Preparation and application of Ti3C2Tx MXene-based conductive antibacterial hydrogel dressing

By using Ti3C2Tx MXene-based conductive antibacterial hydrogel in diabetic chronic wound dressings, combined with photothermal therapy and electrical stimulation, the problem of existing dressings being difficult to be antibacterial and promoting healing at the same time is solved, achieving efficient wound healing and bacterial killing. And has good safety and sensing performance.

CN118718080APending Publication Date: 2024-10-01HAINAN UNIV
View PDF 0 Cites 4 Cited by

Patent Information

Application Number
CN202410788916.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-19
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

It is difficult for existing diabetic chronic wound dressings to achieve antibacterial, anti-inflammatory and healing promotion at the same time, and the use of antibiotics leads to bacterial resistance and toxic side effects, and there is a lack of effective multi-functional dressings.

Method used

Ti3C2Tx MXene-based conductive antibacterial hydrogel is used to form a hydrogel through the coupling of oxidized sodium alginate and acrylamide, in which MXene nanosheets are incorporated as photothermal agents and conductive fillers, and photothermal therapy and electrical stimulation are combined to kill Kills bacteria and promotes cell proliferation.

Benefits of technology

It achieves efficient bacterial killing and wound healing, accelerates the healing process of diabetic chronic wounds, causes little damage to normal cells, and has good stretch sensitivity and sensing performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118718080A_ABST
    Figure CN118718080A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of medical treatment, and particularly relates to preparation and application of a Ti3C2Tx MXene-based conductive antibacterial hydrogel dressing. In a preparation method, firstly, oxidized sodium alginate is prepared; then, synthesizing an MXene nanosheet; dissolving 4 parts by mass of oxidized sodium alginate and 20 parts by mass of acrylamide in 30 parts by mass of ultrapure water under stirring, dropwise adding 5 parts by mass of 0.1 Mol / L NaOH solution after the oxidized sodium alginate and the acrylamide are completely dissolved, and stirring for 20 minutes; a solution A is obtained; adding water into the MXene nanosheet, and fusing to obtain an MXene solution with the concentration of 0.5%, so as to obtain a solution B; finally, mixing the solution A and the solution B according to the volume ratio of 1: 1, and then adding 10 parts by mass of ammonium persulfate and 10 parts by mass of tetramethylethylenediamine; transferring the gel precursor into a mold, and reacting at room temperature for 30 seconds to realize gelation, so as to obtain the conductive antibacterial hydrogel. The Ti < 3 > C < 2 > T < x > MXene-based conductive antibacterial hydrogel disclosed by the invention is applied to preparation of wound dressing medicines and sensing materials for treating diabetes mellitus.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of medical technology, and in particular relates to the preparation and application of a Ti3C2Tx MXene-based conductive antibacterial hydrogel dressing. Background Art

[0002] Diabetes is a chronic metabolic disorder characterized by high blood sugar levels that affects tens of thousands of people around the world; according to the World Health Organization, there are currently 422 million people with diabetes, approximately 1.6 million people die each year, and diabetes will become the seventh leading cause of death by 2030. Diabetic foot ulcers are lesions that form on the foot and are unable to undergo the normal wound healing process. They are a chronic, difficult-to-heal complication of diabetes that can lead to lower limb amputation or even death, placing a heavy burden on patients and the healthcare system.

[0003] The microenvironment of diabetic wounds is complex, including hyperglycemia, hypoxia and chronic inflammation. Due to the long inflammation period and reduced angiogenesis, the nutrient supply is insufficient, the endothelial cell function is damaged, and the high sugar environment is conducive to bacterial growth. Methicillin-resistant Staphylococcus aureus (MRSA) is one of the main terrible clinical pathogens that cause life-threatening diseases such as acute endocarditis and sepsis. Once multidrug-resistant MDR bacteria invade the damaged parts of human skin, it will cause severe infection in the skin wounds exposed to the air and difficult to heal. Therefore, the healing process of diabetic wounds is greatly hindered.

[0004] Wound dressings come in many forms; however, their suitability varies depending on the characteristics of the wound; dressing selection depends on several variables, including depth, location, size, amount of exudate, inflammation, and adhesion to the wound; wet dressings have the ability to enhance the wound repair process compared to dry dressings; moisturizing dressings can protect the wound, reduce the risk of infection, and promote granulation tissue formation; these materials are classified as gauze, film, or gel based on their physical properties; dry dressings may adhere to the wound, causing additional pain and tissue damage.

[0005] As the number of diabetic patients increases worldwide, the demand for care and treatment of chronic wounds closely related to it is also increasing; due to the extensive use of antibiotics, multidrug-resistant (MDR) strains have begun to appear. MDR strains make infection treatment more difficult and increase the risk of transmission, threatening public health. Among the many medical products for treating wound infections, medical dressings including hydrogels can prevent bacterial infection to a certain extent through barrier effects. Although chronic inflammation can be relieved by adding antibiotics, anti-inflammatory drugs and growth factors to dressings, these bioactive drugs are easily inactivated, easily cause bacterial resistance and have non-negligible toxic side effects, making medical dressings incapable of combating diabetic chronic wounds. At present, there are very few studies and products on multifunctional dressings that are both antibacterial and anti-inflammatory and promote healing for diabetic chronic wounds.

[0006] To this end, the present invention starts from the characteristics of chronic wounds and discloses a medical hydrogel dressing for diabetic chronic wounds, which uses PTT to kill bacteria in the wound and uses ES to promote cell proliferation and accelerate wound healing. Summary of the invention

[0007] The purpose of the present invention is to provide the preparation and application of Ti3C2Tx MXene-based conductive antibacterial hydrogel dressings, which are medical hydrogel dressings for diabetic chronic wounds, use PTT to kill bacteria in the wound, use ES to promote cell proliferation, and accelerate wound healing.

[0008] The technical solution adopted by the present invention is as follows:

[0009] The preparation of Ti3C2Tx MXene-based conductive antibacterial hydrogel dressing includes the following steps:

[0010] Step 1: preparing oxidized sodium alginate;

[0011] Step 2: Synthesis of MXene nanosheets;

[0012] Step 3: 4 parts by mass of oxidized sodium alginate and 20 parts by mass of acrylamide are dissolved in 30 parts by mass of ultrapure water under stirring, and after they are completely dissolved, 5 parts by mass of 0.1Mol / L NaOH solution are added dropwise, and stirred for 20 minutes to obtain solution A;

[0013] Step 4: Add water to the MXene nanosheets obtained in step 2 to obtain a 0.5% MXene solution to obtain solution B;

[0014] Step 5: Mix solution A and solution B in a volume ratio of 1:1, and then add 10 parts by mass of ammonium persulfate and 10 parts by mass of tetramethylethylenediamine; ammonium persulfate and tetramethylethylenediamine are used to stabilize free radicals and promote free radical polymerization of AM; transfer the gel precursor to the mold, react at room temperature for 30 seconds to achieve gelation, and obtain a conductive antibacterial hydrogel.

[0015] Preferably, the specific steps of preparing oxidized sodium alginate in step 1 are as follows:

[0016] Step 101: Disperse 10 g of sodium alginate in 50 mL of ethanol, and then add 50 mL of water containing 10 g of sodium periodate to the solution;

[0017] Step 102: magnetically stirring the mixture in a dark environment at 25° C. for a certain period of time;

[0018] Step 103: Add 5 mL of ethylene glycol and stir for a certain period of time to stop the reaction;

[0019] Step 104: Pour 500 mL of ethanol into the reaction mixture; collect the precipitate by suction filtration;

[0020] Step 105: The crude oxidized sodium alginate is dialyzed with deionized water for 3 days, and then freeze-dried to obtain a spongy oxidized sodium alginate solid.

[0021] Preferably, the magnetic stirring time in step 102 is 5 hours; and the stirring time in step 103 is 2 hours.

[0022] Preferably, in step 2, the specific steps of synthesizing MXene nanosheets are as follows:

[0023] Step 201: 1.6 g of LiF was added to 20 mL of 9 M hydrochloric acid solution, and the mixture solution was stirred for 30 min using a magnetic stirrer to form a uniform solution;

[0024] Step 202: slowly add 1 g of Ti3AlC2 powder into the solution to avoid strong heat release;

[0025] Step 203: Transfer the reaction bottle to an oil bath and continue stirring for a certain period of time;

[0026] Step 204: Centrifuge the resulting dispersion for one cycle to obtain a multilayer Ti3C2T x MXene;

[0027] Step 205: washing the obtained precipitate with a diluted HCl solution and centrifuging again;

[0028] Step 206: washing the sediment with deionized water and repeating the centrifugation until the pH value of the supernatant reaches 5-6;

[0029] Step 207: Wash the multilayer Ti3C2T x Disperse with 20 mL of deionized water, crush for a certain period of time, and finally freeze-dry to obtain MXene nanosheets.

[0030] Preferably, the oil bath temperature in step 203 is 35° C., and the continuous stirring time is 24 h.

[0031] Preferably, in step 207, ultrasonic crushing is used for crushing, and the crushing time is 6 hours; freeze drying is performed by a freeze dryer, and the freeze drying time is 36 hours;

[0032] Ti3C2T x Application of MXene-based conductive antibacterial hydrogels in the preparation of drugs and sensing materials for the treatment of diabetic wound dressings.

[0033] The technical effects achieved by the present invention are:

[0034] In this invention, based on the characteristics of diabetic wounds, a Ti3C2T x MXene's conductive antibacterial hydrogel is used to treat diabetic infected wounds. The structural advantage of the hydrogel's high water content maintains a moist wound healing environment and relieves wound discomfort. At the same time, the photothermal properties and conductive advantages of the hydrogel are used to kill bacteria in the wound, promote cell proliferation, and accelerate wound healing.

[0035] In the present invention, first, oxidized sodium alginate (OSA) is coupled with acrylamide (AM) through Schiff base bonds, and free radical polymerization between OSA side chain double bonds and free AM monomers leads to the formation of oxidized sodium alginate-polyacrylamide (OSA-PAM) hydrogel. The synergistic effect of dynamic Schiff base bonds and hydrogen bonding interactions between OSA and PAM chains endows OSA-PAM hydrogel with excellent mechanical properties. Then, MXene is incorporated into the hydrogel precursor solution as a photothermal agent and conductive filler, and the resulting POM hydrogel also exhibits excellent photothermal properties, controllable conductivity and stretch sensitivity.

[0036] In the present invention, through in vitro experiments, it is proved that POM hydrogel has excellent photothermal antibacterial effect, with a sterilization rate of more than 99%; by utilizing its good conductivity, applying electrical stimulation during cell culture, its ability to promote cell proliferation and cell migration can be clearly observed; at the same time, it has good tensile sensitivity and can be used as a piezoresistive sensor to monitor human body movements and facial micro-expressions. In the MRSA-infected chronic wound mouse model, after applying laser and electrical stimulation treatment using POM hydrogel, good antibacterial effect and healing promotion effect were achieved, the possibility of microbial resistance was low, and the damage to normal cells was small; therefore, POM hydrogel provides a new solution for killing bacteria in vivo and promoting skin wound healing.

[0037] In the present invention, according to existing reports, the safe power of 808nm laser is 0.33W / cm 2 , the safe power of 1064nm laser is 1W / cm 2 ; Usually in the PTT treatment process, the laser wavelength used is mostly 808nm, and the power density is relatively high; the present invention uses 1064nm laser to be used for Ti3C2T x The hydrogel based on MXene nanosheets kills MDR bacteria while ensuring the safety of laser power to the human body; the hydrogel synthesized by the present invention has the characteristics of high toughness and high stretchability. Compared with hydrogels of similar applications, most of which have a stretching rate of less than 1000%, the POM hydrogel has a stronger stretching rate, which can reach 2470%. It is not easy to be damaged in the process of covering wounds and detecting human body movements, showing its stretchability and durability. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1 is a schematic diagram of the synthesis of POM hydrogel in Example 1 of the present invention;

[0039] Figure 2 is a synthetic chemical formula diagram of OSA in Example 1 of the present invention;

[0040] Figure 3 FTIR graphs of SA, OSA and OSA-AM in Example 1 of the present invention;

[0041] Figure 4 is the XRD pattern of the MXene nanosheet in Example 1 of the present invention;

[0042] Figure 5 is a DLS graph of the MXene nanosheet in Example 1 of the present invention;

[0043] Figure 6 is a SEM image of the MXene nanosheet in Example 1 of the present invention;

[0044] Figure 7 is a UV-vis graph of the MXene nanosheet in Example 1 of the present invention;

[0045] Figure 8 This is a photograph of PO and POM hydrogel formation in Example 1 of the present invention;

[0046] Fig. 9 is a scanning electron microscope image of PO and POM hydrogels in Example 1 of the present invention;

[0047] Fig.10 1 is an EDS distribution diagram of the POM hydrogel with a scale of 10 μm and elements of C, O, N, Ti, and Na respectively in Example 1 of the present invention;

[0048] Fig.11 is a compressive stress-strain curve of the PO hydrogel in Example 1 of the present invention;

[0049] Fig.12 is a tensile stress-strain curve of the PO hydrogel in Example 1 of the present invention;

[0050] Fig.13 is a tensile stress-strain curve diagram of the POM hydrogel in Example 1 of the present invention;

[0051] Fig.14 is an adhesion strength curve of the hydrogel in Example 1 of the present invention;

[0052] Fig.15 Schematic diagram of the adhesion ability of POM hydrogel in Example 1 of the present invention;

[0053] Fig.16 is the conductivity diagram of the POM hydrogel in Example 2 of the present invention;

[0054] Fig.17 This is a schematic diagram of a circuit based on 0.5% POM hydrogel in Example 2 of the present invention;

[0055] Fig.18 It is a temperature rise curve of 0.5% POM hydrogel under 1064nm laser irradiation in Example 2 of the present invention;

[0056] Fig.19 This is a photothermal temperature rise curve of the POM hydrogel in Example 2 of the present invention;

[0057] Fig. 20 It is a line graph for calculating the photothermal conversion efficiency of 0.5% POM hydrogel in Example 2 of the present invention;

[0058] Fig.21 is a graph of relative resistance changes when the finger is bent at different angles in the second embodiment of the present invention;

[0059] Fig. 22 is a graph showing the relative resistance change when the wrist is repeatedly bent in the second embodiment of the present invention;

[0060] Fig.23 is a graph of relative resistance changes of angry and surprised expressions in Example 2 of the present invention;

[0061] Fig.24 is a graph of relative resistance changes of smiling and laughing expressions in Example 2 of the present invention;

[0062] Fig.25 is a graph of relative resistance change of saliva swallowing in Example 2 of the present invention;

[0063] Fig.26 is a graph showing a relative resistance change when the word China is spoken in the second embodiment of the present invention;

[0064] Fig. 27 This is a schematic diagram of operating a mobile phone screen in Embodiment 2 of the present invention;

[0065] Fig.28 This is a photo of the dilution plate coating of MDRE.coli and MASR in Example 2 of the present invention;

[0066] Fig.29 is a statistical graph of the survival rate of MDRE.coli in Example 2 of the present invention;

[0067] Fig.30 is a statistical graph of the survival rate of MASR in Example 2 of the present invention;

[0068] Fig.31 is the live / dead staining image of MDRE.coli and MRSA at a scale of 75 μm in Example 2 of the present invention;

[0069] Fig.32 This is a graph of the toxicity of the hydrogel to L929 cells measured by MTT in Example 2 of the present invention;

[0070] Fig.33 is a live / dead staining image of L929 cells in Example 2 of the present invention with a scale of 100 μm;

[0071] Fig.34 This is a diagram of the in vitro proliferation of fibroblasts after electrical stimulation in Example 2 of the present invention with a scale of 250 μm;

[0072] Fig.35 is an in vitro scratch microscope image with a scale of 200 μm in Example 2 of the present invention;

[0073] Fig.36This is a diagram of wound healing in Example 2 of the present invention with a scale of 2 mm;

[0074] Fig.37 is a statistical diagram of the remaining wound area in the second embodiment of the present invention;

[0075] Fig.38 is an H&E staining image of the wound tissue in Example 2 of the present invention;

[0076] Fig.39 This is a Masson staining image of the wound tissue in Example 2 of the present invention. DETAILED DESCRIPTION

[0077] In order to make the purpose and advantages of the present invention more clearly understood, the present invention is specifically described below in conjunction with embodiments. It should be understood that the following text is only used to describe one or several specific embodiments of the present invention, and does not strictly limit the scope of protection of the specific claims of the present invention.

[0078] like Figure 1 As shown, the preparation of Ti3C2Tx MXene-based conductive antibacterial hydrogel dressing includes the following steps:

[0079] Step 1: preparing oxidized sodium alginate;

[0080] Disperse 10g of sodium alginate in 50mL of ethanol, then add 50mL of water containing 10g of sodium periodate to the above solution; stir the mixture magnetically in a dark environment at 25°C for 5h; add 5mL of ethylene glycol and stir for another 2h to stop the reaction; pour 500mL of ethanol into the reaction mixture; collect the precipitate by suction filtration; dialyze the crude oxidized sodium alginate with deionized water for 3 days, and freeze-dry it in a freeze dryer for 1h; obtain a spongy oxidized sodium alginate solid, the reaction formula is as follows: Figure 2 As shown;

[0081] In the present invention, oxidized sodium alginate is referred to as OSA in English; sodium alginate is referred to as SA in English; acrylamide is referred to as AM in English; the present invention explores the characterization of OSA in the following aspects: Figure 3 In the infrared spectrum shown in the figure, it is observed that the absorption curve of OSA is different from that of SA at 1732 cm -1 There is a small absorption peak at 1732 cm -1 , which verifies that the hydroxyl groups on the sodium alginate have been successfully oxidized to generate aldehyde groups; after OSA and AM are combined, 1732cm -1 The peak at 1610cm -1 The sharp peak at 1670 cm-1 corresponds to the stretching vibration of C=N. -1The sharp peak at corresponds to the stretching vibration of C=C, indicating that the aldehyde group in OSA and the amino group in AM are successfully combined through Schiff base bonds;

[0082] Step 2: Synthesis of MXene nanosheets;

[0083] 1.6 g LiF was added to 20 mL of 9 M hydrochloric acid solution, and the mixture solution was stirred for 30 min using a magnetic stirrer to form a uniform solution; 1 g Ti3AlC2 powder was slowly added to the solution to avoid strong heat release; the reaction bottle was transferred to a 35 °C oil bath and stirred continuously for 24 h; the resulting dispersion was centrifuged for one cycle to obtain multilayer Ti3C2T x MXene; the obtained precipitate was washed with a diluted HCl solution and centrifuged again; the precipitate was washed with deionized water and centrifuged repeatedly until the pH value of the supernatant reached 5-6; the washed multilayer Ti3C2T x Disperse with 20 mL of deionized water, crush by ultrasonication, crush for 6 hours, and finally freeze-dry to obtain MXene nanosheets.

[0084] The present invention explores the characterization of MXene nanosheets; MXene nanosheets are prepared by strong acid etching plus ultrasonic exfoliation; XRD Figure 4 The analysis shown in the figure shows that after etching Ti3AlC2 with a strong acid solution, the peak originally located at 10° shifted, and the peaks at 38° and 60° disappeared, indicating that the present invention has successfully etched away the Al layer in the MAX phase of Ti3AlC2; after the nanosheets were peeled off by ultrasound, DLS of MXene solutions of different concentrations was obtained; Figure 5 From the test results shown, it can be seen that the obtained Ti3C2T x The size of nanosheets is 100-200nm; from Ti3C2T x SEM images of nanosheets, such as Figure 6 As shown in the above observation, the size of the nanosheets is relatively uniform, which can also confirm that Ti3C2T x The size of the nanosheets is 100-200nm; through the UV-visible absorption spectra of MXene solutions of different concentrations, such as Figure 7 As shown, Ti3C2T x The nanosheets have a maximum absorption peak at 760nm and an absorption peak at 970nm. As the concentration of MXene increases, the UV absorption peak also increases.

[0085] In the present invention, PO hydrogel (without adding MXene) was prepared according to the material ratio in Table 1; it was found through experiments that in group 1, when the amount of OSA added was 0, pure AM could only form a viscous liquid and could not cross-link to form a hydrogel; in groups 2, 3, 4, and 5, after adding OSA, they could react quickly to form a hydrogel, because OSA was combined with AM through Schiff base bonds, increasing the cross-linking sites, and the long chains of OSA and PAM were physically entangled to form a cross-linking network; with the increase of the amount of OSA added, the morphology of the hydrogel gradually became softer, more elastic, and more viscous; but when the amount of OSA added in group 6 reached 0.4g, only a viscous liquid body could be formed, and gelation could not be formed; this may be because with the increase of the amount of OSA, the amount of aldehyde group increases accordingly, most of the AM is combined with OSA, the free AM becomes less, and the formed PAM long chain decreases, so gelation cannot be formed.

[0086]

[0087] Table 1: Hydrogel material ratio

[0088] Step 3: 4 parts by mass of oxidized sodium alginate and 20 parts by mass of acrylamide are dissolved in 30 parts by mass of ultrapure water under stirring, and after they are completely dissolved, 5 parts by mass of 0.1Mol / L NaOH solution are added dropwise, and stirred for 20 minutes to obtain solution A;

[0089] Step 4: Add water to the MXene nanosheets obtained in step 2 to obtain a 0.5% MXene solution to obtain solution B;

[0090] Step 5: Mix solution A and solution B in a volume ratio of 1:1, and then add 10 parts by mass of ammonium persulfate and 10 parts by mass of tetramethylethylenediamine; ammonium persulfate and tetramethylethylenediamine are used to stabilize free radicals and promote free radical polymerization of AM; transfer the gel precursor to the mold, react at room temperature for 30 seconds to achieve gelation, and obtain a conductive antibacterial hydrogel; Figure 8 shown.

[0091] In the present invention, the microstructure characterization of the hydrogels was investigated; the micromorphology of PO and POM hydrogels was identified by SEM images; all hydrogels showed obvious 3D porous structures, such as Fig. 9 As shown in the figure, this porous structure is conducive to the incorporation of conductive fillers, and the porous structure has a great relationship with maintaining the structural stability of the hydrogel and giving it mechanical properties; compared with the image of PO hydrogel, some Ti3C2T xNanosheets; characteristic peaks of C, O, N, Ti, and Na can be detected in the energy spectrum (EDS) of POM hydrogel, and the EDS element distribution map; Fig.10 As shown, Ti3C2T x The nanosheets are evenly distributed in the POM hydrogel.

[0092] In the present invention, the mechanical characterization of the hydrogel is investigated; Fig.11 As shown in the figure, it is the stress-strain curve of PO hydrogel under compression; the compressive strength of PO hydrogel increases with the increase of OSA content, and decreases with the further increase of OSA content after reaching the maximum value; the presence of an appropriate amount of OSA template will cross-link the PAM chain to tighten the anti-compression network structure; Fig.12 As shown, the stress-strain curve of PO hydrogel during stretching is shown; the tensile strength of PO hydrogel increases with the increase of OSA content, and after reaching the maximum value, it decreases with the further increase of OSA content; Fig.13 As shown in the figure, when the MXene concentration is 0.5%, the mechanical properties of the hydrogel are enhanced and the tensile strain increases; when the MXene concentration continues to increase to 1%, the tensile strain decreases due to the excessively high content.

[0093] In the present invention, the adhesion performance of the hydrogel is investigated; the good adhesion performance of the hydrogel can make the hydrogel and the skin fit closely together, prevent bacteria in the external environment from further infecting the wound, and confine the bacteria in the wound to the hydrogel. An electronic universal testing machine is used to perform a lap shear test, and the hydrogel is adhered to the pig skin to measure the adhesion of the hydrogel to the pig skin. Fig.15 As shown in Figure 2, 0.5% POM exhibits good adhesion and has a certain adhesion to human skin, glass, metal, and plastic; Fig.16 As shown, this adhesion may be related to the amino, hydroxyl and a small amount of aldehyde groups on the surface of the hydrogel, which can adhere to the amino groups on the skin surface by forming hydrogen bonds.

[0094] Embodiment 2:

[0095] Ti3C2T x Application of MXene-based conductive antibacterial hydrogels in the preparation of drugs and sensing materials for the treatment of diabetic wound dressings.

[0096] In the present invention, the conductive properties of POM hydrogels are investigated; the conductivity of POM hydrogels with different MXene contents is measured; Fig.16As shown in Figure 2, it was found that the conductivity was significantly improved after adding MXene to the hydrogel, and as the MXene content increased, the conductivity also increased. This may be because the increase in the contact area between the MXene nanosheets improved the conductive path inside the hydrogel, thereby increasing the conductivity of the hydrogel; Fig.17 As shown, 0.5% POM hydrogel is connected to the LED light bulb circuit. After the wire contacts the hydrogel, the LED light bulb can be successfully lit, indicating that POM hydrogel has good conductive properties. The conductivity of these hydrogels is mainly attributed to the conductive properties of MXene nanosheets. It can be used in electrical stimulation therapy to promote cell proliferation and differentiation at the wound, and can also be used in flexible electronic devices to collect human movement and expression information.

[0097] In the present invention, the photothermal performance characterization of the hydrogel is investigated; an infrared thermal imager is used to detect the photothermal effect of the hydrogel under a 1064nm laser, and the temperature is recorded every 30s for 10 minutes; the thermal image can intuitively present the temperature changes, such as Fig.18 As shown, at 0.6, 0.7, 0.8, 0.9 W / cm 2 There is a photothermal effect at a power density of 0.9W / cm. As the power density increases, the final temperature of the photothermal system will also increase. 2 Finally, it reached 95°C; according to the curve, the present invention found that the temperature of the hydrogel rose rapidly in the initial 30s, rose slightly in 30-100s, and stabilized after 100s; Fig.19 as well as Fig. 20 As shown, the hydrogel is at 0.8W / cm 2 The temperature changes of hydrogels with different MXene concentrations are shown under laser irradiation; the temperature of PO hydrogel remained basically unchanged after 10 minutes of laser irradiation, and there was no photothermal effect; while 0.5% POM and 1% POM both heated up rapidly after laser irradiation, and finally stabilized at around 60°C, with no obvious difference, indicating that POM hydrogel has excellent and stable photothermal effect, and its photothermal performance will not be further improved after MXene reaches a certain concentration; it is calculated that the photothermal conversion efficiency is 52.1% under 1064nm laser irradiation.

[0098] In the present invention, the electrical sensing performance test was conducted. Since the 0.5% POM hydrogel has strong adhesion ability, excellent toughness and stretching ability, good conductivity and rapid responsiveness of electrical signals, the hydrogel has the potential to be used as a wearable strain sensor for detecting human body movements and facial micro-expressions; Fig.21 As shown in the figure, the hydrogel is attached to the finger, bent at a fixed angle and left for a period of time, and the relative resistance changes at different angles can be observed. The hydrogel is fixed on the wrist; as shown in the figure Fig. 22 As shown in the figure, the relative resistance change can also be detected after repeated bending; obviously, the 0.5% POM hydrogel strain sensor can accurately detect the movement of human joints and display it as an electrical signal; in addition to having a good response to large-scale movements such as human joint activities, it can also respond to small movements, such as sticking it to the forehead; Fig.23 As shown in FIG. 1 , it is used to detect the change between facial expressions of anger (frown) and surprise (raised eyebrows); it is attached to the cheek; Fig.24 As shown, it is used to detect changes in facial expressions such as smiling and laughing; it is attached to the throat, such as Fig.25 as well as Fig.26 As shown in the figure, it can detect the changes in electrical signals when swallowing and speaking the word China; finally, POM hydrogel can also be used as an electronic skin to touch the mobile phone screen; Fig. 27 As shown, click and slide accurately.

[0099] In the present invention, the in vitro antibacterial activity of POM hydrogel was explored. Based on the above performance tests on POM hydrogel, the 0.5% POM group was selected as the best group. Gram-negative multidrug-resistant Escherichia coli (MDRE.coli) and Gram-positive methicillin-resistant Staphylococcus aureus (MRSA) were used to evaluate the in vitro antibacterial activity. Specifically, the bacterial suspension cultured to an OD value of 0.5 was diluted 10 times, 500 μL was taken and dropped onto the surface of the hydrogel, and then irradiated with a 1064 nm laser at 0.8 W / cm -2 The bacterial suspension was sampled and diluted to 1×10 4 The diluted suspension was then plated on solid LB medium and cultured at 37°C for 14 h. The number of colonies was counted and normalized to that of the untreated control. Three independent replicates were performed for each experiment.

[0100] The antibacterial effect of POM hydrogel on Escherichia coli and Staphylococcus aureus can be seen. Fig.28 As shown in the figure, it can be seen that the number of bacteria in the hydrogel-treated group irradiated with near-infrared light was significantly reduced compared with the first two groups; the control group and the PO group irradiated with near-infrared light; and the killing rate for these two drug-resistant bacteria reached more than 99%, as shown in the figure. Fig.29 as well as Fig.30 In addition, the viability of the two bacteria before and after interaction with POM hydrogel was evaluated by fluorescence staining, as shown in Fig.31 As shown; after 10 minutes of treatment, MRSA grew well in the control group, but both bacteria showed more red fluorescence in the hydrogel-treated group irradiated with near-infrared light; Fig.31As shown, it indicates that most of the bacteria have been killed; the above results show that POM hydrogel has a very significant bactericidal effect on MDRE.coli and MASR under the irradiation of 1064nm laser, mainly because the high heat generated by the hydrogel under laser irradiation denatures the bacterial protein.

[0101] In the present invention, cytotoxicity and cell proliferation were evaluated; To further study the biocompatibility of POM hydrogels in vitro, a standard MTT assay was performed to test the effect of in vitro cytotoxicity on L929 cells; Fig.32 As shown, in Fig.33 In the experiment, live-dead staining was performed on L929 cells after co-culture with the hydrogel for 1 day, and it was found that the cells were in good survival state, which was consistent with the results shown by MTT; the results showed that the prepared hydrogel exhibited excellent biocompatibility and could avoid negative effects in subsequent in vivo experiments.

[0102] In the present invention, in vitro electrical stimulation of cells is investigated. Skin tissue is sensitive to electricity, and conductive dressings can promote cell adhesion, proliferation, migration and differentiation, which is beneficial to accelerate wound healing. Therefore, the excellent conductivity of POM hydrogel is utilized to apply electrical stimulation to promote fibroblast proliferation and promote skin wound healing. Fig.34 As shown in the figure, the effect of electrical stimulation (ES) on fibroblast proliferation was studied; the number of cells in the POM+ES (hydrogel plus electrical stimulation) group was significantly higher than that in other groups, indicating that POM+ES can promote cell proliferation; at the same time, the results of the in vitro scratch test showed that Fig.35 As shown, it is obvious that the POM+ES group had the highest scratch closure rate within 24 hours, indicating the promoting effect of POM+ES in cell migration; these results show that POM hydrogel has a strong pro-healing effect and can significantly accelerate the proliferation and migration of fibroblasts through electrical stimulation, which is beneficial to promote wound healing.

[0103] In the present invention, the in vivo evaluation of POM hydrogel was conducted by constructing a diabetic mouse model using streptozotocin solution. If the blood glucose concentration of the mice was higher than 16.7 mmol / L for 3 consecutive days, the model was successfully established. Then, a diabetic wound infection model was further constructed. 10 μL of MRSA bacterial solution (1×10 8CFU / mL) was dripped onto the wound. After the bacterial solution was absorbed by the wound, a breathable sealing film was attached and incubated in a closed environment for 24 hours before treatment began. The mice were randomly divided into 6 groups: the Blank group was covered with a breathable sealing film; the 3M commercial hydrogel group was covered with 3M commercial hydrogel; the POM hydrogel group was covered with POM hydrogel; the POM+NIR group was covered with POM hydrogel, and then irradiated with 1064nm laser for 10min; the POM+ES group was covered with POM hydrogel, and then a DC power supply was used to give an electrical stimulation of 150mV for 15min; the POM+NIR+ES group was covered with POM hydrogel, and then a DC power supply was used to give an electrical stimulation of 150mV for 15min, and then irradiated with 1064nm laser for 10min; the healing of the mouse wounds was observed and photographed every day, and the mouse wounds were drawn and the area was counted using ImageJ. The results are as follows Fig.36 As shown in the figure, after treatment on day 0, the wound healing of mice was observed and recorded. It was found that on the third day, the wound healing effect of the POM+ES+NIR group was significantly better than that of the other groups, and the control group and the 3M group had the slowest healing speed. Within 14 days, the wound site of the POM+ES+NIR group was basically covered by smooth newly generated skin (only 0.36% remained). In comparison, the wounds of the other groups healed slightly slower ( Fig.32 ), 22.5%, 30%, 17.5%, 13.3%, and 2.44% of the Blank group, 3M commercial hydrogel group, POM hydrogel group, POM+NIR group, and POM+ES group, respectively, remained to be further cured; Fig.37 As shown in the figure; this wound healing result proves that POM hydrogel has efficient bactericidal activity under 1064nm laser irradiation, and after 150mV, 10min electrical stimulation, it promotes cell proliferation and cell migration, so that wound healing is accelerated; on the 3rd, 7th and 14th days, one mouse in each group was killed, and the wound tissue was taken out and immersed in 4% paraformaldehyde solution, and then embedded in paraffin and sliced ​​for histological evaluation by hematoxylin / eosin (H&E) and Masson staining; as shown in the figure Fig.38 As shown in the figure, the recovery of mouse skin wound tissue was detected by H&E staining. It was observed that on the 3rd day, all groups had severe inflammatory reactions. On the 7th and 14th days, the inflammation in the POM+ES+NIR group subsided significantly, subcutaneous hemorrhage regenerated blood vessels, and gradually generated hair follicle tissue. The fibroblasts in other groups also proliferated to varying degrees. The wound tissue was observed by Masson staining, as shown in the figure. Fig.39As shown, on the 14th day, skin tissue sections of the POM+ES+NIR treatment group showed complete granulation, hair follicles and connective tissue, and regeneration of collagen fibers in the wound surface; while the other groups still had varying degrees of inflammation and less granulation; these results indicate that POM hydrogel can kill invading bacteria and promote wound healing through PTT and ES treatment under 1064nm laser irradiation and electrical stimulation.

[0104] In the present invention, compared with the hydrogel in the prior art, the present invention utilizes the excellent photothermal conversion ability of MXene, and the hydrogel developed thereby has significant photothermal antibacterial ability; since POM hydrogel has good near-infrared photothermal effect, the photothermal temperature can reach above 60°C, and the photothermal conversion efficiency is also higher. In antibacterial research, the inhibitory effect of POM hydrogel on multidrug-resistant Escherichia coli and methicillin-resistant Staphylococcus aureus is as high as more than 99%; according to existing literature and FDA reports, the safe power of 808nm laser is 0.33W / cm 2 , the safe power of 1064nm laser is 1W / cm 2 The laser used in the present invention is 1064 nm, with a power of 0.8 W / cm 2 ,In the in vivo wound healing experiment, it was proved that POM hydrogel could promote the healing speed of the wound, while also ensuring the safety of the laser to the human body, as shown in Table 2;

[0105]

[0106] Table 2 is a comparison of the photothermal effects of the hydrogels of the present invention and those reported recently.

[0107] In the present invention, POM hydrogel exhibits good electrical conductivity (conductivity reaches 6×10 -2 S / m), provides a conductive path when used as a piezoresistive sensor, can show corresponding electrical signal changes as the human body moves, and exhibits good sensing performance, as shown in Table 3;

[0108] Hydrogel Conductivity Patents / Literature CEC / PF / CNT2 <![CDATA[2.6×10 -3 S / m]]> Existing Literature1 CMCS / THB / Cu / GB2 <![CDATA[5.04×10 -4 S / m]]> Existing Literature2 QCS-CD-AD / GO4 <![CDATA[2.04×10 -6 S / cm]]> Existing literature3 MNOH <![CDATA[4.2×10 -2 S / m]]> Existing literature5 PTCM-Gly5 <![CDATA[2×10 -1 S / cm]]> Existing literature6 0.5%POM <![CDATA[6×10 -2 S / m]]> This article

[0109] Table 3 is a comparison of the conductivity of hydrogels reported in this paper and recently

[0110] In the table:

[0111] Existing literature 1:

[0112] "Conductive adhesive self-healing nanocomposite hydrogel wound dressing for photothermal therapy of infected full-thickness skin wounds" Authors: Jiahui He, Mengting Shi;

[0113] Existing literature 2:

[0114] "Photothermal antibacterial antioxidant conductive self-healing hydrogel with nitric oxide release accelerates diabetic wound healing"; Authors: Jiahui He, Zhenlong Li;

[0115] Existing literature 3:

[0116] "Injectable self-healing supramolecular hydrogels with conductivity and photo-thermal antibacterial activity to enhance complete skin regeneration"; Authors: Beilin Zhang, Jiahui He;

[0117] Existing literature 4:

[0118] "Artificial nonenzymatic antioxidant MXene nanosheet-anchored injectable hydrogel as a mild photothermal-controlled oxygen release platform for diabetic wound healing"; Authors: Yang Li, Rongzhan Fu;

[0119] Existing literature 5:

[0120] "Conductive MXene nanocomposite organogel for flexible, healable, low-temperature tolerant strain sensors"; Authors: Hui Liao, Xuelin Guo;

[0121] Existing literature 6:

[0122] "Transparent and conductive amino acid-tackified hydrogels as wearable strain sensors"; Author: Yang Gao;

[0123] Existing literature 7:

[0124] "Artificial nonenzymatic antioxidant MXene nanosheet-anchored injectable hydrogel as a mild photothermal-controlled oxygen release platform for diabetic wound healing"; Author:

[0125] Yang Li, Rongzhan Fu, Zhiguang Duan;

[0126] Existing literature 8 "MXene-assisted ablation of cells with a pulsed near-infrared laser"; Author: Sergiy Kyrylenko, Oleksiy Gogotsi, Ivan Baginskiy;

[0127] Existing literature 9:

[0128] "In situ assembled titanium carbide-based heterojunctions for the synergistic enhancement of NIR-II photothermal / photodynamic therapy against breast cancer"; Author:

[0129] Hai Zhu, Xuequan Zhang, Qiusheng Wang;

[0130] Existing literature 10:

[0131] "Minimally invasive antitumor therapy using biodegradable nanocompositemic ellar hydrogel with funct ionalities of NIR-II photothermalablation and vascular disruption"; Author:

[0132] Na Tao, Yandi Liu, Yingjiao Wu.

[0133] Specifically, the present invention proposes the preparation and application of conductive antibacterial hydrogels. Among wound dressings, hydrogels have become the most promising wound dressing candidates; this is mainly due to their excellent hydrophilicity, biocompatibility and three-dimensional porous structure similar to the extracellular matrix (ECM). Compared with traditional dressings, hydrogels generally show better therapeutic effects on wounds prone to bacterial infection. They are a polymer network that has the ability to swell and retain a large amount of water but is insoluble in water; therefore, hydrogels are used as an interactive wound dressing for uninfected low-exudation wounds. Depending on the swelling ability of the gel, they can also be used to cover wounds with moderate or high exudation; hydrogels are commonly used to treat burns and wounds, and can also promote healing and remove scabs, and can be used to clean wounds; however, in some cases, hydrogel wound dressings require the application of other dressings to ensure adhesion to the wound bed (e.g., hydrocolloids); in addition, these dressings need to be replaced regularly every two to three days; therefore, hydrogel dressings can be non-adhesive (alginate, gelatin, carboxymethyl cellulose) or completely biodegradable.

[0134] Antibacterial hydrogels are generally loaded with antibiotics to prevent bacterial infection. However, overuse of antibiotics can lead to bacterial resistance. Photothermal therapy (PTT) provides a new antibacterial method. PTT is an innovative method to combat drug-resistant bacteria by converting light energy into heat through a photothermal agent (PTA). PTA is delivered to the bacterial surface, causing membrane rupture, protein denaturation, and irreversible damage. MXene has excellent light absorption properties throughout the visible and near-infrared ranges, showing excellent photothermal conversion potential. Based on the inherent photothermal properties of MXene, it shows great application potential in PTT.

[0135] The transition from the inflammatory phase to the proliferative phase is crucial for wound healing; the purpose of proliferation is to reduce the area of ​​damaged tissue through angiogenesis and fibrosis, thereby producing effective epithelialization, which can stimulate the activation of keratinocytes to close the wound. It has been reported that electrical stimulation (ES) can accelerate wound healing by reducing the inflammatory response and enhancing the proliferation and migration of fibroblasts.

[0136] In summary: In the diabetic infected wound treatment experiment, the wound of the final treatment group of the present invention was completely healed within 14 days, and the healing speed was faster than that of the control group, which proves that the POM hydrogel of the present invention has application as a diabetic infected wound care dressing.

[0137] The above is only a preferred embodiment of the present invention. It should be noted that, for those skilled in the art, several improvements and modifications can be made without departing from the principles of the present invention, and these improvements and modifications should also be considered as the protection scope of the present invention. The structures, devices and operating methods not specifically described and explained in the present invention shall be implemented according to the conventional means in the art unless otherwise specified and limited.

Claims

1. Preparation of Ti3C2Tx MXene-based conductive antibacterial hydrogel dressing, characterized by: The following steps are involved: Step 1: preparing oxidized sodium alginate; Step 2: Synthesis of MXene nanosheets; Step 3: Take 4 parts by mass of oxidized sodium alginate and 20 parts by mass of acrylamide and dissolve them in 30 parts by mass of ultrapure water under stirring. After they are completely dissolved, add 5 parts by mass of 0.1Mol / L NaOH solution dropwise and stir for 20 minutes; Solution A is obtained; Step 4: Add water to the MXene nanosheets obtained in step 2 to obtain a 0.5% MXene solution to obtain solution B; Step 5: Mix solution A and solution B in a volume ratio of 1:1, and then add 10 parts by mass of ammonium persulfate and 10 parts by mass of tetramethylethylenediamine; The gel precursor was transferred into a mold and reacted at room temperature for 30 seconds to achieve gelation to obtain a conductive antibacterial hydrogel.

2. The preparation of the Ti3C2Tx MXene-based conductive antibacterial hydrogel dressing according to claim 1, characterized in that: The specific steps of preparing oxidized sodium alginate in step 1 are as follows: Step 101: Disperse 10 g of sodium alginate in 50 mL of ethanol, and then add 50 mL of water containing 10 g of sodium periodate to the solution; Step 102: magnetically stirring the mixture in a dark environment at 25° C. for a certain period of time; Step 103: Add 5 mL of ethylene glycol and stir for a certain period of time to stop the reaction; Step 104: Pour 500 mL of ethanol into the reaction mixture; collect the precipitate by suction filtration; Step 105: The crude oxidized sodium alginate is dialyzed with deionized water for 3 days, and then freeze-dried to obtain a spongy oxidized sodium alginate solid.

3. The preparation of the Ti3C2Tx MXene-based conductive antibacterial hydrogel dressing according to claim 2, characterized in that: The duration of the magnetic stirring in step 102 is 5 hours; the duration of the stirring in step 103 is 2 hours.

4. The preparation of the Ti3C2Tx MXene-based conductive antibacterial hydrogel dressing according to claim 3, characterized in that: In step 2, the specific steps of synthesizing MXene nanosheets are as follows: Step 201: 1.6 g of LiF was added to 20 mL of 9 M hydrochloric acid solution, and the mixture solution was stirred for 30 min using a magnetic stirrer to form a uniform solution; Step 202: slowly add 1 g of Ti3AlC2 powder into the solution to avoid strong heat release; Step 203: Transfer the reaction bottle to an oil bath and continue stirring for a certain period of time; Step 204: Centrifuge the resulting dispersion for one cycle to obtain a multilayer Ti3C2T x MXene; Step 205: washing the obtained precipitate with a diluted HCl solution and centrifuging again; Step 206: washing the sediment with deionized water and repeating the centrifugation until the pH value of the supernatant reaches 5-6; Step 207: Wash the multilayer Ti3C2T x Disperse with 20 mL of deionized water, treat with ultrasonic exfoliation for a certain period of time, and finally freeze-dry to obtain MXene nanosheets.

5. The preparation of the Ti3C2Tx MXene-based conductive antibacterial hydrogel dressing according to claim 4, characterized in that: The oil bath temperature in step 203 is 35° C., and the continuous stirring time is 24 h.

6. The preparation of the Ti3C2Tx MXene-based conductive antibacterial hydrogel dressing according to claim 5, characterized in that: In step 207, the preparation is performed by ultrasonic stripping, and the ultrasonic treatment time is 6 hours.

7. The preparation of the Ti3C2Tx MXene-based conductive antibacterial hydrogel dressing according to claim 6, characterized in that: In step 207, freeze drying is performed using a freeze dryer, and the freeze drying time is usually 36 hours.

8. The Ti3C2T3 according to any one of claims 1 to 7 x Application of MXene-based conductive antibacterial hydrogels in the preparation of drugs and sensing materials for the treatment of diabetic wound dressings.

Citation Information

Cited By

  • Fecal fungi cryopreservation and unfreezing method and cryoprotectant

    CN115595270A

  • A method for the cryopreservation and thawing of fecal bacteria and a cryoprotective agent

    CN115595270B

  • Floatable hydrogel photo-thermal conversion material as well as preparation method and application thereof

    CN119708540A

  • Conductive electrospinning dressing with photo-thermal antibacterial function as well as preparation method and application of conductive electrospinning dressing

    CN119838042A