer region.
[0053] Furthermore, the growth temperature of the second P-type hole injection layer is higher than that of the first P-type hole injection layer, and the growth temperature of the second P-type semiconductor layer is higher than that of the first P-type semiconductor layer. The first P-type hole injection layer and the first P-type semiconductor layer close to the multi-quantum well light-emitting layer adopt a relatively low growth temperature, which can prevent high-temperature growth from damaging the material quality of the multi-quantum well light-emitting layer. The second P-type hole injection layer and the second P-type semiconductor layer far away from the multi-quantum well light-emitting layer adopt a high-temperature growth mode, which can improve atomic mobility and are more inclined to the growth of two-dimensional materials, which is beneficial to the merging of V-pits in semiconductor materials and obtaining high-quality epitaxial layer materials, so as to improve the brightness and yield performance of the Micro-LED chip. BRIEF DESCRIPTION OF THE DRAWINGS
[0054] Figure 1 This is a schematic diagram of the structure of the Micro-LED epitaxial wafer provided by the present invention. DETAILED DESCRIPTION
[0055] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. Examples of the embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements with the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present invention, and should not be construed as limiting the present invention. In addition, it should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.
[0056] In the description of the present invention, it is necessary to understand that the terms "length", "width", "up", "down", "left", "right", "horizontal", "top", "bottom", etc. indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention.
[0057] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.
[0058] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection, an electrical connection, or mutual communication; it can be a direct connection, or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0059] In the present invention, unless otherwise clearly specified and limited, a first feature being "above" or "below" a second feature may include that the first and second features are in direct contact, or may include that the first and second features are not in direct contact but are in contact through another feature between them. Moreover, a first feature being "above", "above" and "above" a second feature includes that the first feature is directly above and obliquely above the second feature, or simply indicates that the first feature is higher in level than the second feature. A first feature being "below", "below" and "below" a second feature includes that the first feature is directly below and obliquely below the second feature, or simply indicates that the first feature is lower in level than the second feature.
[0060] The disclosure below provides many different embodiments or examples to realize different structures of the present invention. In order to simplify the disclosure of the present invention, the parts and settings of specific examples are described below. Of course, they are only examples, and the purpose is not to limit the present invention. In addition, the present invention can repeat reference numbers and / or reference letters in different examples, and this repetition is for the purpose of simplification and clarity, which itself does not indicate the relationship between the various embodiments and / or settings discussed. In addition, the examples of various specific processes and materials provided by the present invention, but those of ordinary skill in the art can be aware of the application of other processes and / or the use of other materials.
[0061] In the present invention, "preferred" and "better" are only used to describe implementation methods or embodiments with better effects, and it should be understood that they do not constitute a limitation on the scope of protection of the present invention. In the present invention, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features. In the present invention, when involving numerical ranges, unless otherwise specified, the two endpoints of the numerical range are included.
[0062] To solve the above problems, the present invention provides a Micro-LED epitaxial wafer, such as Figure 1 As shown, it includes a substrate 100, on which an N-type semiconductor layer 200, a stress release layer 300, a multi-quantum well light-emitting layer 400, a first P-type hole injection layer 500, a first P-type semiconductor layer 600, a second P-type hole injection layer 700, a second P-type semiconductor layer 800, and a P-type ohmic contact layer 900 are sequentially arranged;
[0063] The growth temperature of the second P-type hole injection layer 700 is higher than the growth temperature of the first P-type hole injection layer 500;
[0064] The growth temperature of the second P-type semiconductor layer 800 is higher than the growth temperature of the first P-type semiconductor layer 600 .
[0065] In the Micro-LED of the present invention, no electron blocking layer is provided on the multi-quantum well light-emitting layer. Under the low operating current density of the Micro-LED, electron leakage has not occurred or the proportion is very low. The electron blocking layer structure not only does not block electrons, but blocks the injection of holes, thereby reducing the quantum efficiency of the device. The present invention is provided with two P-type hole injection layers and two P-type semiconductor layers, that is, a first P-type hole injection layer, a first P-type semiconductor layer, a second P-type hole injection layer, and a second P-type semiconductor layer are sequentially stacked and grown from bottom to top. The present invention can eliminate the blocking effect of the electron blocking layer structure on hole injection, improve the hole injection efficiency of the P-type material, and improve the matching degree of the electron hole concentration in the multi-quantum well light-emitting layer region.
[0066] Furthermore, the growth temperature of the second P-type hole injection layer is higher than that of the first P-type hole injection layer, and the growth temperature of the second P-type semiconductor layer is higher than that of the first P-type semiconductor layer. The first P-type hole injection layer and the first P-type semiconductor layer close to the multi-quantum well light-emitting layer adopt a relatively low growth temperature, which can prevent high-temperature growth from damaging the material quality of the multi-quantum well light-emitting layer. The second P-type hole injection layer and the second P-type semiconductor layer far away from the multi-quantum well light-emitting layer adopt a high-temperature growth mode, which can improve atomic mobility and are more inclined to the growth of two-dimensional materials, which is beneficial to the merging of V-pits in semiconductor materials and obtaining high-quality epitaxial layer materials, so as to improve the brightness and yield performance of the Micro-LED chip.
[0067] (i) The specific structure of the first P-type hole injection layer 500 is as follows:
[0068] In some embodiments, the first P-type hole injection layer includes a first AlGaN layer, an AlN layer, a first AlInGaN layer, a second AlInGaN layer, a second AlGaN layer, and a GaN layer stacked in sequence.
[0069] In some embodiments, the thickness of the first AlGaN layer is 1 nm to 16 nm; exemplary thicknesses of the first AlGaN layer are 2 nm, 4 nm, 6 nm, 8 nm, 10 nm, 12 nm, and 14 nm, but are not limited to the above. The Al composition of the first AlGaN layer is 0.25 to 0.75; the first AlGaN layer is not intentionally doped.
[0070] In some embodiments, the thickness of the AlN layer is 1 nm to 16 nm; exemplary thicknesses of the AlN layer are 2 nm, 4 nm, 6 nm, 8 nm, 10 nm, 12 nm, and 14 nm, but are not limited to the above. The AlN layer is not intentionally doped.
[0071] In some embodiments, the thickness of the first AlInGaN layer is 2nm to 36nm; exemplary thicknesses of the first AlInGaN layer are 2nm, 4nm, 6nm, 8nm, 10nm, 12nm, 14nm, 16nm, 18nm, 20nm, 22nm, 24nm, 26nm, 28nm, 30nm, 32nm, 34nm, but are not limited to the above. The Al component of the first AlInGaN layer is 0.25 to 0.75; the In component of the first AlInGaN layer is 0.01 to 0.06; the first AlInGaN layer is not intentionally doped.
[0072] In some embodiments, the thickness of the second AlInGaN layer is 2nm~36nm; exemplary thicknesses of the second AlInGaN layer are 2nm, 4nm, 6nm, 8nm, 10nm, 12nm, 14nm, 16nm, 18nm, 20nm, 22nm, 24nm, 26nm, 28nm, 30nm, 32nm, 34nm, but are not limited to the above. The Al component of the second AlInGaN layer is 0.16~0.6; the In component of the second AlInGaN layer is 0.02~0.08; the Mg doping concentration of the second AlInGaN layer is 2.8×10 18 atoms / cm 3 ~1.6×10 19 atoms / cm 3; The exemplary Mg doping concentration of the second AlInGaN layer is 3×10 18 atoms / cm 3 , 4×10 18 atoms / cm 3 , 5×10 18 atoms / cm 3 , 6×10 18 atoms / cm 3 ,7×10 18 atoms / cm 3 , 8×10 18 atoms / cm 3 ,9×10 18 atoms / cm 3 , 1×10 19 atoms / cm 3 , but not limited to the above.
[0073] In some embodiments, the thickness of the second AlGaN layer is 1 nm to 16 nm; exemplary thicknesses of the second AlGaN layer are 2 nm, 4 nm, 6 nm, 8 nm, 10 nm, 12 nm, 14 nm, but are not limited to the above. The Al composition of the second AlGaN layer is 0.25 to 0.75; the second AlGaN layer is not intentionally doped.
[0074] In some embodiments, the thickness of the GaN layer is 1 nm to 16 nm; exemplary thicknesses of the GaN layer are 2 nm, 4 nm, 6 nm, 8 nm, 10 nm, 12 nm, and 14 nm, but are not limited to the above. The GaN layer is not intentionally doped.
[0075] In some embodiments, the Al composition of the first AlInGaN layer is greater than the Al composition of the second AlInGaN layer; and the In composition of the first AlInGaN layer is less than the In composition of the second AlInGaN layer.
[0076] The wide bandgap AlN and AlGaN materials in the first P-type hole injection layer mainly limit carriers and reduce the electron mobility rate to prevent electron injection into the P-type material and cause electron leakage, while the low bandgap AlInGaN material can store some holes and weaken the blocking effect on hole injection of the P-type material, so as to improve the hole injection efficiency of the P-type material. The AlInGaN material is doped with Mg element, which can provide some holes to the multi-quantum well light-emitting layer to participate in light emission, further improve the hole injection efficiency and improve the electron-hole matching in the multi-quantum well light-emitting layer, so as to improve the light-emitting efficiency of Micro-LED.
[0077] (II) The specific structure of the first P-type semiconductor layer 600 is as follows:
[0078] In some embodiments, the first P-type semiconductor layer is a Mg-doped AlInGaN layer; the Mg doping concentration of the first P-type semiconductor layer is 1.5×10 19 atoms / cm 3 ~3.6×10 20 atoms / cm 3 The exemplary Mg doping concentration of the first P-type semiconductor layer is 2×10 19 atoms / cm 3 , 3×10 19 atoms / cm 3 , 4×10 19 atoms / cm 3 , 5×10 19 atoms / cm 3 , 6×10 19 atoms / cm 3 ,7×10 19 atoms / cm 3 , 8×10 19 atoms / cm 3 ,9×10 19 atoms / cm 3 , 1×10 20 atoms / cm 3 , 2×10 20 atoms / cm 3 , but not limited to the above.
[0079] In some embodiments, the thickness of the first P-type semiconductor layer is 8 nm to 250 nm; exemplary thicknesses of the first P-type semiconductor layer are 10 nm, 50 nm, 100 nm, 150 nm, and 200 nm, but are not limited to the above.
[0080] In some embodiments, the Al component in the first P-type semiconductor layer decreases along the growth direction; and the Mg doping concentration in the first P-type semiconductor layer decreases along the growth direction.
[0081] The first P-type semiconductor layer serves as a main functional layer for providing holes for Micro-LEDs.
[0082] (III) The specific structure of the second P-type hole injection layer 700 is as follows:
[0083] In some embodiments, the second P-type hole injection layer is an AlGaN / InGaN superlattice layer; the AlGaN / InGaN superlattice layer includes alternately stacked AlGaN layers and Mg-doped InGaN layers, and the number of alternating periods is 3-25.
[0084] In some embodiments, the thickness of the AlGaN layer is 1.2 nm to 7.5 nm; exemplary thicknesses of the AlGaN layer are 2 nm, 3 nm, 4 nm, 5 nm, and 6 nm, but are not limited to the above; and the Al component of the AlGaN layer is 0.25 to 0.6.
[0085] In some embodiments, the thickness of the Mg-doped InGaN layer is 1.2nm~7.5nm; exemplary thicknesses of the Mg-doped InGaN layer are 2nm, 3nm, 4nm, 5nm, 6nm, but not limited to the above; the In component of the Mg-doped InGaN layer is 0.02~0.1.
[0086] In some embodiments, the Mg doping concentration of the Mg-doped InGaN layer is 3.2×10 18 atoms / cm 3 ~2.5×10 19 atoms / cm 3 The exemplary Mg doping concentration of the Mg-doped InGaN layer is 4×10 18 atoms / cm 3 , 5×10 18 atoms / cm 3 , 6×10 18 atoms / cm 3 ,7×10 18 atoms / cm 3 , 8×10 18 atoms / cm 3 ,9×10 18 atoms / cm 3 , 1×10 19 atoms / cm 3 , 2×10 19 atoms / cm 3 , but not limited to the above.
[0087] The wide bandgap AlGaN material in the second P-type hole injection layer mainly plays the role of limiting carriers, reducing the electron mobility rate, and preventing electrons from being injected into the P-type material to cause electron leakage, while the low bandgap InGaN material can reserve some holes and at the same time weaken the blocking effect on hole injection of the P-type material, so as to improve the hole injection efficiency of the P-type material. InGaN material is doped with Mg element, which can provide some holes to the multi-quantum well light-emitting layer to participate in light emission, further improving the hole injection efficiency and improving the electron-hole matching in the multi-quantum well light-emitting layer, so as to improve the light-emitting efficiency of Micro-LED.
[0088] (IV) The specific structure of the second P-type semiconductor layer 800 is as follows:
[0089] In some embodiments, the second P-type semiconductor layer is a Mg-doped GaN layer; the Mg doping concentration of the second P-type semiconductor layer is 1.2×10 19 atoms / cm 3 ~2.5×10 20 atoms / cm 3 The exemplary Mg doping concentration of the second P-type semiconductor layer is 2×10 19 atoms / cm 3 , 3×10 19 atoms / cm 3 , 4×10 19 atoms / cm 3 , 5×10 19 atoms / cm 3 , 6×10 19 atoms / cm 3 ,7×10 19 atoms / cm 3 , 8×10 19 atoms / cm 3 ,9×10 19 atoms / cm 3 , 1×10 20 atoms / cm 3 , 2×10 20 atoms / cm 3 , but not limited to the above.
[0090] In some embodiments, the thickness of the second P-type semiconductor layer is 6 nm to 200 nm; exemplary thicknesses of the second P-type semiconductor layer are 10 nm, 50 nm, 100 nm, 150 nm, and 200 nm, but are not limited to the above.
[0091] In some embodiments, the Mg doping concentration in the second P-type semiconductor layer decreases along the growth direction.
[0092] (V) The specific structure of the P-type ohmic contact layer 900 is as follows:
[0093] In some embodiments, the P-type ohmic contact layer is an AlInGaN layer heavily doped with Mg; the Mg doping concentration of the P-type ohmic contact layer is 3.2×10 19 atoms / cm 3 ~8.5×10 20 atoms / cm 3 The exemplary Mg doping concentration of the P-type ohmic contact layer is 4×10 19 atoms / cm 3 , 5×10 19 atoms / cm 3 , 6×10 19 atoms / cm 3 ,7×10 19 atoms / cm 3 , 8×10 19 atoms / cm 3 ,9×10 19 atoms / cm 3 , 1×10 20 atoms / cm 3 , 2×10 20 atoms / cm 3 , 3×10 20 atoms / cm 3 , 4×10 20 atoms / cm 3 , 5×10 20 atoms / cm 3 , 6×10 20 atoms / cm 3 ,7×10 20 atoms / cm 3 , 8×10 20 atoms / cm 3 , but not limited to the above.
[0094] In some embodiments, the thickness of the P-type ohmic contact layer is 1 nm to 30 nm; exemplary thicknesses of the P-type ohmic contact layer are 5 nm, 15 nm, 20 nm, 25 nm, and 30 nm, but are not limited to the above examples.
[0095] In some embodiments, the In component in the heavily Mg-doped AlInGaN layer increases along the growth direction.
[0096] Accordingly, the present invention provides a method for preparing a Micro-LED epitaxial wafer, comprising the following steps:
[0097] S1. Prepare substrate;
[0098] S2, depositing an N-type semiconductor layer, a stress release layer, a multi-quantum well light-emitting layer, a first P-type hole injection layer, a first P-type semiconductor layer, a second P-type hole injection layer, a second P-type semiconductor layer, and a P-type ohmic contact layer on the substrate in sequence;
[0099] The growth temperature of the second P-type hole injection layer is higher than the growth temperature of the first P-type hole injection layer;
[0100] A growth temperature of the second P-type semiconductor layer is higher than a growth temperature of the first P-type semiconductor layer.
[0101] In some embodiments, the growth temperature of the first P-type hole injection layer is 780° C. to 920° C., and the growth pressure is 50 torr to 360 torr;
[0102] The growth temperature of the first P-type semiconductor layer is 718° C. to 856° C., and the growth pressure is 30 torr to 500 torr;
[0103] The growth temperature of the second P-type hole injection layer is 880° C. to 1050° C., and the growth pressure is 50 torr to 360 torr;
[0104] The growth temperature of the second P-type semiconductor layer is 900° C. to 1050° C., and the growth pressure is 30 torr to 500 torr;
[0105] The growth temperature of the P-type ohmic contact layer is 850° C. to 950° C., and the growth pressure is 30 torr to 500 torr.
[0106] Correspondingly, the present invention also provides a Micro-LED, which includes the above-mentioned Micro-LED epitaxial wafer.
[0107] The present invention is further described below with specific embodiments:
[0108] Example 1
[0109] This embodiment provides a Micro-LED epitaxial wafer, including a substrate, on which an N-type semiconductor layer, a stress release layer, a multi-quantum well light-emitting layer, a first P-type hole injection layer, a first P-type semiconductor layer, a second P-type hole injection layer, a second P-type semiconductor layer, and a P-type ohmic contact layer are sequentially provided;
[0110] The growth temperature of the second P-type hole injection layer is 1000° C., and the growth temperature of the first P-type hole injection layer is 900° C.;
[0111] The growth temperature of the second P-type semiconductor layer is 1050°C, and the growth temperature of the first P-type semiconductor layer is 800°C.
[0112] The first P-type hole injection layer includes a first AlGaN layer, an AlN layer, a first AlInGaN layer, a second AlInGaN layer, a second AlGaN layer and a GaN layer stacked in sequence.
[0113] The first P-type semiconductor layer is a Mg-doped AlInGaN layer.
[0114] The second P-type hole injection layer is an AlGaN / InGaN superlattice layer.
[0115] The second P-type semiconductor layer is a Mg-doped GaN layer.
[0116] The P-type ohmic contact layer is an AlInGaN layer heavily doped with Mg.
[0117] Example 2
[0118] This embodiment provides a Micro-LED epitaxial wafer, including a substrate, on which an N-type semiconductor layer, a stress release layer, a multi-quantum well light-emitting layer, a first P-type hole injection layer, a first P-type semiconductor layer, a second P-type hole injection layer, a second P-type semiconductor layer, and a P-type ohmic contact layer are sequentially provided;
[0119] The growth temperature of the second P-type hole injection layer is 950° C., and the growth temperature of the first P-type hole injection layer is 900° C.;
[0120] The growth temperature of the second P-type semiconductor layer is 1000° C., and the growth temperature of the first P-type semiconductor layer is 800° C.
[0121] The first P-type hole injection layer includes a first AlGaN layer, an AlN layer, a first AlInGaN layer, a second AlInGaN layer, a second AlGaN layer and a GaN layer stacked in sequence.
[0122] The first P-type semiconductor layer is a Mg-doped AlInGaN layer.
[0123] The second P-type hole injection layer is an AlGaN / InGaN superlattice layer.
[0124] The second P-type semiconductor layer is a Mg-doped GaN layer.
[0125] The P-type ohmic contact layer is an AlInGaN layer heavily doped with Mg.
[0126] Example 3
[0127] This embodiment provides a Micro-LED epitaxial wafer, including a substrate, on which an N-type semiconductor layer, a stress release layer, a multi-quantum well light-emitting layer, a first P-type hole injection layer, a first P-type semiconductor layer, a second P-type hole injection layer, a second P-type semiconductor layer, and a P-type ohmic contact layer are sequentially provided;
[0128] The growth temperature of the second P-type hole injection layer is 1000° C., and the growth temperature of the first P-type hole injection layer is 920° C.;
[0129] The growth temperature of the second P-type semiconductor layer is 1050°C, and the growth temperature of the first P-type semiconductor layer is 850°C.
[0130] The first P-type hole injection layer includes a first AlGaN layer, an AlN layer, a first AlInGaN layer, a second AlInGaN layer, a second AlGaN layer and a GaN layer stacked in sequence.
[0131] The first P-type semiconductor layer is a Mg-doped AlInGaN layer.
[0132] The second P-type hole injection layer is an AlGaN / InGaN superlattice layer.
[0133] The second P-type semiconductor layer is a Mg-doped GaN layer.
[0134] The P-type ohmic contact layer is an AlInGaN layer heavily doped with Mg.
[0135] Comparative Example 1
[0136] This comparative example provides a Micro-LED epitaxial wafer, including a substrate, on which an N-type semiconductor layer, a stress release layer, a multi-quantum well light-emitting layer, an electron blocking layer, a P-type semiconductor layer, and a P-type ohmic contact layer are sequentially provided;
[0137] The electron blocking layer is an AlInGaN electron blocking layer.
[0138] The first P-type semiconductor layer is a Mg-doped GaN layer.
[0139] The P-type ohmic contact layer is an AlInGaN layer heavily doped with Mg.
[0140] The epitaxial wafers prepared in Examples 1 to 3 and Comparative Example 1 were made into 20 μm×20 μm Micro-LED chips and tested at 3 μA / 10 μA / 30 μA currents. The test results are shown in Table 1.
[0141] Table 1 Test results of Micro-LED chips prepared in Examples 1 to 3 and Comparative Example 1
[0142]
[0143] Among them, XRD (002) data can characterize screw dislocations, and XRD (102) data can characterize mixed dislocations of screw dislocations and edge dislocations. The smaller the value of XRD (002) or XRD (102), the lower the dislocation density and the better the crystal quality. Comparing the test data, it can be seen that the present invention can improve the hole injection efficiency of the P-type semiconductor layer and improve the matching degree of the electron hole concentration in the multi-quantum well light-emitting layer region, thereby improving the light efficiency of the Micro-LED chip at low operating current density.
[0144] In the description of this specification, the description with reference to the terms "some embodiments", "illustrative embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials, or characteristics described in conjunction with the embodiments or examples are included in at least one embodiment or example of the present application. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials, or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.
[0145] The above is a preferred embodiment of the invention. It should be pointed out that a person skilled in the art can make several improvements and modifications without departing from the principle of the invention. These improvements and modifications are also considered to be within the scope of protection of the invention.
Claims
1. A Micro-LED epitaxial wafer, characterized in that: It comprises a substrate, on which an N-type semiconductor layer, a stress release layer, a multi-quantum well light-emitting layer, a first P-type hole injection layer, a first P-type semiconductor layer, a second P-type hole injection layer, a second P-type semiconductor layer, and a P-type ohmic contact layer are sequentially arranged; The growth temperature of the second P-type hole injection layer is higher than the growth temperature of the first P-type hole injection layer; The growth temperature of the second P-type semiconductor layer is higher than the growth temperature of the first P-type semiconductor layer; The first P-type hole injection layer includes a first AlGaN layer, an AlN layer, a first AlInGaN layer, a second AlInGaN layer, a second AlGaN layer and a GaN layer stacked in sequence; The first P-type semiconductor layer is a Mg-doped AlInGaN layer; The second P-type hole injection layer is an AlGaN / InGaN superlattice layer; The second P-type semiconductor layer is a Mg-doped GaN layer.
2. The Micro-LED epitaxial wafer according to claim 1, characterized in that: The thickness of the first AlGaN layer is 1 nm to 16 nm; The Al composition of the first AlGaN layer is 0.25-0.75; The thickness of the AlN layer is 1 nm to 16 nm; The thickness of the first AlInGaN layer is 2nm~36nm; The Al composition of the first AlInGaN layer is 0.25-0.75; The In composition of the first AlInGaN layer is 0.01-0.06; The thickness of the second AlInGaN layer is 2nm~36nm; The Al composition of the second AlInGaN layer is 0.16-0.6; The In composition of the second AlInGaN layer is 0.02-0.08; The first AlInGaN layer is not intentionally doped, and the Mg doping concentration of the second AlInGaN layer is 2.8×10 18 atoms / cm 3 ~1.6×10 19 atoms / cm 3 ; The thickness of the second AlGaN layer is 1 nm to 16 nm; The Al composition of the second AlGaN layer is 0.25-0.75; The GaN layer is not intentionally doped, and the thickness of the GaN layer is 1 nm to 16 nm.
3. The Micro-LED epitaxial wafer according to claim 2, characterized in that: The Al composition of the first AlInGaN layer is greater than the Al composition of the second AlInGaN layer; The In composition of the first AlInGaN layer is smaller than the In composition of the second AlInGaN layer.
4. The Micro-LED epitaxial wafer according to claim 1, wherein: The Mg doping concentration of the first P-type semiconductor layer is 1.5×10 19 atoms / cm 3 ~3.6×10 20 atoms / cm 3 ; The thickness of the first P-type semiconductor layer is 8nm-250nm; The Al component in the first P-type semiconductor layer decreases along the growth direction; The Mg doping concentration in the first P-type semiconductor layer decreases along the growth direction.
5. The Micro-LED epitaxial wafer according to claim 1, wherein: The AlGaN / InGaN superlattice layer includes an AlGaN layer and a Mg-doped InGaN layer alternately stacked, and the number of alternating periods is 3 to 25; The thickness of the AlGaN layer is 1.2nm~7.5nm; The Al composition of the AlGaN layer is 0.25-0.6; The thickness of the Mg-doped InGaN layer is 1.2 nm to 7.5 nm; The In component of the Mg-doped InGaN layer is 0.02-0.1; The Mg doping concentration of the Mg-doped InGaN layer is 3.2×10 18 atoms / cm 3 ~2.5×10 19 atoms / cm 3 .
6. The Micro-LED epitaxial wafer according to claim 1, characterized in that: The Mg doping concentration of the second P-type semiconductor layer is 1.2×10 19 atoms / cm 3 ~2.5×10 20 atoms / cm 3 ; The thickness of the second P-type semiconductor layer is 6nm-200nm; The Mg doping concentration in the second P-type semiconductor layer decreases along the growth direction.
7. The Micro-LED epitaxial wafer according to claim 1, characterized in that: The P-type ohmic contact layer is an AlInGaN layer heavily doped with Mg; The Mg doping concentration of the P-type ohmic contact layer is 3.2×10 19 atoms / cm 3 ~8.5×10 20 atoms / cm 3 ; The thickness of the P-type ohmic contact layer is 1nm~30nm; The In component in the heavily Mg-doped AlInGaN layer increases gradually along the growth direction.
8. A method for preparing a Micro-LED epitaxial wafer according to any one of claims 1 to 7, characterized in that: The following steps are involved: S1. Prepare substrate; S2, depositing an N-type semiconductor layer, a stress release layer, a multi-quantum well light-emitting layer, a first P-type hole injection layer, a first P-type semiconductor layer, a second P-type hole injection layer, a second P-type semiconductor layer, and a P-type ohmic contact layer on the substrate in sequence; The growth temperature of the second P-type hole injection layer is higher than the growth temperature of the first P-type hole injection layer; A growth temperature of the second P-type semiconductor layer is higher than a growth temperature of the first P-type semiconductor layer.
9. A Micro-LED, characterized in that: The Micro-LED includes the Micro-LED epitaxial wafer as described in any one of claims 1 to 7.