Adsorbent for adsorbing and separating olefin and alkane and preparation method thereof

By controlling the exchangeable cation ratio and moisture content of the X-type molecular sieve in the adsorbent, the problem of separation of high carbon number olefins and alkanes is solved, the separation efficiency and product purity are improved, the life of the adsorbent is extended, and energy consumption is reduced.

CN118718981APending Publication Date: 2024-10-01CHINA PETROLEUM & CHEMICAL CORP +1

Patent Information

Application Number
CN202310318163.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-03-28
Publication Date
2024-10-01

Smart Images

  • Figure CN118718981A_ABST
    Figure CN118718981A_ABST
Patent Text Reader

Abstract

The invention relates to an adsorbent for adsorbing and separating olefin and alkane and a preparation method, the adsorbent comprises an active component and a binder, the active component is an X-type molecular sieve, 40-60% of exchangeable cations of the X-type molecular sieve are one or more of K < + >, Cs < + > and Rb < + >, and the remaining exchangeable cations are Na < + >; the water content of the adsorbent is less than or equal to 1.5 mass percent. According to the adsorbent for adsorbing and separating olefin and alkane, the olefin can be effectively adsorbed in the microchannels of the molecular sieve with high selectivity, high-carbon olefin and alkane can be adsorbed and separated at a high separation degree, and isomerization reaction and polymerization reaction of olefin can be effectively inhibited while adsorption separation is performed; further, the purity and the yield of the high-carbon olefin are improved, and the service life of the adsorbent is prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of adsorption separation, and in particular to an adsorbent for adsorption separation of olefins and alkanes and a preparation method thereof. Background Art

[0002] α-olefins are used in different fields due to their different carbon numbers. Among them, α-olefins with 4 to 8 carbon numbers can be used as polyethylene comonomers, α-olefins with 6 to 10 carbon numbers are important intermediates for the production of plasticizers, α-olefins with 8 to 12 carbon numbers are mainly used to produce lubricant base oils (PAO), and α-olefins with 12 to 18 carbon numbers are mainly used to produce fine chemicals such as detergent raw materials. At present, with the development of petrochemical and fine chemical industries, the market demand for α-olefins is increasing.

[0003] The sources of α-olefins mainly include ethylene polymerization resources, Fischer-Tropsch synthetic oil resources, alkane dehydrogenation resources containing normal olefins and alkanes, coking kerosene, etc. Among these olefin resources, except for the olefins from ethylene polymerization with higher purity, the other resources mainly contain olefins and alkanes with the same or adjacent carbon numbers. Therefore, in order to obtain high-purity olefins from these resources, they must be separated. + The difference in boiling points between olefins and alkanes with the same carbon number is very small, and the difference in boiling points between olefin isomers is also very small, so distillation separation is very difficult and energy consumption is very high. Extractive distillation uses the different effects of extractants on the relative volatility of olefins and alkanes to achieve alkane-olefin separation, but as the carbon number increases, the difference in physical properties between olefins and alkanes becomes smaller and smaller, and the selection of extractants becomes more and more difficult. Adsorption separation technology uses the selective adsorption of adsorbents to separate substances with similar boiling points. The characteristics of this technology are high separation efficiency, low energy consumption, environmentally friendly process, and strong adaptability to raw material fractions. However, for the separation of high-carbon number olefins and alkanes, the development of adsorbents with high adsorption capacity and high selectivity is still a key technical barrier that needs to be overcome.

[0004] CN111001382A discloses a method for preparing a Fischer-Tropsch oil alkane-olefin separation adsorbent, which includes a pre-adsorbent and a main adsorbent. The oxygen-containing compounds in the raw material are first removed, and then a 13X molecular sieve or a mixed crystal molecular sieve of 13X and LTA is used as an adsorbent to separate olefins by simulated moving bed technology. USP3510423 uses a mixture of C10-C15 alkanes and olefins as a raw material, and separates olefins by a simulated moving bed adsorption separation process of 8 beds. The adsorbent uses an Ag-exchanged X or Y-type molecular sieve. The purity of the olefin product can reach 98% by mass, but there are problems such as relatively narrow raw material adaptability and low yield of high carbon number olefins; US20080051619 discloses a method for adsorbing and separating olefins from C9-C20 components, using NaX as an adsorbent and cycloalkane as a desorbent, and adopting simulated moving bed technology, but olefins are more likely to react on the molecular sieve adsorbent, resulting in reduced product purity; US3720604 believes that CuY has strong selectivity for olefins, but its reaction activity for olefins is also high, so it is proposed to first use alkaline Cu 2+ Solution exchange NaY molecular sieve, and then with olefins and Cu 2+ The solution was treated at 172°C to obtain Cu-exchanged Y molecular sieve with high selectivity and low reactivity.

[0005] How to develop and design an adsorbent with high adsorption capacity to improve olefin selectivity and effectively inhibit olefin isomerization and polymerization reactions is a technical problem that needs to be solved urgently. Summary of the invention

[0006] The present invention provides an adsorbent for adsorbing and separating olefins and alkanes and a preparation method thereof, so as to improve the olefin selectivity of the adsorbent and effectively inhibit the isomerization reaction and polymerization reaction of the olefins.

[0007] In the first aspect, the present invention relates to an adsorbent for adsorption separation of olefins and alkanes, comprising an active component and a binder, wherein the active component is an X-type molecular sieve, and 40-60% of the exchangeable cations of the X-type molecular sieve are K + , Cs + and Rb + One or more of the following, the remaining exchangeable cations being Na + ; The moisture content of the adsorbent is ≤1.5% by mass.

[0008] Optionally, the molar ratio of silicon oxide to aluminum oxide in the X-type molecular sieve is 2.0 to 3.0, preferably 2.2 to 2.5.

[0009] Optionally, the average particle size of the X-type molecular sieve is 0.5 μm to 3.5 μm, preferably 0.8 μm to 1.2 μm.

[0010] Optionally, the particle size of the adsorbent is 0.3 mm to 1.0 mm.

[0011] Optionally, based on the mass of the adsorbent, the mass proportion of the active component is 95.0% to 99.5%, and the mass proportion of the binder is 0.5% to 5.0%.

[0012] Optionally, 45-55% of the exchangeable cations of the X-type molecular sieve are K + , Cs + and Rb + One or more of the following, the remaining exchangeable cations being Na + .

[0013] Optionally, the adsorbent is used to separate α-olefins and alkanes having a carbon number of 6-16; preferably, the adsorbent is used to separate α-olefins and alkanes having a carbon number of 12-16.

[0014] In a second aspect, the present invention relates to a method for preparing the above-mentioned adsorbent, comprising the following steps:

[0015] (1) mixing NaX molecular sieve with clay, rolling into balls, screening, drying and calcining to obtain molecular sieve balls; (2) in-situ crystallizing the molecular sieve balls obtained in step (1) with an alkaline solution, then washing with water and drying to obtain NaX molecular sieve matrix balls; (3) using a K-containing + , Rb + and Cs + The NaX molecular sieve matrix beads obtained in step (2) are subjected to cation exchange with an alkali metal salt solution of one or more alkali metal ions, followed by washing with water and drying to obtain alkali metal ion-exchanged NaX molecular sieve beads; (4) the NaX molecular sieve beads obtained in step (3) are calcined and activated to a calcination amount of ≤1.5% by mass, based on the mass of the NaX molecular sieve beads.

[0016] Optionally, the clay in step (1) is kaolinite, dickite, perlite, refractory stone or halloysite.

[0017] Optionally, in step (1), the mass ratio of the NaX molecular sieve to the clay is (90-95):(5-10), small balls with a particle size of 0.3 mm to 1.0 mm are sieved out by the sieving, the drying temperature is 80° C. to 100° C., and the calcining temperature is 500° C. to 700° C.

[0018] Optionally, in step (2): the alkaline solution is a mixed solution of sodium hydroxide and water glass, the concentration of sodium hydroxide in the mixed solution is 0.5 mol / L to 2.5 mol / L, and the mass concentration of water glass in terms of silicon dioxide is 5 g / L to 15 g / L; the temperature of the in-situ crystallization is 85°C to 95°C, and the time is 4h to 6h; the water washing is carried out until the pH of the washed water is less than 9, and the drying temperature is 80°C to 100°C.

[0019] Optionally, in step (3), the alkali metal salt solution comprises one or more of chloride, nitrate and carbonate of the alkali metal ion; in the alkali metal salt solution, K + The ion concentration is 0.1mol / L~0.3mol / L, and / or Rb + The ion concentration is 0.05mol / L~0.3mol / L, and / or Cs + The ion concentration is 0.15mol / L~0.4mol / L; the cation exchange time is 4-10h, and the cation exchange temperature is 85℃~105℃; the water washing is carried out until no salt solution remains, and the drying temperature is 80℃~100℃.

[0020] Optionally, in step (4): the calcination activation temperature is 400°C to 600°C; the calcination activation is performed to a base amount of ≤1% by mass, based on the mass of the NaX type molecular sieve pellets.

[0021] Beneficial effects:

[0022] The adsorbent for adsorptive separation of olefins and alkanes of the present invention can effectively adsorb olefins in the micropores of the molecular sieve with high selectivity, can adsorb and separate high-carbon olefins and alkanes with a high degree of separation, and can effectively inhibit the isomerization reaction and polymerization reaction of olefins while performing the adsorptive separation, thereby facilitating the improvement of the purity and yield of high-carbon olefins and facilitating the extension of the life of the adsorbent. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 The pulse envelope curve diagram obtained when testing the adsorption performance of the adsorbent prepared in Example 1 is shown in Figure 1;

[0024] Figure 2 This is a structural diagram of the pulse test device used in Test Example 1;

[0025] Figure 3 This is a structural diagram of the continuous pulse cycle test device used in Test Example 2.

[0026] Description of Reference Numerals

[0027] 1 pulse liquid; 2 desorption liquid; 3 first exhaust port; 4 first rotor flowmeter; 5 first blind end; 6 first preheating furnace; 7 first outer insulation jacket; 8 inner heating furnace; 9 first adsorption column; 10 first back pressure valve; 11 first sampling port; 12 waste liquid tank;

[0028] 21 circulating liquid; 22 second sampling port; 23 second exhaust port; 24 second rotor flowmeter; 25 second blind end; 26 second back pressure valve; 27 second adsorption column; 28 heating furnace; 29 second outer insulation jacket; 30 second preheating furnace; 31 water absorption desiccant tank; 32 circulating liquid tank. DETAILED DESCRIPTION

[0029] The present application is further described in detail below through the accompanying drawings and embodiments. Through these descriptions, the characteristics and advantages of the present application will become clearer and more specific.

[0030] The word "exemplary" is used exclusively herein to mean "serving as an example, embodiment, or illustration." Any embodiment described herein as "exemplary" is not necessarily to be construed as preferred or advantageous over other embodiments. Although various aspects of the embodiments are shown in the drawings, the drawings are not necessarily drawn to scale unless otherwise noted.

[0031] In addition, the technical features involved in different embodiments of the present application described below can be combined with each other as long as they do not conflict with each other.

[0032] The present invention provides an adsorbent for adsorption separation of olefins and alkanes, comprising an active component and a binder, wherein the active component is an X-type molecular sieve, and 40-60% of the exchangeable cations of the X-type molecular sieve are K + , Cs + and Rb + One or more of the following, the remaining exchangeable cations being Na + ; The moisture content of the adsorbent is ≤1.5% by mass.

[0033] It should be noted that when a large amount of water remains in the adsorbent, it will not only occupy the effective pore volume of the adsorbent, but also reduce the adsorption selectivity of the adsorbent. The adsorbent of the present invention controls the water content of the adsorbent to ≤1.5% by mass so that the adsorption selectivity of the adsorbent is high and the adsorption capacity is large. On the other hand, the K + , Cs + and Rb + One or more cations in the X-type molecular sieve occupy 40-60% of the exchangeable cation sites in the X-type molecular sieve, thereby enabling the adsorbent of the present invention to effectively inhibit the isomerization reaction and polymerization reaction of olefins, significantly improve the olefin yield, and extend the life of the adsorbent.

[0034] According to one embodiment, the molar ratio of silicon oxide to aluminum oxide in the X-type molecular sieve is 2.0 to 3.0, preferably 2.2 to 2.5.

[0035] It should be noted that the molar ratio of silicon oxide to aluminum oxide in the X-type molecular sieve is the ratio of silicon oxide to aluminum oxide in the molecular sieve framework.

[0036] According to one embodiment, the average particle size of the X-type molecular sieve is 0.5 μm to 3.5 μm, preferably 0.8 μm to 1.2 μm.

[0037] According to one implementation, the particle size of the adsorbent is 0.3 mm to 1.0 mm.

[0038] As a preferred embodiment, based on the mass of the adsorbent, the mass proportion of the active component is 95.0% to 99.5%, and the mass proportion of the binder is 0.5% to 5.0%.

[0039] It should be noted that, as a preferred embodiment, based on the mass of the adsorbent, the mass proportion of the active component is 98.0% to 99.5%, and the mass proportion of the binder is 0.5% to 2.0%. The higher the mass proportion of the active component, i.e., the X-type molecular sieve, the better the adsorption capacity of the adsorbent, and the better adsorption and separation effect can be achieved.

[0040] As a preferred embodiment, 45-55% of the exchangeable cations of the X-type molecular sieve are K + , Cs + and Rb + One or more of the following, the remaining exchangeable cations being Na + .

[0041] According to one embodiment, the adsorbent is used to separate α-olefins and alkanes having a carbon number of 6-16;

[0042] Preferably, the adsorbent is used to separate α-olefins and alkanes having a carbon number of 12-16.

[0043] It should be noted that the adsorbent of the present invention can be applied to the separation of α-olefins from resources such as Fischer-Tropsch synthetic oil and normal alkane dehydrogenation products containing high-carbon olefins. The adsorbent has a high adsorption capacity, high selectivity for high-carbon olefins, especially olefins with more than 12 carbon atoms, fast adsorption and desorption rates, and can effectively inhibit the isomerization and polymerization reactions of olefins.

[0044] In a second aspect, the present invention provides a method for preparing the above-mentioned adsorbent, comprising the following steps:

[0045] (1) mixing NaX molecular sieve with clay, rolling into balls, screening, drying and calcining to obtain molecular sieve balls;

[0046] (2) in-situ crystallizing the molecular sieve beads obtained in step (1) with an alkaline solution, and then washing and drying to obtain NaX molecular sieve matrix beads;

[0047] (3) Use K + , Rb + and Cs + The NaX molecular sieve matrix beads obtained in step (2) are subjected to cation exchange with an alkali metal salt solution of one or more alkali metal ions, and then washed with water and dried to obtain alkali metal ion-exchanged NaX molecular sieve beads;

[0048] (4) calcining and activating the NaX type molecular sieve pellets obtained in step (3) to a calcination base amount of ≤1.5% by mass based on the mass of the NaX type molecular sieve pellets.

[0049] It should be noted that in the preparation method of the present invention, step (1) is the agglomeration of the active component and the binder, and the agglomeration method is rolling ball forming; in the molecular sieve spheres obtained by step (1), the surface of the NaX molecular sieve is wrapped or coated by clay; after the in-situ crystallization of step (2), part of the silicon source and aluminum source in the clay coated on the surface of the NaX molecular sieve are extracted from the spheres to the surface of the spheres and the pores, and then NaX molecular sieve crystals are generated on the inner wall and surface of the pores of the molecular sieve spheres, and the remaining silicon and aluminum source of the clay in the spheres exists as a matrix in the NaX molecular sieve matrix spheres. Therefore, after the in-situ crystallization of step (2), the binder component (clay) in the molecular sieve spheres is crystallized into NaX molecular sieve to increase the adsorption capacity of the adsorbent.

[0050] According to one embodiment, the clay in step (1) is kaolinite, dickite, perlite, refractory stone or halloysite.

[0051] It should be noted that the binder may be a kaolin mineral, specifically kaolinite, dickite, perlite, refractory stone, halloysite, etc., preferably halloysite.

[0052] According to one implementation mode, in step (1):

[0053] The mass ratio of the NaX molecular sieve to the clay is (90-95):(5-10), and small balls with a particle size of 0.3 mm to 1.0 mm are sieved out through the sieving. The drying temperature is 80° C. to 100° C., and the calcining temperature is 500° C. to 700° C.

[0054] Based on one embodiment, in step (2): the alkaline solution is a mixed solution of sodium hydroxide and water glass, the concentration of sodium hydroxide in the mixed solution is 0.5mol / L to 2.5mol / L, and the mass concentration of water glass in terms of silicon dioxide is 5g / L to 15g / L. Preferably, the concentration of sodium hydroxide in the mixed solution is 1mol / L to 1.5mol / L, and the mass concentration of water glass in terms of silicon dioxide is 5 to 10g / L. The temperature of the in-situ crystallization is 85°C to 95°C, and the time is 4h to 6h. The water washing is carried out until the pH of the washed water is less than 9, and the drying temperature is 80°C to 100°C, or 80°C to 110°C. When performing in-situ crystallization, the liquid-to-solid ratio (v) of the alkaline solution to the molecular sieve beads can be 2:1.

[0055] According to one embodiment, in step (3), the alkali metal salt solution comprises one or more of the chloride, nitrate and carbonate of the alkali metal ion. + The ion concentration is 0.1mol / L~0.3mol / L, and / or Rb + The ion concentration is 0.05mol / L~0.3mol / L, and / or Cs + The ion concentration is 0.15mol / L to 0.4mol / L. It should be noted that in the alkali metal salt solution, K + , Rb + or Cs + The ion concentration can be 0.05mol / L to 0.5mol / L, preferably 0.15mol / L to 0.4mol / L. The time of the cation exchange is 4-10 hours. The temperature of the cation exchange is 85°C to 105°C. The water washing is performed until no salt solution remains, and the drying temperature is 80°C to 100°C.

[0056] It should be noted that in step (3), by controlling the K + , Rb + and / or Cs + The ion concentration, cation exchange time, and volume space velocity / liquid-to-solid volume ratio of the alkali metal salt solution can make the prepared adsorbent have K + , Cs + and Rb + One or more ions in the X-type molecular sieve occupy 40 to 60% of the exchangeable cation sites.

[0057] It should be noted that the cation exchange in step (3) can be carried out by a column exchange method or a step-by-step kettle exchange method. When the cation exchange is carried out by a column exchange method, K +The ion concentration is 0.1mol / L~0.3mol / L, and / or Rb + The ion concentration is 0.05mol / L~0.3mol / L, and / or Cs + The ion concentration is 0.15mol / L to 0.4mol / L, and the volume space velocity of the alkali metal salt solution is 3.5L / h to 5L / h. For example, when the volume space velocity is 4L / h, the liquid-to-solid volume ratio of the alkali metal salt solution to the NaX molecular sieve matrix beads is 30:1. When the cation exchange is performed by the step-by-step kettle exchange method, 0.1mol / L to 0.3mol / L of K + Salt solution, 0.05mol / L~0.3mol / L Rb + Salt solution and 0.15mol / L~0.4mol / L Cs + The salt solution is subjected to cation exchange respectively, wherein the liquid-to-solid volume ratio during each step-by-step kettle exchange can be (2-4):1.

[0058] It should be noted that the same alkali metal ion can be exchanged multiple times using the step-by-step kettle exchange method, and the concentration of the alkali metal ion in the alkali metal salt solution during the two exchanges can be the same or different.

[0059] According to one embodiment, in step (4), the calcination activation temperature is 400° C. to 600° C. The calcination activation is performed to a base amount of ≤1% by mass based on the mass of the NaX molecular sieve pellets.

[0060] It should be noted that the calcination in step (4) can be carried out at 400° C. to 600° C. in a nitrogen or dry air atmosphere. For example, during the calcination in a nitrogen atmosphere, the moisture content can be controlled by controlling the activation temperature and time. After the activation is completed, the adsorbent can be calcined again, and the moisture content can be determined by the ratio of the reduced weight to the weight of the adsorbent.

[0061] The present invention is further illustrated by examples below, but the present invention is not limited thereto. The reagents used in the following examples, except for those otherwise specified, can all be commercially available finished reagents. Among them, the NaX molecular sieve used is from Sinopec Catalyst Qilu Branch.

[0062] In the following examples / comparative examples, the proportion of alkali metal cations in the exchangeable cation sites was measured by X-ray fluorescence spectroscopy analysis and the calculation method was (in terms of Cs + Taking the exchangeable cation site ratio as an example, the exchangeable cation of X-type molecular sieve is Cs + and Na + ): Cs + The proportion of exchangeable cation sites = σ Cs2O ÷MCs2O ÷(σ Cs2O ÷M Cs2O +σ Na2O ÷M Na2O ), where σ Cs2O is the mass fraction of Cs2O in the adsorbent measured by X-ray fluorescence spectroscopy, M Cs2O is the relative molecular mass of Cs2O, σ Na2O is the mass fraction of Na2O in the adsorbent measured by X-ray fluorescence spectroscopy, M Na2O is the relative molecular mass of Na2O. The calculation method for the proportion of other alkali metal cations in the exchangeable cation sites is the same as above. It should be noted that the exchangeable cations of the X-type molecular sieve include several alkali metal ions, and the denominator (bracket) corresponds to the data of these alkali metal ions.

[0063] Example 1

[0064] (1) Preparation of pellets

[0065] A certain amount of NaX molecular sieve (silicon oxide / aluminum oxide molar ratio in the framework is 2.2, average crystal particle size is 1 μm, relative crystallinity is 91%) and halloysite are uniformly mixed according to a mass ratio of 95:5, the mixed powder is added into a rotary high-speed granulator for rolling, deionized water is sprayed into the material and the mixed powder is scattered during the rolling process, and the water used for spraying is 38% of the mass of the mixed powder; small balls with a diameter of 0.3 mm to 0.8 mm are sieved, dried at 100° C., and calcined at 540° C. for 4 hours to obtain small balls;

[0066] (2) In-situ crystallization

[0067] The above-mentioned small balls are placed in a mixed solution of 1.5 mol / L sodium hydroxide and water glass (silicon dioxide concentration 10 g / L) for crystallization at a temperature of 95° C. for 6 hours; the crystallized small balls are washed with deionized water until the pH of the washed water is less than 9, and dried at 95° C. for 12 hours to obtain NaX alkali-treated balls;

[0068] (3) Ion exchange

[0069] The NaX alkali-treated balls obtained in step (2) were subjected to ion exchange by a column exchange method, wherein the exchange liquid was a 0.20 mol / L cesium chloride salt solution; the ion exchange conditions were: temperature 95°C, pressure 0.1 MPa, exchange liquid volume space velocity 4 L / h, exchange time 8 h, and the volume ratio of the cesium chloride salt solution to the balls was 30:1; after the ion exchange was completed, the balls were washed with deionized water 10 times the volume of the balls, dried, and calcined in a nitrogen flow at 500°C for 6 hours to obtain an adsorbent X-1, wherein Cs + The ions account for 52% of the exchangeable cationic sites and the alkali groups account for 99.0%.

[0070] Example 2

[0071] The adsorbent was prepared according to the method of Example 1, except that the exchange solution used in the ion exchange process in step (3) was a 0.30 mol / L cesium chloride salt solution, the exchange time was 10 h, and the volume ratio of the cesium chloride salt solution to the beads was 30:1. Adsorbent X-2 was prepared. Cs + The ions account for 60% of the exchangeable cationic sites and the alkali groups account for 99.1%.

[0072] Example 3

[0073] The adsorbent was prepared according to the method of Example 1, except that the ion exchange in step (3) was a step-by-step kettle exchange. The first step was carried out with a 0.15 mol / L cesium chloride salt solution for 4 h, and the second step was carried out with a 0.20 mol / L cesium chloride salt solution for 4 h. Adsorbent X-3 was obtained. Cs + The ions accounted for 43% of the exchangeable cationic sites and the alkali sites accounted for 99.2%. The liquid-to-solid volume ratio was 4:1 during both exchanges.

[0074] Example 4

[0075] The adsorbent was prepared according to the method of Example 1, except that the exchange solution used in the ion process of step (3) was a 0.15 mol / L rubidium chloride salt solution, the exchange time was 8 h, and the volume ratio of the rubidium chloride salt solution to the beads was 30:1. Adsorbent X-4 was obtained. Rb + The ions account for 49% of the exchangeable cationic sites and the alkali groups account for 99.3%.

[0076] Example 5

[0077] The adsorbent was prepared according to the method of Example 1, except that the exchange solution used in the ion process of step (3) was a 0.25 mol / L rubidium chloride salt solution, the exchange time was 10 h, and the volume ratio of the rubidium chloride salt solution to the beads was 30:1. Adsorbent X-5 was prepared. Rb + The ions account for 57% of the exchangeable cationic sites and the alkali groups account for 99.1%.

[0078] Example 6

[0079] The adsorbent was prepared according to the method of Example 1, except that the exchange liquid used in the ion process of step (3) was a 0.10 mol / L rubidium chloride salt solution, the exchange time was 10 h, and the volume ratio of the rubidium chloride salt solution to the beads was 30:1. Adsorbent X-6 was prepared. Rb + The ions account for 43% of the exchangeable cationic sites and the alkali groups account for 99.0%.

[0080] Example 7

[0081] The adsorbent was prepared according to the method of Example 1, except that the exchange solution in step (3) was a mixed solution of potassium chloride and cesium chloride salt solution, wherein the concentration of the potassium chloride solution was 0.15 mol / L, and the concentration of the cesium chloride solution was 0.2 mol / L, to obtain adsorbent X-7. Cs in adsorbent X-7 was 0.15 mol / L. + ions account for 54% of the exchangeable cation sites, K + The ions account for 2% of the exchangeable cationic sites and the alkali groups account for 99.3%.

[0082] Comparative Example 1

[0083] (1) Preparation of pellets

[0084] A certain amount of NaX molecular sieve (with a silicon oxide / aluminum oxide molar ratio of 2.3 in the framework, an average grain size of 1 μm, and a relative crystallinity of 91%) and halloysite are uniformly mixed according to a mass ratio of 95:5, and the mixed powder is added into a rotary high-speed granulator for rolling. During the rolling process, deionized water is sprayed into the material and the mixed powder is scattered. The water used for spraying is 38% of the mass of the mixed powder. Small balls with a diameter of 0.3 mm to 0.8 mm are sieved, dried at 100° C., and calcined at 540° C. for activation for 4 hours.

[0085] (2) In-situ crystallization

[0086] The above-mentioned small balls were placed in a mixed solution of 1.5 mol / L sodium hydroxide and water glass (silicon dioxide concentration 10 g / L) for crystallization, wherein the liquid-to-solid ratio was 2, the crystallization temperature was 95°C, and the time was 6 hours. The crystallized small balls were washed with deionized water until the pH of the washed water was less than 9, and dried in an oven at 110°C for 12 hours to obtain NaX alkali-treated balls, which were then calcined and activated at 500°C in a nitrogen atmosphere to obtain adsorbent Y-1, and the alkali content of adsorbent Y-1 was 99.3%.

[0087] Comparative Example 2

[0088] The adsorbent was prepared according to the method of Example 1, except that the ion exchange in step (3) was performed in a kettle, the concentration of the cesium chloride salt solution was 0.10 mol / L, and the exchange time was 6 h. Adsorbent Y-2 was obtained. Cs + The ions account for 28% of the exchangeable cationic sites and the alkali groups account for 99.1%.

[0089] Comparative Example 3

[0090] The adsorbent was prepared according to the method of Example 1, except that the exchange solution used in the ion exchange process in step (3) was a 0.50 mol / L cesium chloride salt solution, the exchange time was 10 h, and the volume ratio of the cesium chloride salt solution to the beads was 40:1. Adsorbent Y-3 was prepared. Cs + The ions account for 71% of the exchangeable cationic sites and the alkali groups account for 99.2%.

[0091] Comparative Example 4

[0092] The adsorbent was prepared according to the method of Example 1, except that after the ion exchange in step (3), the pellets were washed with deionized water 10 times the volume of the pellets and activated in a nitrogen stream at 350° C. for 6 hours to obtain adsorbent Y-4. Cs + The ions account for 51% of the exchangeable cationic sites and the alkali groups account for 98.2%.

[0093] Comparative Example 5

[0094] The adsorbent was prepared according to the method of Example 1, except that after the ion exchange in step (3), the pellet was washed with deionized water 10 times the volume of the pellet and activated in a nitrogen stream at 300°C for 6 hours to obtain adsorbent Y-5. + The ions account for 52% of the exchangeable cationic sites and the alkali groups account for 97.5%.

[0095] Test Example 1

[0096] In the adsorption separation operation, adsorption selectivity and adsorption-desorption rate are important indicators for measuring the performance of the adsorption separation system. The olefin / alkane adsorption separation performance of adsorbents X-1 to X-7 prepared in Examples 1-7 and adsorbents Y-1 to Y-5 prepared in Comparative Examples 1-5 was tested, and the adsorption performance of the adsorbents is shown in Table 1.

[0097] Specifically, Figure 2 As shown, the adsorbent performance is measured by a pulse test device and a dynamic pulse test method (single column pulse test). The first adsorption column 9 used in the pulse test is a stainless steel coil with an inner diameter of 6 mm and a length of 2300 mm, and the adsorbent filling amount is about 65 mL. It is placed in an automatic temperature-controlled internal heating furnace 8 for heating. The pulse liquid 1 and the desorption liquid 2 are fed into the first adsorption column 9 by a micro plunger pump. The upper outlet of the first adsorption column 9 is connected to the first back pressure valve 10 and connected to the effluent collector. The first back pressure valve 10 controls the system pressure.

[0098] The pulse liquid components used in the experiment are 5% by mass of 1-decene, n-decane, 1-undecene, n-undecane, 1-dodecene, n-dodecane, 1-tridecene, n-tridecane, 1-tetradecene, n-tetradecane, 1-hexadecene, n-hexadecane, each accounting for 5% by mass, and 40% by mass of isooctane, and the desorption liquid (desorbent) is 50% by mass of 1-hexene and 50% by mass of n-hexane.

[0099] The dynamic pulse test process is as follows: the activated and dehydrated adsorbent is loaded into the first adsorption column 9 and shaken to fill, N2 is introduced to remove the air in the system, and the desorption liquid 2 is introduced to increase the system pressure to 1.2MPa. The desorption liquid 2 is fed to the first preheating furnace 6 through a feed pump to gradually increase the temperature of the desorption liquid 2 to 135°C, and then the injection of the desorption liquid 2 is stopped for 1.0h. -1 After 8 mL of pulse liquid 1 is passed through at a volumetric space velocity, the desorption liquid 2 is re-injected for desorption, and the effluent sample is taken at the first sampling port 11 every 2 mL for composition analysis. Among them, the first adsorption column 9 is composed of an internal heating furnace 8 and a first external insulation sleeve 7 to maintain a constant temperature in the first adsorption column 9; after the experiment, the material in the first adsorption column 9 is switched to the waste liquid tank 12 through the first back pressure valve 10. The pulse liquid 1 and the desorption liquid 2 are respectively provided with a first exhaust port 3 on the pipeline entering the system. N2 enters the system after the flow is counted by the first rotor flowmeter 4. The first blind end 5 is arranged on the pipeline between the first rotor flowmeter 4 and the first preheating furnace 6.

[0100] like Figure 1 As shown in the figure (the adsorption column is filled with the adsorbent prepared in Example 1), the injection volume of the desorption liquid (desorbent) is used as the abscissa, and the mass concentration of each component in the pulse liquid is used as the ordinate. The pulse envelope curve of each component in the pulse feed is drawn, and the separation degree (R) and half peak width (W) of each component are calculated. 1 / 2 ). The narrower the half-peak width of the envelope of each component, the faster the adsorption and desorption rate of the adsorbent for the component. According to the effective pore volume of the adsorbent, the dead volume of the adsorption system is given, which is taken as the zero point, and the distance from the midpoint of the half-peak width of the envelope curve of each component to the zero point is measured as the net retention volume (ΔM). Separation degree (R) is one of the indicators of the separation efficiency of the adsorbent. The separation degree is equal to the ratio of the difference in the net retention volume of adjacent pulse peaks to the average half-peak width of the two pulse peaks. Under the same operating parameters, the greater the separation degree, the better the adsorption separation performance.

[0101] Table 1

[0102]

[0103] From the data in Table 1, it can be seen that K + , Cs + and / or Rb + The higher the proportion, the better. In Example 3, Cs +ions account for 71% of the exchangeable cation sites, with C 10 = / nC 10 and C 11 = / nC 11 The separation effect is reduced.

[0104] Test Example 2

[0105] The olefin isomerization reaction degrees of the adsorbents X-1 to X-7 prepared in Examples 1-7 and the adsorbents Y-1 to Y-5 prepared in Comparative Examples 1-5 were tested. The results are shown in Table 2.

[0106] Specifically, the degree of olefin isomerization (Di) is determined by Figure 3 The continuous pulse cycle test device shown is measured using a continuous pulse cycle test (long-term pulse cycle test).

[0107] The collector at the lower end outlet of the second adsorption column 27 of the pulse test device is connected to the pulse feed tank, and a long-term pulse circulation test is carried out. The circulating liquid is 1 kg of a mixed solution (mass fraction 50% 1-hexene + 50% n-hexane). During the pulse circulation process, the components of the circulating liquid for a certain circulation time are analyzed, and the degree of isomerization reaction (Di) is calculated by the mass fraction loss of 1-hexene. The degree of isomerization reaction (Di) = (M0-Mx) ÷ M0, where Mx is the mass fraction of 1-hexene in the circulating liquid after a certain circulation time, and M0 is the mass fraction of 1-hexene in the initial circulating liquid. The test results of the degree of isomerization reaction at different times are shown in Table 2.

[0108] Through Figure 3 When the continuous pulse cycle test device shown in the figure is tested, the activated and dehydrated adsorbent is loaded into the second adsorption column 27 for shaking and filling, N2 is introduced to remove the air in the system, and the circulating liquid 21 is introduced to increase the system pressure to 1.2MPa. The flow of N2 is counted by the second rotor flowmeter 24, and then flows into the system; after the test, the nitrogen in the system flows out through the second exhaust port 23 when it needs to flow out. The second blind end 25 is located in the pipeline between the second rotor flowmeter 24 and the second preheating furnace 30. The circulating liquid 21 is fed to the second preheating furnace 30 through the feed pump, so that the temperature of the circulating liquid 21 is increased to 135°C, and the temperature in the second adsorption column 27 is kept constant by the heating furnace 28 and the second outer insulation jacket 29. After the adsorbent is separated, the circulating liquid 21 returns to the circulating liquid tank 32 through the outlet of the second adsorption column 27, and samples are taken at the second sampling port 22 through the three-way valve before returning. After the experiment, the circulating liquid 21 after the experiment is dehydrated and recovered by the water absorption drying tank 31. The circulating fluid 21 is switched to the water absorption desiccant tank 31 via the second back pressure valve 26 .

[0109] Table 2

[0110]

[0111] Test Example 3

[0112] According to the method of Test Example 2, the olefin isomerization reaction degree of the adsorbents X-1 to X-7 prepared in Examples 1-7 and the adsorbents Y-1 to Y-5 prepared in Comparative Examples 1-5 was tested, except that the circulating liquid was 1 kg of a mixed solution containing 50% by mass of 1-dodecene and 50% by mass of n-dodecane, and the results are shown in Table 3. Isomerization reaction degree (Di) = (M0-Mx) ÷ M0, where Mx is the mass fraction of 1-dodecene in the circulating liquid after a certain period of circulation, and M0 is the mass fraction of 1-dodecene in the initial circulating liquid.

[0113] Table 3

[0114]

[0115] From the data in the above table, we can see that K + , Cs + and / or Rb + When the proportion exceeds a certain value, it no longer has a significant effect on controlling the degree of isomerization reaction.

[0116] In α-olefins, the carbon-carbon double bond in the α-olefin with a larger carbon number has a smaller effect on the properties of the entire olefin molecule, the closer the properties of the α-olefin are to the alkanes with the same carbon number, and the greater the technical difficulty of separating the α-olefin from the mixture. It can be seen from the above test results that, firstly, the adsorbent of the present invention has high adsorption selectivity for high-carbon olefins, especially olefins with 12 carbon numbers and above, and a fast mass transfer rate. Secondly, it can effectively inhibit the isomerization reaction and polymerization reaction of olefins, especially the low degree of isomerization reaction of olefins with 12 carbon numbers and above, which can significantly improve the olefin yield and extend the life of the adsorbent and desorbent; the adsorbent of the present invention is used to simulate the moving bed adsorption separation process to separate olefins and alkanes, which can greatly reduce energy consumption and improve the economy of the process.

[0117] Test Example 4

[0118] The mass percentage of the active component molecular sieve in the adsorbent prepared in Examples 1-7 was tested, and the results are shown in Table 4.

[0119] Specifically, the proportion of active component molecular sieve in the adsorbent is measured by toluene adsorption. The toluene adsorption of NaX molecular sieve raw powder used to prepare the adsorbent in Examples 1-7 is used as the standard sample. The ratio of toluene adsorption of different adsorbents to the standard sample is the proportion of active component molecular sieve.

[0120] Table 4

[0121]

[0122] It can be seen from the data in Table 4 that in the method for preparing the adsorbent of the present invention, the binder component in the molecular sieve beads is transformed into X molecular sieve through in-situ crystallization, which can increase the mass proportion of the active molecular sieve and further increase the adsorption capacity of the adsorbent.

[0123] In the description of the present application, it should be noted that the terms "upper", "lower", "inside", "outside", "front", "back", "left", "right", etc. indicate directions or positional relationships based on the directions or positional relationships in the working state of the present application. They are only for the convenience of describing the present application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific direction, be constructed and operated in a specific direction. Therefore, they should not be understood as limitations on the present application.

[0124] In the description of this application, it should be noted that, unless otherwise clearly specified and limited, the terms "install", "connect" and "connect" should be understood in a broad sense. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to specific circumstances.

[0125] The present application has been described above in conjunction with preferred embodiments, but these embodiments are only exemplary and serve only as an illustration. On this basis, various replacements and improvements may be made to the present application, all of which fall within the scope of protection of the present application.

Claims

1. An adsorbent for the adsorption and separation of olefins and alkanes, characterized in that: The invention comprises an active component and a binder, wherein the active component is an X-type molecular sieve, and 40 to 60% of the exchangeable cations of the X-type molecular sieve are K + , Cs + and Rb + One or more of the following, the remaining exchangeable cations being Na + ; The moisture content of the adsorbent is ≤1.5% by mass.

2. The adsorbent according to claim 1, characterized in that The molar ratio of silicon oxide to aluminum oxide in the X-type molecular sieve is 2.0 to 3.0, preferably 2.2 to 2.

5.

3. The adsorbent according to claim 2, characterized in that The average particle size of the X-type molecular sieve is 0.5 μm to 3.5 μm, preferably 0.8 μm to 1.2 μm.

4. The adsorbent according to claim 3, characterized in that The particle size of the adsorbent is 0.3 mm to 1.0 mm.

5. The adsorbent according to claim 4, characterized in that Based on the mass of the adsorbent, the mass proportion of the active component is 95.0% to 99.5%, and the mass proportion of the binder is 0.5% to 5.0%.

6. The adsorbent according to claim 5, characterized in that 45-55% of the exchangeable cations of the X-type molecular sieve are K + , Cs + and Rb + One or more of the following, the remaining exchangeable cations being Na + .

7. The adsorbent according to claim 1, characterized in that The adsorbent is used to separate α-olefins and alkanes with carbon numbers of 6 to 16; Preferably, the adsorbent is used to separate α-olefins and alkanes having a carbon number of 12-16.

8. A method for preparing the adsorbent according to any one of claims 1 to 7, characterized in that: The steps include: (1) mixing NaX molecular sieve with clay, rolling into balls, screening, drying and calcining to obtain molecular sieve balls; (2) in-situ crystallizing the molecular sieve beads obtained in step (1) with an alkaline solution, and then washing and drying to obtain NaX molecular sieve matrix beads; (3) Use K + , Rb + and Cs + The NaX molecular sieve matrix beads obtained in step (2) are subjected to cation exchange with an alkali metal salt solution of one or more alkali metal ions, and then washed with water and dried to obtain alkali metal ion-exchanged NaX molecular sieve beads; (4) calcining and activating the NaX type molecular sieve pellets obtained in step (3) to a calcination base amount of ≤1.5% by mass based on the mass of the NaX type molecular sieve pellets.

9. The method according to claim 8, characterized in that The clay in step (1) is kaolinite, dickite, perlite, refractory stone or halloysite.

10. The method according to claim 9, characterized in that In step (1): The mass ratio of the NaX molecular sieve to the clay is (90-95):(5-10), and small balls with a particle size of 0.3 mm to 1.0 mm are sieved out through the sieving. The drying temperature is 80° C. to 100° C., and the calcining temperature is 500° C. to 700° C.

11. The method according to claim 10, characterized in that In step (2): The alkaline solution is a mixed solution of sodium hydroxide and water glass, the concentration of sodium hydroxide in the mixed solution is 0.5 mol / L to 2.5 mol / L, and the mass concentration of water glass in terms of silicon dioxide is 5 g / L to 15 g / L; The temperature of the in-situ crystallization is 85°C to 95°C, and the time is 4h to 6h; the water washing is carried out until the pH of the washed water is less than 9, and the temperature of the drying is 80°C to 100°C.

12. The method according to claim 11, characterized in that In step (3): The alkali metal salt solution comprises one or more of chloride, nitrate and carbonate of the alkali metal ion; In the alkali metal salt solution, K + The ion concentration is 0.1mol / L~0.3mol / L, and / or Rb + The ion concentration is 0.05mol / L~0.3mol / L, and / or Cs + The ion concentration is 0.15mol / L~0.4mol / L; The cation exchange time is 4-10h, and the cation exchange temperature is 85°C to 105°C; The water washing is performed until no salt solution remains, and the drying temperature is 80°C to 100°C.

13. The method according to claim 12, characterized in that In step (4): The calcination activation temperature is 400°C to 600°C; The calcination activation is performed to a base amount of ≤1% by mass based on the mass of the NaX type molecular sieve pellets.

Citation Information

Patent Citations

  • Mesoporous X-type molecular sieve, adsorbent based on molecular sieve, and preparation and application thereof

    CN104477937A

  • Adsorbent for separating ethylbenzene from C8 aromatic hydrocarbons, and preparation method thereof

    CN106552582A

  • Ethylbenzene adsorbent and preparation method therefor

    CN106552583A

  • Coalescence type adsorbent preparation method

    CN110508240A

Cited By

  • Tail gas adsorbent evaluation method and application

    CN118937147A