Adsorbent for hyaluronic acid purification and impurity removal and preparation method thereof

By using particle regulators to form micelles in the preparation of silica gel, the particle size of silica gel nanoparticles can be precisely adjusted to increase the specific surface area, solving the problem of insufficient adsorption capacity of existing silica gel adsorbents and achieving efficient purification and impurity removal of hyaluronic acid. Reduce waste residue generation.

CN118718982APending Publication Date: 2024-10-01QILU UNIVERSITY OF TECHNOLOGY (SHANDONG ACADEMY OF SCIENCES)
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410719753.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-05
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The existing silica gel adsorbent has a small specific surface area, resulting in insufficient adsorption and separation capabilities for proteins in hyaluronic acid, increasing treatment costs and producing protein-rich waste residue, causing environmental pressure.

Method used

By adding a suitable concentration of particle regulator solution during the silica gel preparation process, micelles are formed to limit excessive dehydration condensation and particle agglomeration of orthosilicic acid, precisely adjust the particle size of silica gel nanoparticles, and increase the specific surface area.

Benefits of technology

It significantly increases the specific surface area of ​​the silica gel adsorbent, enhances the adsorption and separation ability of proteins in hyaluronic acid, achieves efficient purification and impurity removal, reduces the amount of adsorbent and reduces the generation of waste residue.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118718982A_ABST
    Figure CN118718982A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of silica gel preparation, and particularly relates to an adsorbent for hyaluronic acid purification and impurity removal and a preparation method thereof. The preparation method comprises the following steps: (1) preparing sol: firstly, adding a solution of a particle regulator into a raw material sodium silicate solution, and uniformly mixing; adding the raw material sulfuric acid solution into the sodium silicate solution for reaction to prepare sol; the particle conditioning agent is one or more of hexadecyl trimethyl ammonium bromide, hexadecyl trimethyl ammonium chloride or dodecyl trimethyl ammonium bromide; (2) preparing gel: sequentially carrying out aging, alkali soaking and water washing on the obtained sol to prepare the gel; and (3) preparing the adsorbent: drying and activating the prepared gel to obtain the adsorbent. The specific surface area of the prepared adsorbent reaches 530-750m < 2 > / g, the adsorption separation capacity on protein in hyaluronic acid is enhanced, and efficient purification and impurity removal of hyaluronic acid are realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of silica gel preparation, and specifically relates to an adsorbent for purifying and removing impurities from hyaluronic acid and a preparation method thereof. Background Art

[0002] Hyaluronic acid is an acidic mucopolysaccharide. Its unique molecular structure and physical and chemical properties show a variety of important physiological functions in the body, such as lubricating joints, regulating the permeability of blood vessel walls, regulating the diffusion and movement of proteins, water and electrolytes, and promoting wound healing. More importantly, hyaluronic acid has a special water-retaining effect. It is the best moisturizing substance found in nature and is called an ideal natural moisturizing factor. For example, a 2% pure hyaluronic acid aqueous solution can firmly retain 98% of water. These excellent properties make it an important raw material for cosmetics, medicines, foods and health products.

[0003] Hyaluronic acid is generally prepared by microbial fermentation, with glucose as the carbon source fermentation liquid, and streptococci, lactic acid cocci and other bacteria are selected to ferment in the culture medium for 48 hours. After the fermentation is completed, the fermentation product obtained is a colloidal solution rich in enzymes and other proteins. The fermentation product needs to be purified and impurities removed to obtain a high-purity, high-quality hyaluronic acid product.

[0004] At present, silica gel is widely used as an adsorbent to purify and remove impurities from hyaluronic acid, especially for the removal of enzymes and other proteins that are rich in hyaluronic acid. Silica gel is made by acidifying sodium silicate with sulfuric acid, so that silicate ions and hydrogen ions combine to form orthosilicic acid and precipitate, and then spontaneously dehydrate and condense to form polysilicic acid aging products. The surface of silica gel is rich in hydroxyl groups and has a strong binding ability to proteins, so it is extremely suitable for the purification and removal of hyaluronic acid.

[0005] The overall adsorption capacity of silica gel is highly dependent on the size of the specific surface area. The formation of polysilicic acid has a crucial influence on the pore structure and specific surface area of ​​the final silica gel product. However, the formation of orthosilicic acid and its dehydration condensation process are usually difficult to accurately control, which can easily cause the particle size of silica gel particles to be too large, thereby bringing a huge negative impact on the specific surface area of ​​silica gel. The silica gel currently used to adsorb proteins such as enzymes in hyaluronic acid has a small adsorption specific surface area. The small specific surface area leads to insufficient adsorption and separation capacity per unit mass of adsorbent, and the adsorbent dosage required per unit fermentation liquid is large, which greatly increases the treatment cost. At the same time, a large amount of protein-rich eutrophic waste residues and waste liquids are produced, which puts great economic and environmental pressure on enterprises and the environment.

[0006] Therefore, it is urgent to develop a new type of silica gel adsorbent with a large specific surface area and strong ability to adsorb and separate proteins in hyaluronic acid, so as to achieve the purpose of efficient purification and impurity removal of hyaluronic acid. Summary of the invention

[0007] The present invention aims to provide a method for preparing an adsorbent for purifying and removing impurities from hyaluronic acid, by which a hyaluronic acid adsorbent with a specific surface area of ​​530-750m 2 / g of adsorbent enhances the adsorption and separation capacity of proteins in hyaluronic acid, achieving efficient purification and impurity removal of hyaluronic acid.

[0008] The present invention regulates the crystal nucleation and growth of silica gel nanoparticles produced by the reaction, thereby reducing the silica gel particle size and increasing the specific surface area. By adding a particle regulator solution of appropriate concentration to the sodium silicate solution used as the raw material for preparing silica gel in advance, micelles are used to limit the excessive dehydration condensation of orthosilicic acid and subsequent particle agglomeration during the subsequent acidification reaction, thereby limiting the increase in the particle size of the silica gel nanoparticles, so that the particle size of the silica gel adsorbent can be accurately adjusted within a certain range, achieving a significant increase in the specific surface area of ​​the silica gel, and thus improving the adsorption and separation efficiency.

[0009] The specific technical solutions are as follows:

[0010] A method for preparing an adsorbent for purifying and removing impurities from hyaluronic acid comprises the following steps:

[0011] (1) Preparation of sol:

[0012] First, add the particle regulator solution to the raw sodium silicate solution and mix them evenly; then add the raw sulfuric acid solution to the sodium silicate solution, react at 25-40°C, and adjust the pH value to 3-4.

[0013] The concentration of the particle regulator solution is 0.1-10 g / L; the volume ratio of the particle regulator solution to the sodium silicate solution is 1:1-10.

[0014] The particle regulator is one or more of dodecyltrimethylammonium bromide, hexadecyltrimethylammonium chloride or hexadecyltrimethylammonium bromide.

[0015] After the reaction is completed, the pH value is maintained at 3-4 to prepare a sol.

[0016] The mass fraction of the sodium silicate solution can be 5-50%, the mass fraction of the sulfuric acid solution can be 5-70%, and the stirring speed can be 80-100 rpm.

[0017] In this step, a particle regulator solution of appropriate concentration is first added to the raw sodium silicate solution, so that a large number of tiny micelles can be formed in the solution during the subsequent process of adding sulfuric acid solution to the sodium silicate solution to acidify and form polysilicic acid. The small amount of orthosilicic acid solution wrapped in the micelles is isolated from the outside, which limits the condensation of orthosilicic acid molecules in the micelles or the agglomeration of particles, and prevents the unlimited epitaxial growth of silica gel particles. The orthosilicic acid concentration inside the micelles is limited, and the particles will not continue to grow after the condensation substrate is exhausted, thereby achieving the purpose of reducing the silica gel particle size and increasing the specific surface area.

[0018] (2) Preparation of gel: The sol obtained in step (1) is aged, soaked in alkali, and washed with water in sequence to obtain a gel.

[0019] (3) Preparation of adsorbent: The gel prepared in step (2) is dried and activated to obtain the adsorbent.

[0020] In the present invention, in the preparation method of the adsorbent, the concentration of the particle regulator solution in step (1) is 1-2.5 g / L, and the volume ratio of the particle regulator solution to the sodium silicate solution is 1:1-5. The particle regulator solution is an aqueous solution of the particle regulator.

[0021] In the present invention, in the method for preparing the adsorbent, in step (1), the concentration of the sodium silicate solution is 15-45wt%, and the concentration of the sulfuric acid solution is 50-70wt%.

[0022] In the present invention, in the method for preparing the adsorbent, the reaction in step (1) is carried out at 25-30°C.

[0023] In the present invention, in the preparation method of the adsorbent, the aging temperature in step (2) is 65-85° C. and the aging time is 0.5-2.5 h.

[0024] In the present invention, in the preparation method of the adsorbent, the alkaline soaking in step (2) is performed by soaking in a KOH solution for 5-10 minutes. The mass fraction of the KOH solution can be 10-45wt%.

[0025] In the present invention, in the method for preparing the adsorbent, the water washing in step (2) is performed with distilled water.

[0026] In the present invention, in the preparation method of the adsorbent, the drying temperature in step (3) is 70-120° C. and the drying time is 5-12 hours.

[0027] In the present invention, in the preparation method of the adsorbent, the activation in step (3) adopts a high-temperature calcination method, the calcination temperature is 400-500° C., and the calcination time is 3-4 hours.

[0028] An adsorbent for purifying and removing impurities from hyaluronic acid, which is prepared by the above-mentioned preparation method; the specific surface area of ​​the adsorbent is 530-750m 2 / g, particle size is 5.5-8nm, and pore size is 2.5-4nm.

[0029] The beneficial effects of the present invention are as follows: the preparation method of the present invention converts the traditional reaction solution into a colloid rich in micelles by adding a particle regulator solution of appropriate concentration to the sodium silicate solution, which is the raw material for preparing silica gel, in advance, and utilizes the micelles to limit the excessive dehydration condensation of orthosilicic acid and the subsequent particle agglomeration, thereby limiting the increase in the particle size of silica gel nanoparticles, so that the particle size of the silica gel adsorbent can be accurately adjusted within a certain range, thereby achieving a significant increase in the specific surface area of ​​the silica gel, and thus improving the adsorption efficiency.

[0030] The specific surface area of ​​the adsorbent prepared by the preparation method of the present invention can reach 530-750m 2 / g, it is estimated that if the hyaluronic acid of the same purity is obtained, the adsorbent prepared by the preparation method of the present invention is higher than the existing silica gel adsorbent (specific surface area 370m 2 / g) can be reduced by at least 30%.

[0031] In summary, the preparation method described in the present invention can accurately adjust the particle size of silica gel within a certain range, increase the specific surface area of ​​the silica gel adsorbent, enhance the adsorption and separation ability of proteins in hyaluronic acid, and achieve efficient purification and impurity removal of hyaluronic acid. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 This is a SEM image of the adsorbent of the present invention. DETAILED DESCRIPTION

[0033] The technical solution of the present invention is described in detail below.

[0034] Example 1

[0035] The preparation method of the adsorbent for purifying and removing impurities from hyaluronic acid comprises the following specific steps:

[0036] (1) Preparation of sol:

[0037] First, a 1 g / L hexadecyltrimethylammonium chloride aqueous solution is added to a 40 wt % sodium silicate solution and mixed evenly, wherein the volume ratio of the hexadecyltrimethylammonium chloride aqueous solution to the sodium silicate solution is 1:1.

[0038] Then, a sulfuric acid solution with a concentration of 50 wt % was added to the sodium silicate solution, and the reaction was carried out at 25° C. and stirred at a speed of 500 r / min, and the pH value was adjusted to 3.

[0039] After the reaction is completed, the pH value is maintained at 4 to prepare a sol.

[0040] (2) Preparation of gel: The sol obtained in step (1) was aged at 65° C. for 2.5 h, then immersed in a 30 wt % KOH solution for 10 min, and finally the filtrate was washed three times with distilled water to obtain a gel.

[0041] (3) Preparation of adsorbent: The gel prepared in step (2) was dried at 70° C. for 12 h, and then placed in a muffle furnace at 500° C. for high-temperature activation for 3 h to obtain the adsorbent.

[0042] Example 2

[0043] The preparation method of the adsorbent for purifying and removing impurities from hyaluronic acid comprises the following specific steps:

[0044] (1) Preparation of sol:

[0045] First, a 2.5 g / L aqueous solution of dodecyltrimethylammonium bromide was added to a 40 wt % sodium silicate solution and mixed evenly, wherein the volume ratio of the aqueous solution of dodecyltrimethylammonium bromide to the sodium silicate solution was 1:5.

[0046] Then, a sulfuric acid solution with a concentration of 50 wt % was added to the sodium silicate solution, and the reaction was carried out at 35° C. and stirred at a speed of 500 r / min, and the pH value was adjusted to 3.

[0047] After the reaction is completed, the pH value is maintained at 3 to prepare a sol.

[0048] (2) Preparation of gel: The sol obtained in step (1) was aged at 75° C. for 1 h, then immersed in a 40 wt % KOH solution for 10 min, and finally the filtrate was washed three times with distilled water to obtain a gel.

[0049] (3) Preparation of adsorbent: The gel prepared in step (2) was dried at 80° C. for 10 h, and then placed in a muffle furnace at 400° C. for high-temperature activation for 4 h to obtain the adsorbent.

[0050] Example 3

[0051] The preparation method of the adsorbent for purifying and removing impurities from hyaluronic acid comprises the following specific steps:

[0052] (1) Preparation of sol:

[0053] First, a 10 g / L hexadecyltrimethylammonium bromide aqueous solution is added to a 40 wt % sodium silicate solution and mixed evenly, wherein the volume ratio of the hexadecyltrimethylammonium bromide aqueous solution to the sodium silicate solution is 1:10.

[0054] Then, a sulfuric acid solution with a concentration of 50 wt % was added to the sodium silicate solution, and the reaction was carried out at 40° C. and stirred at a speed of 500 r / min, and the pH value was adjusted to 4.

[0055] After the reaction is completed, the pH value is maintained at 4 to prepare a sol.

[0056] (2) Preparation of gel: The sol obtained in step (1) was aged at 80° C. for 0.5 h, then immersed in a 20 wt % KOH solution for 10 min, and finally the filtrate was washed three times with distilled water to obtain a gel.

[0057] (3) Preparation of adsorbent: The gel obtained in step (2) was dried at 120° C. for 5 h, and then placed in a muffle furnace at 500° C. for high-temperature activation for 3.5 h to obtain the adsorbent.

[0058] Example 4

[0059] The difference from Example 1 is that the particle regulator used in this example is hexadecyltrimethylammonium bromide.

[0060] The rest is the same as in Example 1.

[0061] Comparative Example 1

[0062] The difference from Example 1 is that the particle regulator used in this comparative example is dodecyltrimethylammonium chloride.

[0063] The rest is the same as in Example 1.

[0064] Comparative Example 2

[0065] The difference from Example 1 is that the particle regulator used in this comparative example is tetradecyltrimethylammonium bromide.

[0066] The rest is the same as in Example 1.

[0067] Comparative Example 3

[0068] The difference from Example 1 is that in this comparative example, during the reaction process of preparing the sol in step (1), the pH value is adjusted to 5.

[0069] The rest is the same as in Example 1.

[0070] Comparative Example 4

[0071] The difference from Example 1 is that in this comparative example, during the reaction process of preparing the sol in step (1), the pH value is adjusted to 1.

[0072] The rest is the same as in Example 1.

[0073] The performance indicators of the adsorbents prepared by the preparation methods of the embodiments and comparative examples are shown in Table 1.

[0074] Table 1 Test indicators of each adsorbent

[0075]

[0076] Experimental Example 1

[0077] 1. Experimental purpose: To investigate the effect of the concentration of the particle regulator solution on the various indicators of the adsorbent.

[0078] 2. Experimental method: Referring to the steps of the preparation method described in Example 1, the single variable is set to the concentration of the aqueous solution of hexadecyltrimethylammonium chloride in step (1) as 0.05 g / L, 0.1 g / L, 0.5 g / L, 1 g / L, 2.5 g / L, 5 g / L, 10 g / L, and 11 g / L, respectively. The other steps and conditions are the same as those in Example 1.

[0079] 3. Experimental results: See Table 2 for details.

[0080] Table 2 Test indicators of each adsorbent

[0081]

[0082] Experimental Example 2

[0083] 1. Experimental purpose: To investigate the effect of the reaction temperature of sulfuric acid solution and sodium silicate solution containing particle regulator on various indicators of the adsorbent.

[0084] 2. Experimental method: Referring to the preparation method steps described in Example 1, the single variable is set to the reaction temperatures of the sodium silicate solution and the sulfuric acid solution in step (1) are 15° C., 25° C., 30° C., 35° C., 40° C., and 45° C., respectively. The other steps and conditions are the same as those in Example 1.

[0085] 3. Experimental results: See Table 3 for details.

[0086] Table 3 Test indicators of various silica gels

[0087]

Claims

1. A method for preparing an adsorbent for purifying and removing impurities from hyaluronic acid, characterized in that: The following steps are involved: (1) Preparation of sol: First, add the particle regulator solution to the raw sodium silicate solution and mix well; then add the raw sulfuric acid solution to the sodium silicate solution, react at 25-40°C, and adjust the pH value to 3-4; Wherein, the concentration of the particle regulator solution is 0.1-10 g / L; the volume ratio of the particle regulator solution: the sodium silicate solution is 1:1-10; The particle regulator is one or more of dodecyltrimethylammonium bromide, hexadecyltrimethylammonium chloride or hexadecyltrimethylammonium bromide; After the reaction is completed, the pH value is maintained at 3-4 to prepare a sol; (2) preparing gel: aging, alkali soaking and water washing the sol obtained in step (1) in sequence to obtain gel; (3) Preparation of adsorbent: The gel prepared in step (2) is dried and activated to obtain the adsorbent.

2. The method for preparing an adsorbent according to claim 1, characterized in that: The concentration of the particle regulator solution in step (1) is 1-2.5 g / L; the volume ratio of the particle regulator solution to the sodium silicate solution is 1:1-5.

3. The method for preparing an adsorbent according to claim 1, characterized in that: In the step (1), the concentration of the sodium silicate solution is 15-45wt%, and the concentration of the sulfuric acid solution is 50-70wt%.

4. The method for preparing an adsorbent according to claim 1, characterized in that: In the step (1), the reaction is carried out at 25-30°C.

5. The method for preparing an adsorbent according to claim 1, characterized in that: The aging temperature in step (2) is 65-85° C. and the aging time is 0.5-2.5 h.

6. The method for preparing an adsorbent according to claim 1, characterized in that: In the step (2), the alkaline soaking is performed by soaking in KOH solution for 5-10 minutes.

7. The method for preparing an adsorbent according to claim 1, characterized in that: The drying temperature in step (3) is 70-120° C. and the drying time is 5-12 hours.

8. The method for preparing an adsorbent according to claim 1, characterized in that: The activation in step (3) is carried out by calcination, the calcination temperature is 400-500° C., and the calcination time is 3-4 hours.

9. An adsorbent for purifying and removing impurities from hyaluronic acid, characterized in that: Prepared by the preparation method described in any one of claims 1 to 8; the specific surface area of ​​the adsorbent is 530-750m 2 / g, particle size is 5.5-8nm, and pore size is 2.5-4nm.

Citation Information

Patent Citations

  • Method of producing high-specific area nano-silicon dioxide

    CN101172608A

  • Preparation method of beer silica gel

    CN102079529A

  • Small-aperture silica gel clarifying agent as well as preparation method and application thereof

    CN118022701A

  • Method for preparing spherical mesoporous nano silicon dioxide by utilizing straw solid waste

    CN118026189A

  • Adsorptivity imparting agent containing porous silica

    US20070166438A1