Method for preparing ecological restoration material from stone mine tailings

Nano-silica is prepared through mechanical grinding and acid-base treatment, and is blended with activated cross-linked polystyrene and combined with EDTA modification to form an efficient adsorption material, which solves the problem of insufficient adsorption capacity of nano-silica in stone mine tailings slag. It achieves efficient removal and recovery of heavy metals and organic matter, ensuring resource reuse and environmental restoration.

CN118718983AActive Publication Date: 2024-10-01中电建路桥集团有限公司 +3

Patent Information

Application Number
CN202410754666.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-12
Publication Date
2024-10-01
Estimated Expiration
2044-06-12

AI Technical Summary

Technical Problem

The small particle size of nano-silica in stone mine tailings results in reduced adsorption capacity and difficulty in recycling. It also has insufficient absorption capacity for macromolecular organic matter and cannot effectively repair the ecological environment.

Method used

Nano-silica particles are prepared through mechanical grinding and acid-base treatment, and are blended with activated cross-linked polystyrene and combined with EDTA modification to form a composite material with high adsorption capacity. Its network structure and surface activity are used to improve the resistance to heavy metals and The adsorption capacity of organic matter and achieve uniform dispersion through ultrasonic dispersion.

Benefits of technology

It achieves efficient adsorption and recovery of heavy metals and organic matter, significantly improves the adsorption capacity of nanosilica, ensures effective removal of environmental pollutants, and the materials are easy to recycle, realizing the reuse of resources.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118718983A_ABST
    Figure CN118718983A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of preparation of ecological restoration materials from mine tailings, in particular to a method for preparing an ecological restoration material from stone mine tailings, which comprises the following steps: S1, mechanically grinding the stone mine tailings; s2, hydrochloric acid treatment and filtration; s3, calcining filter residues and carrying out alkali treatment; s4, adjusting the pH value, and filtering to obtain nano silicon dioxide; s5, performing linear polystyrene crosslinking; s6, cross-linked polystyrene is treated with concentrated acid; and S7, blending the activated crosslinked polystyrene, nano silicon dioxide and EDTA (Ethylene Diamine Tetraacetic Acid) to prepare the ecological restoration material. The nano silicon dioxide is prepared by utilizing the component properties of the tailing slag, and is blended with the activated crosslinked polystyrene and the EDTA, so that organic matters and heavy metals can be efficiently adsorbed, the environment-friendly effect is realized, and the resource of the tailing slag is effectively utilized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of preparing ecological restoration materials from mine tailings, and in particular to a method for preparing ecological restoration materials from stone mine tailings. Background Art

[0002] After the original ore is processed by the selection operation, its main components have been enriched in the concentrate. After some of the ore is neutralized, the minor components or other associated metals of the ore are also recovered. The remaining products with very low useful components are called final tailings. The tailings of stone mines not only occupy a large area, but also have frequent strong winds in autumn. If the particles of some mine tailings are small, it is easy to cause air pollution. Therefore, it is necessary to make resource utilization of mine stone tailings.

[0003] There are many types of stone mine tailings, and their main components include SiO 2 , Fe 2 O 3 , CaO, MgO and Al 2 O 3 etc., SiO 2 It is often the most abundant component in tailings. In some areas, SiO 2 The content can even exceed 80%. After functionalization, the surface of silica particles can be used to absorb heavy metal ions in the environment. For example, when silica particles are mixed with EDTA, the carboxyl and amino groups on them can absorb heavy metal ions and form stable chelates. Based on this characteristic, tailings containing a large amount of silica can be used to prepare silica particles to absorb heavy metal ions in the environment and repair the ecological environment.

[0004] In order to improve the adsorption of heavy metal ions, a larger surface area is often required, and the tailings are often required to be prepared into nano-silicon dioxide. However, due to its small particle size, nano-silicon dioxide is prone to agglomeration when dispersed in water, resulting in a decrease in adsorption capacity, and its particle size is too small to be easily recovered from the environment. In addition, the surface pore size of nano-silicon dioxide is too small, and its ability to absorb large molecular organic matter in the environment is relatively weak. In response to the problems raised in the background technology above, technical personnel in this field have proposed an ecological restoration material using stone mine tailings as raw materials, which can efficiently absorb heavy metals and organic matter in the environment, and is evenly dispersed and easy to recycle, thereby realizing the resource utilization of stone mine tailings. Summary of the invention

[0005] The purpose of the present invention is to provide a method for preparing ecological restoration materials from stone mine tailings to solve the problems raised in the above-mentioned background technology.

[0006] In order to achieve the above purpose, the following technical solutions are provided: A method for preparing ecological restoration materials from stone mine tailings, comprising the following steps: S1: Mechanically grind the stone mine tailings and pass them through a 50-mesh sieve to obtain fine stone mine tailings; S2: reacting the fine stone mine tailings obtained in step S1 with a hydrochloric acid solution, with mechanical stirring during the reaction, and the concentration of the hydrochloric acid used is 2 mol / L, filtering to obtain a filter residue after the reaction is completed, and washing the filter residue with deionized water; S3: putting the filter residue obtained by washing in step S2 into a muffle furnace for calcination, reacting the calcined filter residue with a sodium hydroxide solution in a reactor, heating to 80-95° C. during the reaction, the reaction time is 2-3 hours, filtering out the filter residue, and obtaining a silicate solution; S4: After cooling the silicate solution obtained in step S3, slowly add a 1 mol / L hydrochloric acid solution during stirring to adjust the pH of the solution to 6.2-7.2, a precipitate appears, the precipitate is filtered, washed with deionized water and then vacuum dried, and the obtained silica particles are ball-milled in a planetary ball mill to obtain nano-silicon dioxide; S5: adding linear polystyrene to carbon tetrachloride, adding anhydrous aluminum chloride, stirring and heating to react for 3-4 hours, the heating temperature is 50-80°C, nitrogen is introduced into the solution during the reaction, and then deionized water and anhydrous ethanol are added to terminate the reaction, filtering the residue obtained by the reaction, washing it with ethanol, and then vacuum drying it to obtain cross-linked polystyrene; S6: ultrasonically dispersing the cross-linked polystyrene obtained in step S5 into a mixed acid solution of concentrated sulfuric acid and concentrated nitric acid, stirring and reacting at 40-60° C. for 1-2.5 hours, filtering the solution after the reaction to obtain a filter residue, washing with ethanol, and drying to obtain activated porous cross-linked polystyrene; S7: Ultrasonic dispersion of the activated porous cross-linked polystyrene obtained in step S6 and the nano-silica obtained in step S4 into anhydrous ethanol, stirring for 2 hours, adding 0.1 mol / L EDTA aqueous solution, heating to 40-65°C, and continuing to stir and react for 2-3 hours, filtering to obtain the residue, washing with ethanol, and vacuum drying to obtain the prepared ecological restoration material.

[0007] Furthermore, in step S3, the calcination temperature of the filter residue is 900-1100° C., and the calcination time of the filter residue in the muffle furnace is 3-5 hours.

[0008] Furthermore, the particle size of the nano-silicon dioxide obtained by ball milling in the planetary ball mill in step S4 is 30-60 nm.

[0009] Furthermore, in step S5, the mass ratio of linear polystyrene, carbon tetrachloride, anhydrous aluminum chloride, deionized water and anhydrous ethanol is 1:(40-140):(1-10):(8-60):(2-10).

[0010] Furthermore, in step S6, the concentration of concentrated sulfuric acid is 98wt%, the concentration of concentrated nitric acid is 60wt%, and the volume ratio of concentrated sulfuric acid to concentrated sulfuric acid is 1:2.

[0011] Furthermore, in step S7, the mass ratio of activated porous cross-linked polystyrene, nano-silica and anhydrous ethanol is 1:(1.4-1.7):(20-40), and the volume ratio of anhydrous ethanol to EDTA aqueous solution is 1:0.5.

[0012] Compared with the prior art, the beneficial effects of the present invention are: 1. The present invention uses mine stone tailings as raw materials to prepare environmental repair materials, obtains nano-silicon dioxide particles with small particle size through mechanical grinding, high temperature and acid-base treatment, and grafts EDTA on the surface, which can effectively form stable chelates with heavy metal ions in water, not only effectively repairing the environment, but also saving resources; 2. The nano-silicon dioxide prepared from the mine stone tailings as raw materials in the present invention is blended with activated cross-linked polystyrene, which not only effectively increases the overall surface area of ​​the adsorption material, but also enables the composite material to have a strong adsorption capacity for organic matter; 3. The present invention prepares cross-linked polystyrene with a mesh-like porous structure by reacting linear polystyrene with anhydrous aluminum chloride in carbon tetrachloride, thereby improving its adsorption capacity. The cross-linked polystyrene is further treated with concentrated nitric acid and concentrated sulfuric acid, and nitro and amino groups can be introduced to effectively activate the surface of the polystyrene, and further make the surface of the polystyrene rough and loose, so that the silicon dioxide with strong surface activity itself can be more easily and evenly loaded on the surface of the polystyrene, and can more easily adsorb organic matter and heavy metals in the sewage environment. At the same time, since the polystyrene with a mesh structure is more likely to flocculate and precipitate when adsorbing pollutants, it is easy to synchronously recover the nano silicon dioxide prepared by stone mine tailings added to the sewage environment. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] Figure 1 The present invention is a process flow chart of a method for preparing ecological restoration materials from stone mine tailings. DETAILED DESCRIPTION

[0014] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0015] See also Figure 1 , the present invention provides a technical solution: Example 1 A method for preparing ecological restoration materials from stone mine tailings, comprising the following steps: S1: Mechanically grind the stone mine tailings and pass them through a 50-mesh sieve to obtain fine stone mine tailings; S2: reacting the fine stone mine tailings obtained in step S1 with a hydrochloric acid solution, with mechanical stirring during the reaction, and the concentration of the hydrochloric acid used is 2 mol / L, filtering to obtain a filter residue after the reaction is completed, and washing the filter residue with deionized water; S3: putting the filter residue obtained by washing in step S2 into a muffle furnace for calcination at a temperature of 900° C. for a calcination time of 5 h, reacting the calcined filter residue with a sodium hydroxide solution in a reactor, heating to 80° C. for a reaction time of 3 h, filtering out the filter residue to obtain a silicate solution; S4: After cooling the silicate solution obtained in step S3, a 1 mol / L hydrochloric acid solution is slowly added during stirring to adjust the pH of the solution to 6.2, and a precipitate is formed. The precipitate is filtered, washed with deionized water, and then vacuum dried. The obtained silica particles are ball-milled in a planetary ball mill to obtain nano-silicon dioxide with a particle size of 30 nm; S5: adding linear polystyrene to carbon tetrachloride, adding anhydrous aluminum chloride, stirring and heating to react for 3 hours, the heating temperature is 80°C, nitrogen is introduced into the solution during the reaction, and then deionized water and anhydrous ethanol are added to terminate the reaction, the mass ratio of linear polystyrene, carbon tetrachloride, anhydrous aluminum chloride, deionized water and anhydrous ethanol is 1:40:1:8:2, filtering the residue obtained by the reaction, washing it with ethanol and then vacuum drying it to obtain cross-linked polystyrene; S6: ultrasonically dispersing the cross-linked polystyrene obtained in step S5 into a mixed acid solution of concentrated sulfuric acid and concentrated nitric acid, stirring and reacting at 40° C. for 2.5 hours, wherein the concentration of the concentrated sulfuric acid is 98wt%, the concentration of the concentrated nitric acid is 60wt%, and the volume ratio of the concentrated sulfuric acid to the concentrated sulfuric acid is 1:2, and the residue obtained by filtering the solution after the reaction is washed with ethanol and dried to obtain activated porous cross-linked polystyrene; S7: Ultrasonic disperse the 20 g activated porous cross-linked polystyrene obtained in step S6 and the 28 g nano-silica obtained in step S4 into 400 g anhydrous ethanol, stir for 2 h, add 240 ml 0.1 mol / L EDTA aqueous solution, heat to 40°C and continue stirring for 3 h, filter the residue, wash with ethanol and vacuum dry to obtain the prepared ecological restoration material.

[0016] Example 2 A method for preparing ecological restoration materials from stone mine tailings, comprising the following steps: S1: Mechanically grind the stone mine tailings and pass them through a 50-mesh sieve to obtain fine stone mine tailings; S2: reacting the fine stone mine tailings obtained in step S1 with a hydrochloric acid solution, with mechanical stirring during the reaction, and the concentration of the hydrochloric acid used is 2 mol / L, filtering to obtain a filter residue after the reaction is completed, and washing the filter residue with deionized water; S3: putting the filter residue obtained by washing in step S2 into a muffle furnace for calcination at a temperature of 1100° C. for 3 hours, reacting the calcined filter residue with a sodium hydroxide solution in a reactor, heating the reaction to 95° C. for 2 hours, filtering out the filter residue to obtain a silicate solution; S4: After cooling the silicate solution obtained in step S3, a 1 mol / L hydrochloric acid solution is slowly added during stirring to adjust the pH of the solution to 7.2, and a precipitate is formed. The precipitate is filtered, washed with deionized water, and then vacuum-dried. The obtained silica particles are ball-milled in a planetary ball mill to obtain nano-silicon dioxide with a particle size of 60 nm; S5: adding linear polystyrene to carbon tetrachloride, adding anhydrous aluminum chloride, stirring and heating to react for 4 hours, the heating temperature is 50°C, nitrogen is introduced into the solution during the reaction, and then deionized water and anhydrous ethanol are added to terminate the reaction, the mass ratio of linear polystyrene, carbon tetrachloride, anhydrous aluminum chloride, deionized water and anhydrous ethanol is 1:140:10:60:10, filtering the residue obtained by the reaction, washing it with ethanol and then vacuum drying it to obtain cross-linked polystyrene; S6: ultrasonically dispersing the cross-linked polystyrene obtained in step S5 into a mixed acid solution of concentrated sulfuric acid and concentrated nitric acid, stirring and reacting at 60° C. for 1 h, wherein the concentration of the concentrated sulfuric acid is 98wt%, the concentration of the concentrated nitric acid is 60wt%, and the volume ratio of the concentrated sulfuric acid to the concentrated sulfuric acid is 1:2, and the residue obtained by filtering the solution after the reaction is washed with ethanol and dried to obtain activated porous cross-linked polystyrene; S7: Ultrasonic disperse the 20 g activated porous cross-linked polystyrene obtained in step S6 and the 34 g nano-silica obtained in step S4 into 800 g anhydrous ethanol, stir for 2 h, add 480 ml 0.1 mol / L EDTA aqueous solution, heat to 40-65°C and continue to react for 2-3 h, filter the residue, wash with ethanol and vacuum dry to obtain the prepared ecological restoration material.

[0017] Example 3 A method for preparing ecological restoration materials from stone mine tailings, comprising the following steps: S1: Mechanically grind the stone mine tailings and pass them through a 50-mesh sieve to obtain fine stone mine tailings; S2: reacting the fine stone mine tailings obtained in step S1 with a hydrochloric acid solution, with mechanical stirring during the reaction, and the concentration of the hydrochloric acid used is 2 mol / L, filtering to obtain a filter residue after the reaction is completed, and washing the filter residue with deionized water; S3: putting the filter residue obtained by washing in step S2 into a muffle furnace for calcination at a temperature of 1000° C. for a calcination time of 4.2 h, reacting the calcined filter residue with a sodium hydroxide solution in a reactor, heating to 90° C. during the reaction, and reacting for 2.6 h, filtering out the filter residue to obtain a silicate solution; S4: After cooling the silicate solution obtained in step S3, a hydrochloric acid solution with a concentration of 1 mol / L is slowly added during stirring to adjust the pH of the solution to 7, and a precipitate is formed. The precipitate is filtered, washed with deionized water, and then vacuum dried. The obtained silica particles are ball-milled in a planetary ball mill to obtain nano-silicon dioxide with a particle size of 50 nm; S5: adding linear polystyrene to carbon tetrachloride, adding anhydrous aluminum chloride, stirring and heating to react for 3.6 hours, the heating temperature is 70°C, nitrogen is introduced into the solution during the reaction, and then deionized water and anhydrous ethanol are added to terminate the reaction, the mass ratio of linear polystyrene, carbon tetrachloride, anhydrous aluminum chloride, deionized water and anhydrous ethanol is 1:100:8:35:8, filtering the residue obtained by the reaction, washing it with ethanol and then vacuum drying it to obtain cross-linked polystyrene; S6: ultrasonically dispersing the cross-linked polystyrene obtained in step S5 into a mixed acid solution of concentrated sulfuric acid and concentrated nitric acid, stirring and reacting at 50° C. for 2 h, wherein the concentration of the concentrated sulfuric acid is 98wt%, the concentration of the concentrated nitric acid is 60wt%, and the volume ratio of the concentrated sulfuric acid to the concentrated sulfuric acid is 1:2, and the residue obtained by filtering the solution after the reaction is washed with ethanol and dried to obtain activated porous cross-linked polystyrene; S7: Ultrasonic disperse the 20 g activated porous cross-linked polystyrene obtained in step S6 and the 30 g nano-silica obtained in step S4 into 600 g anhydrous ethanol, stir for 2 h, add 360 ml 0.1 mol / L EDTA aqueous solution, heat to 60°C and continue to react for 2.8 h, filter the residue, wash with ethanol and vacuum dry to obtain the prepared ecological restoration material.

[0018] Comparative Example 1 The difference between Comparative Example 1 and Example 1 is that step S6 is omitted, thereby canceling the cross-linking treatment of polystyrene, and the other steps are exactly the same as Example 1. The linear polystyrene in Comparative Example 1 is treated with concentrated nitric acid and concentrated sulfuric acid and then directly blended with nano-silicon dioxide and EDTA prepared from stone mine tailings.

[0019] Comparative Example 2 The difference between Comparative Example 2 and Example 1 is that step S7 is omitted, thereby eliminating the step of treating the cross-linked polystyrene with concentrated nitric acid and concentrated sulfuric acid. The other steps are exactly the same as those in Example 1. In Comparative Example 2, after cross-linking, the linear polystyrene is directly blended with nano-silicon dioxide and EDTA prepared from stone mine tailings.

[0020] Comparative Example 3 The difference between Comparative Example 3 and Example 1 is that both step S6 and step S7 are omitted, thereby canceling the crosslinking and concentrated acid treatment steps of the linear polystyrene, and the other steps are exactly the same as those in Example 1. The linear polystyrene in Comparative Example 3 is directly blended with nano-silicon dioxide and EDTA prepared from stone mine tailings.

[0021] Six ecological restoration materials were prepared through the above six implementation methods. Under laboratory environmental conditions, 100 mg / L of Pb 2+ Cr 2+ , Cu 2+ and Hg 2+ nitrate solution, each nitrate solution was prepared in six portions, each nitrate solution was 100 ml, the pH of the solution was adjusted to 7, the above nitrate solutions were mixed with the ecological restoration materials prepared in the above six embodiments, the ecological restoration materials added to each nitrate solution were 5 g, after reacting for 15 minutes, the remaining metal particle content in the nitrate solution was calculated, and the removal rate (R / %) was calculated. The results are shown in Table 1 below: Table 1: Heavy metal ion removal rate (R / %) <![CDATA[Pb 2+ ]]> <![CDATA[Cr 2+ ]]> <![CDATA[Cu 2+ ]]> <![CDATA[Hg 2+ ]]> Example 1 87.5 79.3 71.5 75.3 Example 2 91.2 82.1 72.8 76.4 Example 3 89.5 78.4 74.3 72.4 Comparative Example 1 79.3 65.4 56.2 60.8 Comparative Example 2 78.2 66.7 51.3 61.5 Comparative Example 3 69.8 59.8 41.1 50.7

[0022] As shown in Table 1 above, the ecological restoration material prepared by the present invention has a significant effect on the heavy metal Pb in water. 2+ Cr 2+ , Cu 2+ and Hg 2+ It has a very good removal effect, and the removal rate of the above four heavy metal ions can reach more than 70%. Some heavy metal ions such as Pb 2+ It can even reach a removal rate of more than 90%. When linear polystyrene is only treated with concentrated acid or cross-linked, the removal rate is significantly reduced. When there is no concentrated acid treatment or cross-linking treatment, the direct use of linear polystyrene and nano-silica blending further reduces the ability to treat heavy metal ions. Under laboratory environmental conditions, 100 mg / L phenol, o-hydroxybenzoic acid and p-nitroaniline solutions were prepared respectively, six portions of each nitrate solution were prepared, each portion of the nitrate solution was 100 ml, the pH of the solution was adjusted to 7, the above solutions were mixed with the ecological restoration materials prepared in the above six embodiments, 5 g of ecological restoration materials were added to each nitrate solution, and after 15 minutes of reaction, the residual content of phenol, o-hydroxybenzoic acid and p-nitroaniline in each solution was calculated, and the removal rate (R / %) was calculated. The results are shown in Table 2 below: Table 2: Organic matter removal rate (R / %)

[0023] It can be seen from Table 2 above that the ecological restoration material prepared by the embodiment of the present invention has a very good removal effect on the organic matter of phenol, o-hydroxybenzoic acid and p-nitroaniline in water, and the removal rate of the three organic matters is more than 80%. However, when the linear polystyrene is only treated with concentrated acid or only cross-linked, or is not treated with both, its adsorption capacity for organic matter shows a cliff-like decline.

[0024] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing ecological restoration materials from stone mine tailings, characterized in that: The following steps are involved: S1: Mechanically grind the stone mine tailings and pass them through a 50-mesh sieve to obtain fine stone mine tailings; S2: reacting the fine stone mine tailings obtained in step S1 with a hydrochloric acid solution, with mechanical stirring during the reaction, and the concentration of the hydrochloric acid used is 2 mol / L, filtering to obtain a filter residue after the reaction is completed, and washing the filter residue with deionized water; S3: putting the filter residue obtained by washing in step S2 into a muffle furnace for calcination, reacting the calcined filter residue with a sodium hydroxide solution in a reactor, heating to 80-95° C. during the reaction, the reaction time is 2-3 hours, filtering out the filter residue, and obtaining a silicate solution; S4: After cooling the silicate solution obtained in step S3, slowly add a 1 mol / L hydrochloric acid solution during stirring to adjust the pH of the solution to 6.2-7.2, a precipitate appears, the precipitate is filtered, washed with deionized water and then vacuum dried, and the obtained silica particles are ball-milled in a planetary ball mill to obtain nano-silicon dioxide; S5: adding linear polystyrene to carbon tetrachloride, adding anhydrous aluminum chloride, stirring and heating to react for 3-4 hours, the heating temperature is 50-80°C, nitrogen is introduced into the solution during the reaction, and then deionized water and anhydrous ethanol are added to terminate the reaction, filtering the residue obtained by the reaction, washing it with ethanol, and then vacuum drying it to obtain cross-linked polystyrene; S6: ultrasonically dispersing the cross-linked polystyrene obtained in step S5 into a mixed acid solution of concentrated sulfuric acid and concentrated nitric acid, stirring and reacting at 40-60° C. for 1-2.5 hours, filtering the solution after the reaction to obtain a filter residue, washing with ethanol, and drying to obtain activated porous cross-linked polystyrene; S7: Ultrasonic dispersion of the activated porous cross-linked polystyrene obtained in step S6 and the nano-silica obtained in step S4 into anhydrous ethanol, stirring for 2 hours, adding 0.1 mol / L EDTA aqueous solution, heating to 40-65°C, and continuing to stir and react for 2-3 hours, filtering to obtain the residue, washing with ethanol, and vacuum drying to obtain the prepared ecological restoration material.

2. The method for preparing ecological restoration materials from stone mine tailings according to claim 1, characterized in that: In step S3, the calcination temperature of the filter residue is 900-1100° C., and the calcination time of the filter residue in the muffle furnace is 3-5 hours.

3. The method for preparing ecological restoration materials from stone mine tailings according to claim 1, characterized in that: The particle size of the nano-silicon dioxide obtained by ball milling with a planetary ball mill in step S4 is 30-60 nm.

4. The method for preparing ecological restoration materials from stone mine tailings according to claim 1, characterized in that: In the step S5, the mass ratio of linear polystyrene, carbon tetrachloride, anhydrous aluminum chloride, deionized water and anhydrous ethanol is 1:(40-140):(1-10):(8-60):(2-10).

5. The method for preparing ecological restoration materials from stone mine tailings according to claim 1, characterized in that: In step S6, the concentration of concentrated sulfuric acid is 98wt%, the concentration of concentrated nitric acid is 60wt%, and the volume ratio of concentrated sulfuric acid to concentrated nitric acid is 1:

2.

6. The method for preparing ecological restoration materials from stone mine tailings according to claim 1, characterized in that: In step S7, the mass ratio of activated porous cross-linked polystyrene, nano-silica and anhydrous ethanol is 1:(1.4-1.7):(20-40), and the volume ratio of anhydrous ethanol to EDTA aqueous solution is 1:0.5.

Citation Information

Patent Citations

  • Material adsorbing heavy metal in water solution and method

    CN103157440A

  • Hydroximic acid functionalized polymer / inorganic composite chelating adsorption material and preparation method thereof

    CN103586001A

  • Porous crosslinked polystyrene microsphere and preparation method thereof

    CN104861102A

  • Method for preparing SiO2 / polystyrene composite porous material for oil-water separation

    CN110423298A

  • Method for preparing functionalized mesoporous nano-SiO2 material by using quartz sand tailings as raw material, and application of functionalized mesoporous nano-SiO2 material

    CN113800528A

Cited By

  • Method for improving lead-zinc tailings

    CN120515800A