Breathable oil-proof filter element as well as preparation method and application thereof

By needle-punching the prototype base fabric of composite wool and viscose fiber and treating it in a three-proof finishing solution, the problem of oil mist adhering to the filter element material when it passes through, causing clogging and oil leakage, has been solved, and zero oil-related automobiles have been achieved. Breathable and oil-proof effect in parts.

CN118718558AActive Publication Date: 2024-10-01GUANGDONG HUIMING NONWOVEN TECH CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411177167.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-08-28
Filing Date
2024-08-26
Publication Date
2024-10-01
Estimated Expiration
2044-08-26

AI Technical Summary

Technical Problem

Existing filter element materials are prone to adhere to oil mist when oil mist passes through, causing clogging and oil leakage problems. Especially in automobile oil-related equipment, there are pressure changes and oil and gas phenomena, making it difficult to meet the dual requirements of breathability and oil prevention.

Method used

A single-layer filter base fabric is prepared from wool and viscose fiber through a needle punching machine, and is compounded into a prototype base fabric for the filter element. It is soaked in a three-proof finishing solution and then pressed and dried to form an excellent oil-proof, waterproof, and anti-fouling base fabric. , flame retardant and breathable filter element.

Benefits of technology

It achieves high efficiency in blocking oil impact and cooling oil mist, preventing clogging and oil leakage. It is suitable for automobile oil-related parts and has excellent ventilation efficiency and high temperature resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118718558A_ABST
    Figure CN118718558A_ABST
Patent Text Reader

Abstract

The invention discloses a breathable oil-proof filter element. A preparation method of the breathable oil-proof filter element comprises the following steps: needling wool and viscose through a needling machine to form single-layer filter base cloth; compounding more than two layers of single-layer filter base cloth to prepare filter element prototype base cloth; flattening the filter element prototype base cloth; preparing a three-proofing finishing solution, and soaking the flattened filter element prototype base cloth in the prepared three-proofing finishing solution; and pressing, drying and shaping. The invention further discloses application of the breathable oil-proof filter element. According to the invention, the problems of blockage and oil leakage caused by oil mist attached to oil-related parts of automobiles can be solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of filter elements, in particular to an air-permeable and oil-proof filter element. Background Art

[0002] Daily high-temperature operation of oil-related equipment such as automobile reducers and gearboxes will cause changes in the internal pressure of the assembly and the appearance of oil mist and oil gas. When the single valve of the automobile is opened, oil mist will also be brought out. When the oil mist passes through, ordinary core materials will adhere to the oil mist and form blockages, causing oil leakage. Therefore, it is necessary to develop a filter core material with good air permeability and high oil resistance. Summary of the invention

[0003] The purpose of the present invention is to overcome the defect of the common core material in the prior art that oil mist adheres to the core material when the oil mist passes through the core material, and to provide a filter core which is both air-permeable and oil-proof.

[0004] To achieve the above object, the present invention adopts the following technical solution: A method for preparing a breathable oil-proof filter element comprises the following steps: Preparation of single-layer filter base fabric: taking wool and viscose fibers and punching them into single-layer filter base fabric through a needle punching machine; Preparation of filter element prototype base fabric: Compounding two or more layers of single-layer filter base fabric to prepare filter element prototype base fabric; Flattening: Flatten the filter element prototype base fabric; Three-proof finishing: prepare the three-proof finishing solution, and then soak the flattened filter element prototype in the prepared three-proof finishing agent solution; The filter element prototype base fabric after soaking is pressed dry, dried and shaped.

[0005] Furthermore, in the step of preparing the single-layer filter base cloth, the weight ratio of the wool to the viscose fiber is 1:(2-3), and the needle punching speed of the needle punching machine is 600-900 times / min.

[0006] Furthermore, the thickness of the single-layer filter base fabric is 2.5-3.5 mm.

[0007] Furthermore, in the step of preparing the filter element prototype base fabric, a four-layer single-layer filter base fabric is used for needle punching and compounding through a low-speed needle punching machine, and the needle punching speed of the low-speed needle punching machine is 300-500 times / min.

[0008] Furthermore, the three-proof finishing solution is prepared by dissolving the three-proof finishing agent in water, and the mass ratio of the three-proof finishing agent to water is 1: (20-30).

[0009] Furthermore, the three-proof finishing solution is prepared by dissolving a three-proof finishing agent and polyvinyl alcohol in water, the three-proof finishing agent is Olifluan CPCO, and the mass ratio of the three-proof finishing agent to polyvinyl alcohol is (5-6):1.

[0010] Furthermore, the drying temperature is 140-150°C.

[0011] Furthermore, the wool specification is 6D*64mm, and the viscose fiber specification is 3D*51mm.

[0012] The present invention also provides an application of the above-mentioned air-permeable and oil-proof filter element, wherein the air-permeable and oil-proof filter element is used to prepare oil-related components of automobiles, including but not limited to automobile gearboxes, reducers, and one-way valves.

[0013] Compared with the prior art, the present invention has the following beneficial effects: The breathable and oil-proof filter element of the present invention adopts wool and viscose fibers as raw materials, both of which are flame-retardant fibers. They are compounded into a filter element prototype base cloth of required thickness through needle punching. After the needle punching process, it achieves better fluffiness, good ventilation effect and good flame retardant performance. It is soaked with a three-proof finishing agent, which not only makes the surface of the material waterproof, oil-proof and anti-fouling, but also has super high waterproof, oil-proof and anti-fouling effects from the inside to the outside. After being pressed dry, it is put into a drying box for drying so that the material can fully absorb the three-proof finishing agent. The final finalized product has excellent oil-proof, waterproof, anti-fouling, flame-retardant and breathable characteristics, is not easy to carbonize, is resistant to high temperature, and has high ventilation efficiency. It is used in oil-related parts of automobiles to block oil impact and cool oil mist, and solves the problem of oil mist adhesion to oil-related parts of automobiles to form blockages and oil leakage. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0015] Figure 1 It is a filter element prototype base layout diagram of a breathable and oil-proof filter element disclosed in an embodiment of the present invention; Figure 2 A diagram of a breathable and oil-proof filter element disclosed in an embodiment of the present invention; Figure 3 This is a schematic diagram of a breathable and oil-proof filter element disclosed in an embodiment of the present invention placed in a water and oil environment. DETAILED DESCRIPTION

[0016] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0017] It should be noted that the terms "first", "second", "third", "fourth", etc. in the specification and claims of the present invention are used to distinguish different objects rather than to describe a specific order. The terms "including" and "having" in the embodiments of the present invention and any variations thereof are intended to cover non-exclusive inclusions. For example, a process, method, system, product or device including a series of steps or units is not necessarily limited to those steps or units clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.

[0018] The embodiment of the present invention discloses a breathable and oil-proof filter core, which is made by the following method: first, wool and viscose fibers are needled into a single-layer filter base cloth through a needle-punching machine; then two or more layers of the single-layer filter base cloth are compounded to form a filter core prototype base cloth; then the filter core prototype base cloth is flattened; then, a three-proof finishing solution is prepared, and then the flattened filter core prototype base cloth is immersed in the prepared three-proof finishing agent solution; the immersed filter core prototype base cloth is pressed dry, dried, and shaped to obtain the breathable and oil-proof filter core.

[0019] The present embodiment will be described in more detail below in conjunction with the accompanying drawings.

[0020] A breathable oil-proof filter element is prepared by the following method: Preparation of single-layer filter base fabric: taking wool and viscose fibers and punching them into single-layer filter base fabric through a needle punching machine; Preparation of filter element prototype base fabric: Compounding two or more layers of single-layer filter base fabric to prepare filter element prototype base fabric; Flattening: Flatten the filter element prototype base fabric; Three-proof finishing: prepare the three-proof finishing solution, and then soak the flattened filter element prototype in the prepared three-proof finishing agent solution; The filter element prototype base fabric after soaking is pressed dry, dried and shaped.

[0021] In the step of preparing a single-layer filter base cloth, wool and viscose fibers are used as raw materials. Both wool and viscose fibers are flame-retardant fibers. After being needle-punched and mixed, they become semi-finished raw materials for breathable and oil-proof filter elements. In this embodiment, the wool specification is 6D*64mm, and the viscose specification is 3D*51mm. The weight ratio of the wool and the viscose fiber is 1:(2-3). In this embodiment, it is preferred that 30% wool and 70% viscose fibers are mixed and needle-punched. The thickness of the single-layer filter base cloth is 2.5-3.5mm, preferably 3mm, and the needle-punching speed of the needle-punching machine is 600-900 times / min.

[0022] In the step of preparing the filter element prototype base fabric, it is preferred to use a four-layer single-layer filter base fabric to be needle-punched and compounded by a low-speed needle-punching machine, and the needle-punching speed of the low-speed needle-punching machine is 300-500 times / min.

[0023] In this embodiment, a single-layer filter base cloth is prepared with a needling speed of 600-900 times / min, which can enable the wool and viscose fibers to be better integrated on the one hand, and reserve the fluffiness of the multi-layer composite on the other hand; when preparing the filter element prototype base cloth, a needling speed of 300-500 times / min is used, so that the multi-layer structure after composite can be in a better loose state, and the final product has good air permeability.

[0024] In the flattening step, a calender is used for flattening. The temperature of the calender is 120-130°C. The filter element prototype base fabric passes through the calender at a speed of 3 meters per minute. Figure 1 shown.

[0025] In the three-proof finishing step, a three-proof finishing agent with waterproof, oil-proof and anti-fouling functions is added to water for dissolution to prepare a three-proof finishing solution. Specifically, the three-proof finishing agent and water are prepared in a weight ratio of 1: (20-30), the three-proof finishing agent is added to the water, and stirred evenly with a mixer. Then, the three-proof finishing solution is poured into the dipping machine, and the flattened filter element prototype base cloth is soaked evenly through the dipping machine. In this embodiment, the three-proof finishing agent is Olifluan CPCO. In a preferred embodiment, the three-proof finishing solution is prepared by dissolving the three-proof finishing agent Olifluan CPCO and polyvinyl alcohol in water. After polyvinyl alcohol is added to the three-proof finishing solution, the waterproof, oil-proof and anti-fouling properties of the product are significantly improved. Specifically, the three-proof finishing agent is Olifluan CPCO, and the mass ratio of the three-proof finishing agent to polyvinyl alcohol is (5-6):1.

[0026] The soaked filter element prototype base fabric is squeezed dry by a pulping machine, and then enters a drying box to dry at 140-150℃. During drying, it is dried three times at a speed of 3 meters per minute through the upper and lower double mesh belts. After drying, it is shaped and rolled up by a cooling machine. After shaping, it is cut into the required size of breathable and oil-proof filter elements by die cutting and punching, as shown in the attached Figure 2 shown.

[0027] The air-permeable oil-proof filter element of this embodiment does not sink in oil or water. Figure 3 As shown, the air-permeable and oil-proof filter core of this embodiment is placed in a water bottle and an oil bottle, and the air-permeable and oil-proof filter core floats on the surface of the liquid.

[0028] The breathable and oil-proof filter element of this embodiment has the advantages of being oil-proof, waterproof, flame-retardant, and having high ventilation efficiency. It is not easy to carbonize during filtration and is resistant to high temperatures. According to the requirement of air permeability ≤50mm / s, the breathable and oil-proof filter element of this embodiment can be used up to 103 times after circulating ventilation.

[0029] In view of the advantages of being oil-proof, waterproof, flame-retardant, and having high ventilation efficiency, not being easily carbonized during filtration, and being resistant to high temperatures, the breathable and oil-proof filter element of this embodiment is suitable for use in oil-related devices of automobiles, such as automobile gearboxes, reducers, and one-way valves. When oil mist passes through, it can block the impact of oil, cool the oil mist, and prevent blockage and oil leakage. Example 1 A breathable and oil-proof filter element is prepared by the following method: (1) Preparing a single-layer filter base cloth: taking wool and viscose fibers and punching them into a single-layer filter base cloth through a needle-punching machine, the wool specification is 6D*64mm, the viscose fiber specification is 3D*51mm, the weight ratio of the wool to the viscose fiber is 1:2, the needle-punching speed of the needle-punching machine is 600 times / min, and the thickness of the single-layer filter base cloth formed by needle-punching is 2.5mm.

[0030] (2) Preparation of filter element prototype base fabric: four layers of single-layer filter base fabric are needle-punched and compounded by a low-speed needle-punching machine, wherein the needle-punching speed of the low-speed needle-punching machine is 500 times / min. (3) Flattening: The filter element prototype base fabric is flattened using a calender. The flattening temperature of the calender is 130°C, and the filter element prototype base fabric passes through the calender at a speed of 3 meters per minute.

[0031] (4) Three-proof finishing: Prepare a three-proof finishing solution with waterproof, oil-proof and anti-fouling functions, pour the three-proof finishing solution into a dipping machine, and soak the flattened filter element prototype base fabric evenly through the dipping machine. The three-proof finishing solution is prepared by dissolving Olefloxacin CPCO and polyvinyl alcohol in water, and by weight, Olefloxacin CPCO 1 part, 20 parts of water, and 0.5 parts of polyvinyl alcohol.

[0032] (5) The soaked filter element prototype base cloth is pressed dry, dried, and shaped: The soaked filter element prototype base cloth is pressed dry by a pulping machine, and then enters a drying box and is dried at 140°C. During drying, it is dried three times at a speed of 3 meters per minute through an upper and lower double mesh belt. After drying, it is shaped and rolled up by a cooling machine. After shaping, it is cut into a breathable and oil-proof filter element of the required size by die cutting and punching. Example 2 A breathable and oil-proof filter element is prepared by the following method: (1) Preparing a single-layer filter base cloth: taking wool and viscose fibers and punching them into a single-layer filter base cloth through a needle-punching machine, the wool specification is 6D*64mm, the viscose fiber specification is 3D*51mm, the weight ratio of the wool to the viscose fiber is 3:7, the needle-punching speed of the needle-punching machine is 900 times / min, and the thickness of the single-layer filter base cloth formed by needle-punching is 3mm.

[0033] (2) Preparation of filter element prototype base fabric: four layers of single-layer filter base fabric are needle-punched and compounded by a low-speed needle-punching machine, wherein the needle-punching speed of the low-speed needle-punching machine is 300 times / min. (3) Flattening: The filter element prototype base fabric is flattened using a calender. The flattening temperature of the calender is 120°C, and the filter element prototype base fabric passes through the calender at a speed of 3 meters per minute.

[0034] (4) Three-proof finishing: Prepare a three-proof finishing solution with waterproof, oil-proof and anti-fouling functions, pour the three-proof finishing solution into a dipping machine, and soak the flattened filter element prototype base fabric evenly through the dipping machine. The three-proof finishing solution is prepared by dissolving Olefloxacin CPCO and polyvinyl alcohol in water, and by weight, Olefloxacin CPCO 1 part, 25 parts of water, and 0.55 parts of polyvinyl alcohol.

[0035] (5) The soaked filter element prototype base cloth is pressed dry, dried, and shaped: The soaked filter element prototype base cloth is pressed dry by a pulping machine, and then enters a drying box and is dried at 150°C. During drying, it is dried three times at a speed of 3 meters per minute through an upper and lower double mesh belt. After drying, it is shaped and rolled up by a cooling machine. After shaping, it is cut into a breathable and oil-proof filter element of the required size by die cutting and punching. Example 3 A breathable and oil-proof filter element is prepared by the following method: (1) Preparing a single-layer filter base cloth: taking wool and viscose fibers and needle-punching them into a single-layer filter base cloth through a needle-punching machine, the wool specification is 6D*64mm, the viscose fiber specification is 3D*51mm, the weight ratio of the wool to the viscose fiber is 1:3, the needle-punching speed of the needle-punching machine is 700 times / min, and the thickness of the single-layer filter base cloth formed by needle-punching is 3mm.

[0036] (2) Preparation of filter element prototype base fabric: four layers of single-layer filter base fabric are needle-punched and compounded by a low-speed needle-punching machine, wherein the needle-punching speed of the low-speed needle-punching machine is 400 times / min. (3) Flattening: The filter element prototype base fabric is flattened using a calender. The flattening temperature of the calender is 125°C, and the filter element prototype base fabric passes through the calender at a speed of 3 meters per minute.

[0037] (4) Three-proof finishing: Prepare a three-proof finishing solution with waterproof, oil-proof and anti-fouling functions, pour the three-proof finishing solution into a dipping machine, and soak the flattened filter element prototype base fabric evenly through the dipping machine. The three-proof finishing solution is prepared by dissolving Olefloxacin CPCO and polyvinyl alcohol in water, and by weight, Olefloxacin CPCO 1 part, 30 parts of water, and 0.6 parts of polyvinyl alcohol.

[0038] (5) The soaked filter element prototype base fabric is pressed dry, dried, and shaped: The soaked filter element prototype base fabric is pressed dry by a pulping machine, and then enters a drying box and is dried at 145°C. During drying, it is dried three times at a speed of 3 meters per minute through an upper and lower double mesh belt. After drying, it is shaped and rolled up by a cooling machine. After shaping, it is cut into a breathable and oil-proof filter element of the required size by die cutting and punching. Example 4 A breathable and oil-proof filter element is prepared by the following method: (1) Preparing a single-layer filter base cloth: taking wool and viscose fibers and needle-punching them into a single-layer filter base cloth through a needle-punching machine, the wool specification is 6D*64mm, the viscose fiber specification is 3D*51mm, the weight ratio of the wool to the viscose fiber is 1:3, the needle-punching speed of the needle-punching machine is 700 times / min, and the thickness of the single-layer filter base cloth formed by needle-punching is 3mm.

[0039] (2) Preparation of filter element prototype base fabric: four layers of single-layer filter base fabric are needle-punched and compounded by a low-speed needle-punching machine, wherein the needle-punching speed of the low-speed needle-punching machine is 400 times / min. (3) Flattening: The filter element prototype base fabric is flattened using a calender. The flattening temperature of the calender is 125°C, and the filter element prototype base fabric passes through the calender at a speed of 3 meters per minute.

[0040] (4) Three-proof finishing: Prepare a three-proof finishing solution with waterproof, oil-proof and anti-fouling functions, pour the three-proof finishing solution into a dipping machine, and soak the flattened filter element prototype base fabric evenly through the dipping machine. The three-proof finishing solution is prepared by dissolving Olefloxacin CPCO in water, and the weight ratio is 1 part of Olefloxacin CPCO and 30 parts of water.

[0041] (5) The soaked filter element prototype base fabric is pressed dry, dried and shaped: The soaked filter element prototype base fabric is pressed dry by a pulping machine, and then enters a drying box and is dried at 145°C. During drying, it is dried three times at a speed of 3 meters per minute through the upper and lower double mesh belts. After drying, it is shaped and rolled up by a cooling machine. After shaping, it is cut into a breathable and oil-proof filter element of the required size by die cutting and punching.

[0042] Performance Test: (1) Waterproof performance test: The waterproof performance of the breathable oil-proof filter element is simulated according to the AATCC 22 low-speed spray test.

[0043] (2) Oil repellency test: The oil repellency performance of the breathable oil-proof filter element is tested in accordance with the AATCC 118 "Oil Repellency and Hydrocarbon Resistance Test" standard.

[0044] (3) Anti-fouling test: Test the resistance of the breathable oil-proof filter element to liquid stains in accordance with GB / T 30159.1.

[0045] (4) The test results are shown in Table 1. Table 1 Performance test results

[0046] Waterproof rating criteria: 100 points: There are no water droplets or wetting on the surface of the test sample; 90 points: There are slight irregular water droplets adhering to the surface of the test sample and a small amount of wetting; 80 points: The sprayed area on the test sample surface is slightly wet.

[0047] Oil resistance level: Level 5: The test liquid is n-dodecane Level 6: Test liquid is n-decane Level 7: The test liquid is n-octane Level 8: Test liquid is n-heptane Antifouling grade: Level 5: The droplet is clear, with a good arc shape with a large contact angle, and the contact area between the droplet and the sample is not wetted; Level 4: The contact surface between the droplet and the sample is partially or completely dark, and about 3 / 4 of the droplet volume remains on the sample surface; Level 3: The contact surface between the droplet and the sample is partially or completely dark, and about 1 / 2 of the droplet volume remains on the sample surface. From the above test results, it can be seen that adding polyvinyl alcohol to the three-proof finishing solution has a qualitative improvement in waterproof, oil-proof and anti-fouling properties.

[0048] The above is a detailed introduction to a breathable and oil-proof filter element and its preparation method and application disclosed in an embodiment of the present invention. Specific examples are used in this article to illustrate the principle and implementation mode of the present invention. The description of the above embodiments is only used to help understand the method of the present invention and its core idea; at the same time, for general technical personnel in this field, according to the idea of ​​the present invention, there will be changes in the specific implementation mode and application scope. In summary, the content of this specification should not be understood as a limitation on the present invention.

Claims

1. A method for preparing a breathable and oil-proof filter element, characterized in that: The following steps are involved: Preparation of single-layer filter base fabric: taking wool and viscose fibers and punching them into single-layer filter base fabric through a needle punching machine; Preparation of filter element prototype base fabric: Compounding two or more layers of single-layer filter base fabric to prepare filter element prototype base fabric; Flattening: Flatten the filter element prototype base fabric; Three-proof finishing: prepare the three-proof finishing solution, and then soak the flattened filter element prototype in the prepared three-proof finishing agent solution; The filter element prototype base fabric after soaking is pressed dry, dried and shaped.

2. The method for preparing the air-permeable and oil-proof filter element according to claim 1, characterized in that: In the step of preparing the single-layer filter base cloth, the weight ratio of the wool to the viscose fiber is 1:(2-3), and the needle punching speed of the needle punching machine is 600-900 times / min.

3. The method for preparing the air-permeable and oil-proof filter element according to claim 1, characterized in that: The thickness of the single-layer filter base fabric is 2.5-3.5 mm.

4. The method for preparing the air-permeable and oil-proof filter element according to claim 1, characterized in that: In the step of preparing the filter element prototype base fabric, a four-layer single-layer filter base fabric is used for needle punching and compounding through a low-speed needle punching machine, and the needle punching speed of the low-speed needle punching machine is 300-500 times / min.

5. The method for preparing the air-permeable and oil-proof filter element according to claim 1, characterized in that: The three-proof finishing solution is prepared by dissolving the three-proof finishing agent in water, and the mass ratio of the three-proof finishing agent to water is 1: (20-30).

6. The method for preparing the air-permeable and oil-proof filter element according to claim 5, characterized in that: The three-proof finishing solution is prepared by dissolving a three-proof finishing agent and polyvinyl alcohol in water, the three-proof finishing agent is Olifluan CPCO, and the mass ratio of the three-proof finishing agent to polyvinyl alcohol is (5-6):

1.

7. The method for preparing the air-permeable and oil-proof filter element according to claim 1, characterized in that: The drying temperature is 140-150°C.

8. The method for preparing the air-permeable and oil-proof filter element according to claim 1, characterized in that: The wool specification is 6D*64mm, and the viscose fiber specification is 3D*51mm.

9. A breathable and oil-proof filter element, characterized in that: The method is prepared according to any one of claims 1 to 8.

10. An application of the air-permeable and oil-proof filter element according to claim 9, characterized in that: The air-permeable and oil-proof filter element is used in preparing oil-related devices for automobiles.

Citation Information

Patent Citations

  • Anti-flaming washable filter material and preparation technique thereof

    CN101422670A

  • Non-glue cotton nonwoven filtering material and its preparation method

    CN102343185A

  • Production method for two-sided heterochromous self-cleaning jean fabric

    CN104047090A

  • Blending production technology of wool-containing machine washable protective flame-retardant fabric

    CN109023659A

  • Anti-contamination soil release finishing process for sofa fabric

    CN113430829A