Equipment and process method for preparing superfine calcium carbonate from fly ash washing liquid

By designing equipment and processes for preparing ultra-fine calcium carbonate from fly ash wash liquid in the cement kiln co-processing fly ash process, and using sodium carbonate precipitation method and ceramic membrane filtration, the problems of high fly ash wash liquid treatment cost and poor product purity are solved. problem, achieving high-value utilization of fly ash and efficient preparation of nanoscale calcium carbonate.

CN118718945APending Publication Date: 2024-10-01WUHU HAICHUANG ENVIRONMENTAL PROTECTION TECH CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410722826.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-05
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

In the existing cement kiln co-processing fly ash process, the fly ash washout treatment cost is high and the product purity and particle distribution are poor, which cannot effectively solve the problem of suspended solids and ion environmental impact.

Method used

An equipment and process for preparing ultrafine calcium carbonate from fly ash water washing liquid are designed, including a settling tank, a reaction tank, a plate and frame separator, a sodium carbonate tank, a washing tank, a centrifuge and a dryer. Through pretreatment, reaction In the process control and post-processing steps, ceramic membrane filtration and sodium carbonate precipitation are used to control the sodium carbonate addition rate and washing water ratio to achieve ultra-fine and high-purity preparation of calcium carbonate.

Benefits of technology

It achieves high-value utilization of fly ash, reduces the cost of fly ash disposal, and improves the purity and particle distribution of the product through the preparation of ultra-fine calcium carbonate, meeting the industrial application needs of nanoscale calcium carbonate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118718945A_ABST
    Figure CN118718945A_ABST
Patent Text Reader

Abstract

The invention discloses equipment and a process method for preparing superfine calcium carbonate from fly ash water washing liquid, and the equipment comprises a settling tank which can receive the fly ash water washing liquid; the reaction tank is communicated with the settling tank through a pipeline, and the fly ash washing liquid in the settling tank can enter the reaction tank; the first plate and frame separator is arranged on a pipeline between the settling tank and the reaction tank; the sodium carbonate tank can add sodium carbonate into the reaction tank; materials in the reaction tank sequentially pass through a second plate-and-frame separator, a washing tank, a centrifugal machine and a drying machine through pipelines, superfine calcium carbonate is extracted from the fly ash, and high-value utilization of the fly ash is achieved; the fly ash treatment cost is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of fly ash coordinated disposal technology in cement kilns, and in particular relates to equipment and a process method for preparing ultrafine calcium carbonate from fly ash water washing liquid. Background Art

[0002] In the process of implementing the present invention, the inventors found that the prior art has at least the following problems:

[0003] The fly ash co-treatment process of cement kiln involves fly ash water washing and dechlorination. The fly ash water washing liquid produced in this process needs to be treated to remove weight and hardness before evaporation to produce salt. In the process of removing hardness, the fly ash water washing liquid mainly uses sodium carbonate to produce calcium carbonate.

[0004] Disadvantages: The price of sodium carbonate is relatively high, resulting in high fly ash disposal costs; there are more suspended solids in the water wash liquid, and it is a potassium, sodium, and chloride ion-rich environment, which affects the purity and particle distribution of calcium carbonate.

[0005] CN113955889A-Resource recovery process of fly ash washing liquid, discloses a resource recovery process of fly ash washing liquid, the fly ash is washed with water, and then 1-3% of chelating agent is added to the high-concentration washing liquid obtained by filtration after washing to remove heavy metals to obtain a primary purified liquid, NaOH is added to the primary purified liquid, and CO2 is introduced to remove calcium carbonate and magnesium hydroxide mixed residue to obtain a secondary purified liquid, the secondary purified liquid is evaporated and crystallized by an MVR evaporator, potassium salt is recovered, and the remainder is mixed salt waste liquid, and sodium hydroxide and chlorine are obtained by electrolyzing the mixed salt waste liquid, which also cannot solve the above-mentioned technical problems. Summary of the invention

[0006] The technical problem to be solved by the present invention is a device and a process for preparing ultrafine calcium carbonate from fly ash water washing liquid

[0007] In order to solve the above technical problems, the technical solution adopted by the present invention is: a device for preparing ultrafine calcium carbonate from fly ash water washing liquid, comprising:

[0008] Settling tanks, capable of receiving fly ash wash liquid;

[0009] The reaction tank is connected to the settling tank through a pipeline, and the fly ash washing liquid in the settling tank can enter the reaction tank;

[0010] A first plate-frame separator, wherein the pipeline between the settling tank and the reaction tank is provided with a first plate-frame separator;

[0011] A sodium carbonate tank, capable of adding sodium carbonate into the reaction tank;

[0012] The materials in the reaction tank pass through the second plate-frame separator, the washing tank, the centrifuge and the dryer in sequence through the pipeline.

[0013] The reaction tanks include three groups of reaction tanks arranged in parallel.

[0014] A ceramic membrane is arranged on the pipeline between the first plate-frame separator and the reaction tank.

[0015] The process method of the equipment for preparing ultrafine calcium carbonate from the fly ash water washing liquid comprises the following steps: 1) pre-treatment of the fly ash water washing liquid; 2) controlling the reaction process of sodium carbonate and the fly ash water washing liquid; 3) post-treatment of the reaction product.

[0016] In the above step 1), the fly ash washing liquid produced in the fly ash washing and dechlorination process is used to intercept the suspended matter in the fly ash washing liquid after pre-sedimentation, plate and frame filtration, and ceramic membrane filtration. The suspended matter in the produced water is controlled at 30 mg / L and the pH is not less than 10.5. A good pretreatment effect can effectively ensure the purity of the obtained ultrafine calcium carbonate product.

[0017] In the above step 2), a sodium carbonate solution is prepared, wherein the carbonate ion concentration is about 70000-120000 mg / L, the chloride ion concentration is 7-11%, and the temperature is 20-55° C. The amount of sodium carbonate added is reduced to control the increase ratio of the water washing liquid volume after decalcification.

[0018] In the above step 2), the reaction tank volume is 150-1000m3, the stirring speed of the reaction tank is 40-80r / min, a circulating pump is set at the bottom of the reaction tank, and 3-5 reaction tanks are set. The wide stirring speed adjustment range can meet the treatment requirements under the conditions of different water washing liquid components; by adjusting the number of parallel reaction tanks, it can meet the needs of different fly ash water washing liquid treatment volumes.

[0019] In the above step 2), the fly ash water washing liquid enters the reaction tank, and the calcium ion concentration of the fly ash water washing liquid and the sodium carbonate solution is sampled and tested, and the dosage of the sodium carbonate solution is calculated; the agitator and the bottom circulation pump are started to homogenize the fly ash water washing liquid in the reaction tank, and the homogenization time is calculated according to every 100m 3 , homogenize for 2 minutes; turn off the bottom circulation pump, add sodium carbonate solution, the addition ratio is 40%, 15%, 15%, and the interval is 15 minutes; start the bottom circulation pump, add the remaining 30%, wait for 15 minutes, and discharge the material from the reaction tank after reaction. By adjusting the sodium carbonate addition rate, full reaction and control of calcium carbonate crystal form can be achieved.

[0020] The above step 3) includes the following steps: ① After the material is discharged from the reaction tank, it enters the plate frame for separation, and the separated solid phase is broken up and enters the washing tank, and the washing water ratio is controlled to be 1:1.2-3; ② After washing, it enters the centrifuge for separation; ③ The solid phase obtained after separation enters the dryer, uses air flow drying, and is ground and crushed to obtain ultrafine calcium carbonate. After sufficient water washing, the chloride ions in the ultrafine calcium carbonate product are removed to meet the product quality requirements.

[0021] In the above step 3), the particle size of calcium carbonate is ≤100 nm and the purity is greater than 99%.

[0022] According to the characteristics of fly ash water washing liquid, which is rich in suspended matter, potassium, sodium, chloride and sulfate ions, it is divided into several steps: pre-treatment, reaction process control and post-treatment, among which reaction process control is the key.

[0023] Main chemical reaction equation: Ca 2+ +CO3 2- =CaCO3.

[0024] One of the above technical solutions has the following advantages or beneficial effects: ultrafine calcium carbonate is extracted from fly ash to achieve high-value utilization of fly ash; and the cost of fly ash disposal is reduced. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 A schematic diagram of the structure of an apparatus for preparing ultrafine calcium carbonate from fly ash water wash provided in an embodiment of the present invention;

[0026] The marks in the above figures are: 1. sedimentation tank, 2. first plate and frame separator, 3. reaction tank, 4. sodium carbonate tank, 5. second plate and frame separator, 6. washing tank, 7. centrifuge, 8. dryer, 10. ceramic membrane. DETAILED DESCRIPTION

[0027] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0028] See also Figure 1 , a device for preparing ultrafine calcium carbonate from fly ash water washing liquid, comprising: a settling tank, which can receive the fly ash water washing liquid; a reaction tank, which is connected to the settling tank through a pipeline, and the fly ash water washing liquid in the settling tank can enter the reaction tank; a first plate-frame separator, and a first plate-frame separator is provided on the pipeline between the settling tank and the reaction tank; a sodium carbonate tank, which can add sodium carbonate into the reaction tank; the material in the reaction tank passes through the second plate-frame separator, the washing tank, the centrifuge and the dryer in sequence through the pipeline. Ultrafine calcium carbonate is extracted from fly ash, and high-value utilization of fly ash is realized; and the cost of fly ash disposal is reduced.

[0029] The reaction tank comprises three groups of reaction tanks arranged in parallel. A ceramic membrane is arranged on the pipeline between the first plate frame separator and the reaction tank.

[0030] The process method of the equipment for preparing ultrafine calcium carbonate from the fly ash water washing liquid comprises the following steps: 1) pre-treatment of the fly ash water washing liquid; 2) controlling the reaction process of sodium carbonate and the fly ash water washing liquid; 3) post-treatment of the reaction product.

[0031] (1) Analysis of fly ash washing liquid composition and influence of pretreatment process

[0032] The ash content, pH value, ionic strength and other factors of the fly ash water washing liquid will affect the solubility product of calcium carbonate in the preparation of nano calcium carbonate. The heavy metal ions such as Cu2+, Zn2+, Pb2+ and so on will also precipitate with calcium carbonate, thus affecting the product quality. Therefore, the full composition of the fly ash water washing liquid at different pretreatment stages is first analyzed to select the source of the raw material water washing liquid.

[0033] Composition analysis of fly ash washing liquid: The composition of fly ash washing liquid from different pretreatment positions provided by multiple batches of enterprises was analyzed. The ash content was tested by filtration; the concentration of metal cations such as calcium, potassium, sodium, iron, zinc, and lead was tested by ICP and atomic absorption method; the concentration of anions in the washing liquid was tested by titration combined with ion chromatography; the pH value and buffering properties of the washing liquid were tested by combining pH meter with dilute acid titration; and the effect of composition on the calcium carbonate precipitation process was tested by adding carbonate precipitation pre-experiments.

[0034] (2) Control of feed dispersion and optimization of experimental equipment

[0035] Accurately controlling the contact area between the two solutions, regulating the reaction rate, and instantly forming a highly supersaturated system are important means to produce uniform small-particle products. Through quantitative feed control, the effects of high-speed stirring and mixing and cross-flow microporous membrane dispersion on product performance are studied.

[0036] The regulation is mainly carried out by precisely controlling the amount of carbonate added and then stirring at high speed, or by using the water wash liquid as the continuous phase and adding carbonate through microporous filter pressure dispersion.

[0037] (3) Screening of additives and optimization of operating conditions

[0038] Based on the experimental device selected above, different types of organic and inorganic additives were screened to investigate their effects on the morphology of nano-calcium carbonate, so as to achieve customized product properties. The operating temperature, carbonate solution concentration, pH value of fly ash water wash and other conditions were optimized to obtain nano-calcium carbonate products with small particle size and uniform particle size distribution. The preparation technology of nano-calcium carbonate based on fly ash water wash was obtained.

[0039] Determination of optimal operating parameters: Orthogonal experimental methods were used to study the effects of various experimental factors (precipitant type, precipitant quality, stirring rate, stirring time, stirring method, reaction temperature, additive type, additive quality, intake carbon dioxide concentration, intake flow rate, intake pressure, etc.) on the particle size and yield of calcium carbonate, and to determine the key influencing factors of the process. The whiteness of the prepared nano-calcium carbonate was determined by a whiteness meter, its crystal morphology was determined by XRD, its charge was tested by Zeta potential, its surface activity was tested by BET method, its particle size was observed by TEM and SEM, and the product particle size distribution was analyzed by a laser particle size analyzer. The experimental technical parameters were optimized to obtain the optimal conditions for the preparation of nano-calcium carbonate.

[0040] In the above step 1), the fly ash washing liquid produced in the fly ash washing and dechlorination process is subjected to pre-sedimentation, plate and frame filtration, and ceramic membrane filtration to intercept suspended matter in the fly ash washing liquid. The suspended matter in the produced water is controlled at 30 mg / L and the pH is not lower than 10.5.

[0041] In the above step 2), a sodium carbonate solution is prepared, wherein the carbonate ion concentration is about 70000-120000 mg / L, the chloride ion concentration is 7-11%, and the temperature is 20-55°C.

[0042] In step 2) above, the reaction tank volume is 150-1000m 3 , the stirring speed of the reaction tank is 40-80r / min, a circulating pump is set at the bottom of the reaction tank, and 3-5 reaction tanks are set. (

[0043] In the above step 2), the fly ash water washing liquid enters the reaction tank, and the calcium ion concentration of the fly ash water washing liquid and the sodium carbonate solution is sampled and tested, and the dosage of the sodium carbonate solution is calculated; the agitator and the bottom circulation pump are started to homogenize the fly ash water washing liquid in the reaction tank, and the homogenization time is calculated according to every 100m 3 , homogenize for 2 minutes; turn off the bottom circulation pump, add sodium carbonate solution, the addition ratio is 40%, 15%, 15%, and the interval is 15 minutes; start the bottom circulation pump, add the remaining 30%, and wait for 15 minutes. After the material reacts, it is discharged from the reaction tank.

[0044] The above step 3) includes the following steps: ① After the material is discharged from the reaction tank, it enters the plate frame for separation, and the separated solid phase is broken up and enters the washing tank, and the washing water ratio is controlled to be 1:1.2-3; ② After washing, it enters the centrifuge for separation; ③ The solid phase obtained after separation enters the dryer, uses air flow drying, and is ground and crushed to obtain ultrafine calcium carbonate.

[0045] In the above step 3), the particle size of calcium carbonate is ≤100 nm and the purity is greater than 99%.

[0046] Nano calcium carbonate refers to calcium carbonate microparticles with a particle size of less than 100nm. The ultrafine particles lead to changes in the crystal structure and surface electronic structure, resulting in surface effects, small size effects, and macroscopic quantum tunneling effects that ordinary particles do not have. Nano-scale ultrafine calcium carbonate particles have a wide range of industrial application value due to their high porosity, high surface area to volume ratio, and good compatibility. They exhibit excellent physical and chemical properties in mechanics, optics, electricity, etc., and are widely used in rubber, plastics, papermaking, building materials and other industries, with huge commercial value potential.

[0047] The preparation methods of nano calcium carbonate are mainly divided into physical method and chemical method. Heavy nano calcium carbonate is prepared by mechanical crushing method; light or precipitated nano calcium carbonate is prepared by chemical method. The chemical method is mainly divided into precipitation method, carbonization method, emulsion method, sol-gel method, etc., and the crystal form of the product is controllable. Among them, the precipitation method uses water-soluble carbonate and water-soluble calcium salt as raw materials, and the process of preparing nano calcium carbonate under certain conditions through double decomposition reaction has the advantage of high product purity. However, if the precipitation conditions are not precisely controlled, the calcium carbonate prepared by direct mixing usually has a wide particle size distribution and poor dispersibility, and it is very easy to agglomerate and lose the special function of nanoparticles. The solution to this problem can mainly use a dispersion medium to increase the contact area of ​​the interface between the two solutions, finely control the reaction rate, instantly form a highly supersaturated system, and obtain a uniform small particle size product. A small amount of organic additives is also an effective means to regulate the morphology and particle size of calcium carbonate.

[0048] In summary, nano calcium carbonate is prepared by carbonate precipitation method using high concentration of calcium ions in fly ash washing liquid, and used as a high value-added product in rubber, plastic, building materials and other fields, which is of great value to improving the economic benefits of fly ash treatment process and the environmental protection of washing water circulation system. The preparation of nano calcium carbonate by precipitation method can achieve decalcification of washing liquid and production of high-value products at the same time, and the technical route is feasible. By designing the experimental process, accurately controlling the concentration of added liquid and the dispersion method, and screening suitable additives, the technical solution for preparing small particle size and high performance nano calcium carbonate products is feasible.

[0049] According to the characteristics of fly ash water washing liquid, which is rich in suspended matter, potassium, sodium, chloride and sulfate ions, it is divided into several steps: pre-treatment, reaction process control and post-treatment, among which reaction process control is the key.

[0050] Main chemical reaction equation: Ca 2+ +CO3 2- =CaCO3.

[0051] Economic analysis:

[0052] The economic benefits of preparing nano calcium carbonate from fly ash water washing liquid were analyzed, and the nano calcium carbonate was calculated at a yield of 70%, and the results are shown in Table 1. The annual processing capacity of fly ash water washing liquid is 70,000 tons, and the sodium carbonate precipitation method is used to produce nano calcium carbonate. The sodium carbonate consumption is 120kg / t fly ash. Compared with the original calcium carbonate method for decalcification, this method does not consume any additional sodium carbonate. The annual operating cost of the project of preparing nano calcium carbonate from fly ash water washing liquid is 2.265 million yuan, the annual sales volume is 5.5 million yuan, and the annual economic benefits are 2.41 million yuan.

[0053] Table 1 Cost analysis of preparing nano calcium carbonate from fly ash washing liquid

[0054]

[0055]

[0056] Process steps:

[0057] Step 1: Pretreatment: The fly ash washing liquid produced by the existing fly ash washing and dechlorination process is used to intercept the suspended matter in the fly ash washing liquid after pre-sedimentation, plate and frame filtration, and ceramic membrane filtration. The suspended matter in the produced water is controlled at 30 mg / L, and the pH is not less than 10.5. The main components of the suspended matter are fine particles of fly ash, magnesium compounds, macromolecular colloids, etc.

[0058] Step 2: Reaction process control: ① Prepare sodium carbonate solution, carbonate ion concentration is about 70000-120000mg / L, chloride ion concentration is 7-11%, temperature is 20-55℃. ② 150t / d fly ash disposal line, reaction tank volume 150-1000m 3 , the reaction tank is set to stir rapidly at 40-80r / min, the reaction tank is set to have a bottom circulation pump, and 3-5 reaction tanks are set. ③ The fly ash water washing liquid enters the reaction tank, and the calcium ion concentration of the fly ash water washing liquid and the sodium carbonate solution is sampled and tested, and the dosage is calculated. ④ Start the agitator and the bottom circulation pump to homogenize the fly ash water washing liquid in the reaction tank. The homogenization time is calculated as per 100m 3 ⑤ Turn off the bottom circulation pump and add sodium carbonate solution at a ratio of 40%, 15%, and 15%, with an interval of 15 minutes. ⑥ Start the bottom circulation pump and add the remaining 30%, wait for about 15 minutes, and then discharge the reaction tank.

[0059] Step 3: Post-treatment: ① After being discharged from the reaction tank, it enters the plate frame for separation. The separated solid phase is broken up and enters the washing tank. The washing water ratio is controlled to be 1:1.2-3. ② After washing, it enters the centrifuge for separation. ③ The solid phase obtained after separation enters this dryer, uses airflow drying, and is ground and crushed to obtain ultrafine calcium carbonate. ④ Calcium carbonate particle size: ≤100nm, purity greater than 99%.

[0060] The calcium ion content in the fly ash washing liquid reaches 10-15g / L. Decalcification by adding sodium carbonate precipitation is an important part of the resource treatment of the washing liquid. A large amount of solid calcium carbonate is produced in the process and discharged in the form of waste residue. How to achieve high-value utilization of solid calcium carbonate is an important issue to improve the economic benefits of the fly ash treatment process and the environmental protection of the system. Nano-scale calcium carbonate has excellent physical and chemical properties in mechanics, optics, and electricity due to its small particle size and nano effect. It is widely used in rubber, plastics, papermaking, building materials and other industries, and has great commercial value potential. This project intends to use the calcium ions in the fly ash washing liquid to prepare nano-calcium carbonate. By regulating the mixing process of the washing liquid and carbonate, the crystallization characteristics of calcium carbonate are improved, and the preparation technology of nano-calcium carbonate is obtained.

[0061] Firstly, by analyzing the composition of the water wash liquid, the components that may affect the purity of nano-calcium carbonate are identified, and the influence of the composition of the water wash liquid and the pretreatment effect on the crystallization characteristics of calcium carbonate is obtained; the experimental device is designed to quantitatively control the addition rate and contact time of the two aqueous phase solutions, and the supersaturation is changed through high-speed stirring and mixing, cross-flow microporous feeding and other methods, and the calcium carbonate yield, crystal phase, morphology and particle size distribution and other characteristics are regulated; on the basis of the optimal mixing characteristics, through conditional experiments, additives are screened, and operating conditions such as carbonate type and concentration are optimized to obtain calcium carbonate with small particle size and uniform dispersion, thus forming a preparation technology for nano-calcium carbonate from fly ash water wash liquid.

[0062] After adopting the above scheme, ultrafine calcium carbonate is extracted from fly ash, achieving high-value utilization of fly ash and reducing the cost of fly ash disposal.

[0063] In the description of the present invention, it is necessary to understand that the terms "coaxial", "bottom", "one end", "top", "middle", "the other end", "upper", "one side", "top", "inside", "front", "center", "both ends" and the like indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present invention.

[0064] In the present invention, unless otherwise clearly stipulated and limited, the terms such as "installation", "setting", "connection", "fixation" and "screw-on" should be understood in a broad sense. For example, it can be a fixed connection, a detachable connection, or an integral one; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium; it can be the internal connection of two elements or the interaction relationship between two elements. Unless otherwise clearly defined, ordinary technicians in this field can understand the specific meanings of the above terms in the present invention according to the specific circumstances.

[0065] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A device for preparing ultrafine calcium carbonate from fly ash water washing liquid, characterized in that: have: Settling tanks, capable of receiving fly ash wash liquid; The reaction tank is connected to the settling tank through a pipeline, and the fly ash washing liquid in the settling tank can enter the reaction tank; A first plate-frame separator, wherein the pipeline between the settling tank and the reaction tank is provided with a first plate-frame separator; A sodium carbonate tank, capable of adding sodium carbonate into the reaction tank; The materials in the reaction tank pass through the second plate-frame separator, the washing tank, the centrifuge and the dryer in sequence through the pipeline.

2. The device for preparing ultrafine calcium carbonate from fly ash water washing liquid as claimed in claim 1, characterized in that: The reaction tanks include three groups of reaction tanks arranged in parallel.

3. The equipment for preparing ultrafine calcium carbonate from fly ash water washing liquid as claimed in claim 2, characterized in that: A ceramic membrane is arranged on the pipeline between the first plate-frame separator and the reaction tank.

4. The process for preparing ultrafine calcium carbonate from fly ash water washing liquid according to any one of claims 1 to 3, characterized in that: The method comprises the following steps: 1) pre-treatment of fly ash water washing liquid; 2) controlling the reaction process of sodium carbonate and fly ash water washing liquid; and 3) post-treatment of reaction products.

5. The process for preparing ultrafine calcium carbonate from fly ash water washing liquid according to claim 4, characterized in that: In the above step 1), the fly ash washing liquid produced in the fly ash washing and dechlorination process is subjected to pre-sedimentation, plate and frame filtration, and ceramic membrane filtration to intercept suspended solids in the fly ash washing liquid. The suspended solids in the produced water are controlled below 30 mg / L and the pH is not lower than 10.

5.

6. The process for preparing ultrafine calcium carbonate from fly ash water washing liquid according to claim 5, characterized in that: In the above step 2), a sodium carbonate solution is prepared, wherein the carbonate ion concentration is about 70000-120000 mg / L, the chloride ion concentration is 7-11%, and the temperature is 20-55°C.

7. The process for preparing ultrafine calcium carbonate from fly ash water washing liquid according to claim 6, characterized in that: In step 2) above, the reaction tank volume is 150-1000m 3 The stirring speed of the reaction tank is 40-80r / min, a circulating pump is set at the bottom of the reaction tank, and 3-5 reaction tanks are set.

8. The process for preparing ultrafine calcium carbonate from fly ash water washing liquid according to claim 7, characterized in that: In the above step 2), the fly ash water washing liquid enters the reaction tank, and the calcium ion concentration of the fly ash water washing liquid and the sodium carbonate solution is sampled and tested, and the dosage of the sodium carbonate solution is calculated; the agitator and the bottom circulation pump are started to homogenize the fly ash water washing liquid in the reaction tank, and the homogenization time is calculated according to every 100m 3 , homogenize for 2 minutes; turn off the bottom circulation pump and add sodium carbonate solution at a ratio of 40%, 15%, and 15%, with an interval of 15 minutes; Start the bottom circulation pump, add the remaining 30%, wait for 15 minutes, and discharge the material from the reaction tank after reaction.

9. The process for preparing ultrafine calcium carbonate from fly ash water washing liquid according to claim 8, characterized in that: The above step 3) includes the following steps: ① After the material is discharged from the reaction tank, it enters the plate frame for separation, and the separated solid phase is broken up and enters the washing tank, and the washing water ratio is controlled to be 1:1.2-3; ② After washing, it enters the centrifuge for separation; ③ The solid phase obtained after separation enters the dryer, uses air flow drying, and is ground and crushed to obtain ultrafine calcium carbonate.

10. The process for preparing ultrafine calcium carbonate from fly ash water washing liquid according to claim 9, characterized in that: In the above step 3), the particle size of calcium carbonate is ≤100 nm and the purity is greater than 99%.

Citation Information

Cited By

  • Continuous production equipment and process for preparing superfine calcium carbonate from fly ash washing liquid

    CN119701845A

  • Continuous production equipment and process for preparing ultrafine calcium carbonate from fly ash washing liquid

    CN119701845B