Application of solid adsorption material to adsorption of metal elements
Modifying hydroxy iron pillared illite with fulvic acid solves the problem of insufficient adsorption performance of illite, achieves efficient removal of europium and americium, and provides an efficient and stable adsorption material for nuclear waste treatment.
Patent Information
- Application Number
- CN202410955306.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-10-01
AI Technical Summary
In the prior art, the adsorption performance of illite as a natural adsorbent is limited. Especially when the hydrophilicity is strong and the interlayer spacing is small, it is difficult to effectively adsorb radionuclides such as europium and americium, and there is a lack of modification research.
Fulvic acid-modified hydroxy-iron pillared illite (FA-Fe-illite) was prepared as a solid adsorption material by modifying hydroxy-iron pillared illite with fulvic acid. Its improved adsorption performance and structural characteristics can be used to efficiently adsorb europium and americium. .
It achieves highly selective removal of europium and americium, has a high adsorption rate, does not produce solid foreign matter such as mud, facilitates water separation and multiple recycling, and significantly improves the adsorption performance.
Smart Images

Figure CN118718985A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the fields of environmental protection and water treatment, and in particular to application of a solid adsorption material for adsorbing metal elements. Background Art
[0002] With the operation of nuclear reactors and the production and post-processing of nuclear fuel, radioactive nuclear waste and its derived pollutants inevitably pose a serious threat to the ecology. Radioactive nuclides, also known as unstable nuclides, directly endanger human health by spontaneously releasing invisible α, β and other rays. Therefore, how to safely handle and remove radioactive waste has become one of the key issues that need to be considered in the sustainable development of the nuclear industry.
[0003] Eu(III) is a trivalent rare earth element with a long half-life, strong activity and genetic toxicity. If the intake exceeds a certain value for a long time, it will inhibit the activity of human bone cells, thereby affecting the entire bone structure. When studying radioactive nuclides, Eu(III) is usually used as a simulated nuclide of the extremely radioactive and toxic Am(III) in experiments because its ionic radius and physical and chemical properties are similar to those of trivalent actinides.
[0004] So far, the technologies for removing europium mainly include membrane separation, solvent extraction, chemical precipitation, ion exchange and adsorption, etc. Among them, the adsorption method is widely used due to its high efficiency, environmental protection, simple operation and small amount of organic solvents.
[0005] Compared with adsorbents such as carbon materials and graphene, which are expensive, unstable and prone to secondary pollution, my country's clay minerals are not only abundant in reserves, cheap and easy to obtain, but also have special layered structures, large specific surface areas and rich porosity. They have strong adsorption, ion exchange capacity and expansion, and can adsorb metal ions through surface complexation, ion exchange adsorption and interlayer coordination. However, as a natural adsorbent, due to the limited adsorption performance of the original ore, it is generally necessary to undergo modified adsorption treatment.
[0006] Illite is a potassium-rich silicate mica clay mineral, named after the Erie Island in the United States where it was first discovered. Illite is a common clay mineral, often weathered by muscovite and potassium feldspar, and produced in argillaceous rocks, or formed by the alteration of other minerals. Illite is a new mineral species in my country. Illite mines were first discovered in Duchuantou Village, Shuangchao Township, Lucheng District, Wenzhou City, Zhejiang Province. Illite resources in Antu County, Jilin Province are very rich, with proven reserves of more than 140 million tons and prospective reserves of more than 200 million tons. It is a single super-large sandy illite deposit. Illite has excellent chemical and physical properties such as rich potassium, high aluminum, low iron, smooth, bright, delicate, and heat-resistant. Illite can freely release negative ions and far infrared rays. Illite has a wide range of uses. In the ceramic industry, illite is used as a raw material for the production of high-voltage electric porcelain and daily-use porcelain. In the chemical industry, it is used as a filler for papermaking, rubber, and paint. In agriculture, it is used to make potash fertilizers. Illite clay can be used as a flux for high-temperature resistant cylinders and to adsorb cesium in nuclear waste treatment to prevent radiation. Illite can also be used in high-end cosmetics, poultry feed additives, skeleton ingredients and cement ingredients for high-rise buildings, pollution purification and environmental protection in the nuclear industry. Illite is a TOT "sandwich" sandwich structure composed of double-layer silicon-oxygen tetrahedral sheets and single-layer aluminum-oxygen octahedral sheets. In addition to the common properties of clay minerals, it also has the characteristics of a large specific surface area; the good adsorption performance of illite is inseparable from its surface active sites and other related characteristics.
[0007] That is to say, there are existing technologies in the field for using illite or illite clay for nuclear waste treatment and pollution purification in the nuclear industry. However, illite or illite clay, as a natural adsorbent, has limited adsorption performance of the original ore, which undoubtedly limits its application. Specifically, illite, as a natural mineral, has strong hydrophilicity but poor polymer compatibility. The K+ between its layers is embedded in the sheets, resulting in a small interlayer spacing and low ion exchange capacity. Its (002) crystal plane spacing is also small, about This situation affects the adsorption performance of illite, so its modification becomes particularly important.
[0008] However, compared with well-known minerals such as montmorillonite and kaolin, there are fewer studies on the adsorption characteristics of illite in the prior art, and there is no research on the modification of illite.
[0009] Therefore, the art needs a modified illite material as a new solid adsorption material; it also needs to explore and study the preparation method of the new solid adsorption material; and it also needs to explore and study the application of the new solid adsorption material for adsorbing metal elements such as radioactive nuclides. Summary of the invention
[0010] Therefore, the present invention first provides an application of a solid adsorption material for adsorbing metal elements. The solid adsorption material is fulvic acid-modified hydroxy-iron pillared illite. The solid adsorption material is used for adsorbing the metal elements europium or americium.
[0011] In a specific embodiment, the initial concentration of europium or americium in water is above 0.5 mg / L, preferably 2 to 180 mg / L, more preferably 10 to 60 mg / L; and the amount of solid adsorption material used is 0.5 to 4 g / L, preferably 1 to 3 g / L, more preferably 1.2 to 1.6 g / L.
[0012] In a specific embodiment, the contact time between the solid adsorption material and the water containing europium or americium is more than 30 minutes, preferably more than 60 minutes.
[0013] In a specific embodiment, the adsorption reaction temperature of the solid adsorption material and the water containing europium or americium is above 10°C, preferably above 15°C, more preferably 20-40°C.
[0014] In a specific embodiment, the pH value of the water containing europium or americium is 5-9, preferably 6-8.
[0015] In a specific embodiment, after the adsorption is completed, the solid-liquid separation is performed first, and then the solid adsorption material is eluted with hydrochloric acid to obtain europium or americium, and the solid adsorption material is used for recycling.
[0016] In a specific embodiment, the method for preparing the solid adsorption material comprises the following steps:
[0017] Step A, first prepare a hydroxy iron pillaring liquid containing Fe(OH)3; and stir and dissolve illite powder in water to obtain an illite suspension, wherein the water is deionized water or ultrapure water;
[0018] Step B, heating the illite suspension to 45-80° C., and at this temperature, adding the hydroxy iron pillaring liquid dropwise to the illite suspension with stirring, stirring at a constant temperature for a period of time, then standing at the temperature for aging, cooling and solid-liquid separation, washing the obtained solid with water, and obtaining hydroxy iron pillared illite after drying, grinding and sieving;
[0019] Step C, adding the hydroxy-iron pillared illite and fulvic acid into an alkaline solution, reacting for a period of time under stirring and / or shaking conditions, washing the obtained solid with water after solid-liquid separation, and obtaining a solid adsorption material FA-Fe-illite, i.e. fulvic acid-modified hydroxy-iron pillared illite, after drying, grinding and sieving.
[0020] In a specific embodiment, in step A of the preparation method, Fe(NO3)3, water and sodium carbonate are first used to react to prepare the hydroxy iron pillared liquid containing Fe(OH)3, and the reaction temperature is 50-70°C. After stirring the reaction, it is allowed to stand and age at the same temperature for more than 12 hours, and the preferred aging time is more than 24 hours; and the weight ratio of water to illite powder used to form the illite suspension is 100:1-20, preferably 100:6-10; the stirring is magnetic stirring, and the stirring time is more than 30 minutes.
[0021] In a specific embodiment, in step B of the preparation method, the illite suspension is heated to 50-70°C, and after stirring the reaction at a constant temperature for 2-6 hours, it is allowed to stand and age for more than 12 hours; the solid-liquid separation is centrifugal separation, and the separated solid is washed with water for more than 3 times, and after drying and grinding, it is passed through a 200-400 mesh sieve to obtain the hydroxy-iron pillared illite.
[0022] In a specific embodiment, in step C of the preparation method, the fulvic acid is solid fulvic acid, and the mass ratio of the fulvic acid to the hydroxy-iron pillared illite powder is 1:0.5-30, preferably 1:1-15; the alkali solution is a NaOH solution, and the concentration of the NaOH solution is 0.01-1 mol / L, preferably 0.05-0.2 mol / L; and the mass ratio of the solid to the alkali solution is 1:50-200; the reaction is carried out under stirring and / or shaking conditions for more than 12 hours, and the reaction temperature is 10-45°C, preferably 20-35°C; the solid-liquid separation is centrifugal separation, the drying is drying the solid in a vacuum drying oven at 70-100°C, and the screening is passing through a 100-200 mesh sieve; and the prepared adsorbent FA-Fe-illite is stored in the dark.
[0023] The present invention also provides a method for preparing a solid adsorption material, comprising: step A, first preparing a hydroxy-iron pillaring liquid containing Fe(OH)3; and stirring and dissolving illite powder in water to obtain an illite suspension, wherein the water is deionized water or ultrapure water; step B, heating the illite suspension to 45-80°C, and at this temperature, stirring and dripping the hydroxy-iron pillaring liquid into the illite suspension, stirring for a period of time at a constant temperature, then standing and aging at the same temperature, cooling and solid-liquid separation, washing the obtained solid with water, and obtaining hydroxy-iron pillaring illite after drying, grinding and sieving; step C, adding the hydroxy-iron pillaring illite and fulvic acid into an alkaline solution, reacting for a period of time under stirring and / or shaking conditions, washing the obtained solid with water after solid-liquid separation, and obtaining a solid adsorption material FA-Fe-illite, i.e. fulvic acid-modified hydroxy-iron pillaring illite after drying, grinding and sieving.
[0024] The present invention also provides a solid adsorption material prepared by the preparation method as described above.
[0025] The present invention also provides an application of the solid adsorption material prepared by the preparation method described above for adsorbing radioactive nuclides in a water environment.
[0026] The beneficial effects of the present invention include: the solid adsorption material provided by the present invention is fulvic acid-modified hydroxy-iron pillared illite, which has high removal selectivity for europium and americium, and does not produce solid foreign matter such as mud during the adsorption reaction, so there is no need to use a foreign matter removal device, and the europium or americium separated from the water can be recovered by eluting with hydrochloric acid. The solid adsorption material of the present invention has good stability in the process of removing europium and americium from wastewater, and has a high adsorption rate for europium and americium. The fulvic acid-modified hydroxy-iron pillared illite provided by the present invention is a solid adsorbent, which can be easily separated from water and can be recycled many times. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0028] Figure 1 This is the SEM image of illite ore.
[0029] Figure 2 This is the SEM image of hydroxy-iron pillared illite (Fe-illite).
[0030] Figure 3 This is the SEM image of fulvic acid modified hydroxy-iron pillared illite (FA-Fe-illite).
[0031] Figure 4 This is the SEM image of fulvic acid modified hydroxy-iron pillared illite (FA-Fe-illite-Eu) adsorbed with Eu.
[0032] Figure 5 This is the EDS graph of FA-Fe-illite before adsorption of Eu(III).
[0033] Figure 6 This is the EDS graph of FA-Fe-illite after adsorbing Eu(III).
[0034] Figure 7 This is the BET chart for illite.
[0035] Figure 8 This is the BET diagram of Fe-illite.
[0036] Fig. 9 This is the BET diagram of FA-Fe-illite and its pore size distribution diagram.
[0037] Fig.10 FTIR spectra of illite, Fe-illite and FA-Fe-illite.
[0038] Fig.11 XRD patterns of illite, Fe-illite and FA-Fe-illite.
[0039] Fig.12 Comparison of the adsorption properties of illite, Fe-illite and FA-Fe-illite.
[0040] Fig.13 The effect of different ratios of FA to Fe-illite on the adsorption performance of the modified adsorbent.
[0041] Fig.14 Comparison of the adsorption performance of illite and FA-Fe-illite at different pH values.
[0042] Fig.15 Comparison of the adsorption performance of illite and FA-Fe-illite at different adsorbent dosages.
[0043] Fig.16 Comparison of the adsorption rates of illite and FA-Fe-illite at different adsorption times.
[0044] Fig.17 This is the pseudo-first-order kinetic model diagram of illite and FA-Fe-illite.
[0045] Fig.18 This is the pseudo-second-order kinetic model diagram of illite and FA-Fe-illite.
[0046] Fig.19 This is the internal diffusion kinetic model diagram of illite and FA-Fe-illite.
[0047] Fig. 20 Comparison of the adsorption rates of illite and FA-Fe-illite at different initial europium concentrations.
[0048] Fig.21 Langmuir adsorption isotherms of illite and FA-Fe-illite.
[0049] Fig. 22Freundlich adsorption isotherms of illite and FA-Fe-illite.
[0050] Fig.23 is the adsorption rate of illite and FA-Fe-illite at different temperatures.
[0051] Fig.24 These are the adsorption thermodynamic data of illite and FA-Fe-illite.
[0052] Fig.25 This is a comparison chart of the adsorption effects of recycled illite and FA-Fe-illite.
[0053] Fig.26 This is the XPS spectrum of the adsorbent FA-Fe-illite before and after the adsorption of europium, where the electron binding energy represented by the abscissa varies from 0 to 1200 eV.
[0054] Fig. 27 for Fig.26 A high-resolution XPS spectrum of the electron binding energy of the adsorbent FA-Fe-illite after adsorbing europium from 1130 to 1180 eV.
[0055] Fig.28 for Fig.26 A high-resolution XPS spectrum of the local magnification of O1S with an electron binding energy ranging from 526 to 542 eV before the adsorption of europium on the adsorbent FA-Fe-illite.
[0056] Fig.29 for Fig.26 High-resolution XPS spectrum of the local magnification of O1S of FA-Fe-illite-Eu(III) with the electron binding energy ranging from 526 to 542 eV after the adsorbent FA-Fe-illite adsorbs europium. DETAILED DESCRIPTION
[0057] The following will be combined with the accompanying drawings of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0058] Fulvic acid is a substance extracted from humus. It has a low molecular weight and a brown-black or brownish-brown appearance. It is soluble in acid, alkali, ethanol, and water. It is a complex of substances with similar molecular structures and behavioral characteristics. According to solubility, humic acid can be divided into three categories: humic acid (HA, also known as humic acid), palmitic acid (HyA), and fulvic acid (FA, also known as yellow humic acid). The part of humic acid that is insoluble in acid and alkali and insoluble in acetone is called humic acid, the part that is soluble in acetone or ethanol is called palmitic acid, and the part that is soluble in acid, alkali, ethanol, and water is called yellow humic acid (also known as fulvic acid).
[0059] Example 1
[0060] This example is a preparation method and characterization of the solid adsorption material FA-Fe-illite (fulvic acid modified hydroxy iron pillared illite) of the present invention.
[0061] 1. Preparation of iron-pillared illite. At room temperature, weigh 48.48g of Fe(NO3)3 solid and dissolve it in 500ml of deionized water and stir until it is completely dissolved. Then add 6.36g of anhydrous sodium carbonate powder to the solution and stir it continuously for 3h. The temperature is controlled at 60℃ and aged for 48h to obtain a reddish-brown hydroxy-iron pillared liquid. Among them, the Fe(NO3)3 solid reacts with water and anhydrous sodium carbonate to form Fe(OH)3 precipitate. 8 g of commercially available illite powder was added to 100 ml of deionized water, and the mixture was stirred continuously for 1 hour using a magnetic stirrer to prepare an illite suspension, which was heated to 60°C. The prepared hydroxy-iron pillared liquid was slowly added dropwise into the illite suspension while stirring. The mixture was stirred continuously for 4 hours at a constant temperature and then aged for 24 hours. The mixture was cooled to room temperature and centrifuged. The solid was washed at least 3 times with deionized water, dried in a vacuum drying oven at 85°C, and then the blocky solid was ground into powder and passed through a 200-mesh sieve to obtain dark yellow hydroxy-iron pillared illite.
[0062] 2. Preparation of FA-Fe-illite. Weigh a certain amount of hydroxy-iron pillared illite and put it in a 250ml conical flask, add different weights of brown fulvic acid solid, then add 0.1mol / L NaOH solution at a solid-liquid ratio of 1:100 to form a suspension, then shake at 30℃ and 250r / min for 24h, then cool, centrifuge, wash with water, and dry in a vacuum drying oven at 80℃. The obtained block solid (FA-Fe-Illite) is ground and passed through a 100-mesh sieve, and stored away from light for later use.
[0063] 3. The intermittent adsorption method was used to test the effects of illite and FA-Fe-illite on the adsorption performance of Eu(III). This experiment investigated the main factors affecting the adsorption performance, such as the amount of adsorbent (0.5-4 g·L -1), initial pH value (2-9), reaction time (0-210min), reaction temperature (283~313K) and other adsorption conditions were comprehensively investigated. In the adsorption experiment, 0.05g of adsorbent was added to a 30mL conical flask containing europium solution and oscillated in an air oscillator at 220rpm (25℃, 1h). The initial concentration of europium was 30mg / L. The pH value of the solution was adjusted with 1mol / L HNO3 and 1mol / L NaOH, and weak volume reaction was not considered. After saturated adsorption, a needle-type nylon membrane with a pore size of 0.22μm was used for solid-liquid separation. 1ml of filtrate, 1ml of azoarsine III and 3ml of acetic acid-sodium acetate buffer (pH=4) were added to the cuvette. Finally, the mixture was diluted to 10ml with water. After oscillation and standing for 5 minutes, the content of Eu(III) in the solution was determined using UV-Vis. Three parallel experiments were set up for each experiment to ensure the reliability of the results, and all pH values in the present invention were detected at adsorption equilibrium. e (mg·g -1 ) and removal rate R (%) can be calculated by the following formula:
[0064]
[0065]
[0066] In the formula, C0 (mg·L -1 ) and C e (mg·L -1 ) is the initial and equilibrium concentration of Eu(III) before and after adsorption, V (mL) represents the volume of the adsorption solution, and m (mg) represents the mass of the adsorbent. The removal rate R is also called the adsorption rate.
[0067] Example 2
[0068] Figure 1 to Figure 4 SEM images of the adsorbent before and after adsorption.
[0069] Figure 5-6 These are the EDS images before and after adsorption of the adsorbent.
[0070] in Figure 1 This is the SEM image of illite ore. Figure 2 This is the SEM image of hydroxy-iron pillared illite (Fe-illite). Figure 3 This is the SEM image of fulvic acid modified hydroxy-iron pillared illite (FA-Fe-illite). Figure 4 SEM image of fulvic acid-modified hydroxy-iron pillared illite (FA-Fe-illite-Eu(III)) adsorbed with Eu(III). Figure 5This is the EDS graph of FA-Fe-illite before adsorption of Eu(III). Figure 6 This is the EDS graph of FA-Fe-illite after adsorbing Eu(III).
[0071] like Figure 1 As shown in the figure, it can be seen that the illite ore has a clear layered structure and a smooth surface. Figure 2 As shown in Figure 2, after iron pillaring, the illite still has a flaky structure, but abundant pores appear on the surface and the roughness is enhanced, indicating that the pillaring is successful. Figure 3 As shown in the figure, the surface smoothness of FA-Fe-illite is greater than that of illite ore, indicating that FA molecules are successfully loaded onto illite, the pores are reduced, and because FA carries a large number of active functional groups such as -COOH and -NH2, it can affect the adsorption kinetics of europium. Figure 4 The adsorption of Eu(III) on FA-Fe-illite is shown.
[0072] pass Figure 5 and Figure 6 EDS analysis before and after the adsorbent FA-Fe-illite adsorbed Eu(III) showed that the adsorption peak of Eu(III) appeared, indicating that europium had been successfully captured by the adsorbent FA-Fe-illite.
[0073] Example 3
[0074] Figure 7 to Figure 9 It is the N2 adsorption-desorption isotherm (i.e. BET) and pore size distribution diagram of the adsorbent.
[0075] in, Figure 7 This is the BET chart for illite. Figure 8 This is the BET diagram of Fe-illite. Fig. 9 BET diagram and pore size distribution diagram of FA-Fe-illite.
[0076] from Figure 7 to Figure 9 It can be seen that the illite before and after modification belongs to the IV adsorption isotherm with H3 type hysteresis loop, with microporous and mesoporous structure. When the relative pressure is greater than 0.8, the adsorption amount obviously shows a sharp upward trend. According to the specific surface area and pore size analysis of illite before and after modification, compared with the original illite ore, the specific surface area of Fe-illite increases, and the small diameter pillaring agent molecules formed by the hydrolysis of iron salt enter the interlayer of illite to expand its pores, which is consistent with the above SEM characterization results. However, after FA modification, the specific surface area of FA-Fe-illite decreases, and the average pore size increases from 12.5770nm to 28.3975nm. This may be because the surface of the modified illite is loaded with a large number of various acidic oxygen-containing functional groups, thereby improving the adsorption performance of illite for europium.
[0077] Fig.10 FTIR spectra of illite, Fe-illite and FA-Fe-illite.
[0078] from Fig.10 It can be seen that by comparing the changes in the functional groups of illite and Fe-illite, it can be seen that the characteristic absorption peaks of illite before and after pillaring are basically the same, 3630.93cm -1 The sharp absorption peak at 1028.70 cm-1 belongs to the stretching vibration of the hydroxyl bond Al-OH in illite. -1 and 831.78cm -1 The bands at 3424.16 cm-1 are attributed to the in-plane stretching vibration of Si-O and the vibration peak of Si-O-Al. -1 and 1639.05cm -1 The observed absorption peaks correspond to the stretching vibration and bending vibration absorption peaks of HOH in water molecules. The FTIR spectrum of FA-Fe-illite has a peak at 1383.83 cm -1 A new characteristic peak is formed at 1385 cm-1, which is the vibration absorption peak of COOH and CH=O, which is consistent with the absorption peak of FA at 1385 cm-1. -1 The absorption peaks of the modified adsorbents are corresponding to the stretching vibrations of hydroxyl CO and aliphatic CH, indicating that a large number of 3+ The polar groups such as carboxyl groups that underwent complexation and FA-Fe-illite did not produce new absorption peaks at other wave numbers indicated that the loading mode of FA molecules on illite was mainly electrostatic adsorption, which was beneficial to the removal of Eu(III).
[0079] Fig.11 XRD patterns of illite, Fe-illite and FA-Fe-illite.
[0080] from Fig.11 It can be seen that the molecular crystal form of illite before and after modification has not changed significantly, and the original structure has not been destroyed. However, after iron pillaring, the position of the "001" diffraction peak of illite shifted from 8.93° to 6.73°, and then changed to 8.34° after FA modification.
[0081] According to the following Bragg equation:
[0082] 2dsinθ=nλ (3)
[0083] Where d is the spacing between the planes, θ is the diffraction angle between the incident and reflected X-rays, n represents the order of reflection, and λ represents the wavelength of the X-rays (λ=0.15418 nm).
[0084] After calculation, the interlayer spacing of illite, Fe-illite and FA-Fe-illite is 0.99nm, 1.38nm and 1.07nm respectively, indicating that Fe successfully enters the illite interlayer to replace the cations, thus increasing the interlayer spacing. In addition, the reduction in the interlayer spacing of FA-Fe-illite may be due to the fact that FA molecules occupy part of the interlayer of Fe-illite, which is consistent with the Figures 7 to 9 The conclusion corresponding to the BET diagram is consistent with that of the adsorbent, that is, after loading FA molecules, the specific surface area of the adsorbent decreases and the average pore size becomes larger.
[0085] Fig.12 Comparison of the adsorption properties of illite, Fe-illite and FA-Fe-illite. Fig.13 The effect of different ratios of FA to Fe-illite on the adsorption performance of the modified adsorbent.
[0086] Fig.12 In the experiment, 0.05 g illite ore, iron-pillared illite and FA-Fe-illite were added to 30 mL of 30 mg / L europium solution, respectively. After shaking at 25 °C for 60 min, the results were as follows: Fig.12 As shown. It can be seen that the adsorption effect of FA-Fe-illite is much higher than the previous two, so FA-Fe-illite is used as the adsorbent in the following. Fig.13 It can be seen that the experiment prepared modified illite according to different fulvic acid mass ratios to adsorb Eu(III). Compared with the illite ore on the far left, the adsorption effect of the five FA-modified illites with different mass ratios was significantly enhanced. When the mass ratio is 1:1, the removal rate of Eu(III) by FA-Fe-illite can reach 80.13%, and the adsorption amount is 17.15 mg / g. This may be because the modifier fulvic acid can act on illite through ion exchange, hydrogen bonding and van der Waals force, resulting in an increase in the amount of negative charge and adsorption sites on its surface, and its own skeleton structure and a large number of functional groups on the edge can promote the adsorption of Eu. 3+ The electrostatic adsorption and complexation of illite increased the removal rate of Eu(III). Therefore, the mass ratio of FA to Fe-illite was selected as 1:1 for the subsequent modification of the adsorbent.
[0087] Fig.14 Comparison of the adsorption performance of illite and FA-Fe-illite at different pH values. Fig.15 Comparison of the adsorption performance of illite and FA-Fe-illite at different adsorbent dosages.
[0088] from Fig.14It can be seen that the adsorption performance of FA-Fe-illite for Eu(III) is significantly higher than that of illite, and the removal rate increases with the increase of pH value. After adsorption equilibrium, the removal rate of FA-Fe-illite for Eu(III) is increased by about 40% compared with illite. When the pH value is low, there is a large amount of H + 、H3O + With Eu 3+ Compete for surface adsorption sites, and at the same time protonate the active groups carboxyl and amino groups, which hinder the adsorption of Eu(III) due to repulsion. As the pH value increases, the active groups are deprotonated, and the negative charge on the surface of FA-Fe-illite is strengthened, thereby increasing the ion exchange and surface complexation with Eu(III). In addition, when the pH value is higher than 7, the OH- concentration in the solution increases, and Eu(III) begins to precipitate in the form of Eu(OH)3, which is prone to secondary pollution. Therefore, in order to obtain the best removal effect, it is more appropriate to choose pH=7 in subsequent experiments.
[0089] Fig.15 The effects of two adsorbent materials, illite and FA-Fe-illite, on removing Eu(III) were investigated. The results show that in the range of 0.5-4.0 g / L of adsorbent, the removal rate of Eu(III) increases with the increase of dosage. When the dosage is 1.2 g / L, the europium removal rates of illite and FA-Fe-illite are 45.23% and 86.04%, respectively, and then tend to be stable. This may be due to the fact that when the dosage increases initially, there are more adsorption sites available. When equilibrium is reached, the adsorbent surface is blocked and cannot be fully utilized. In addition, excessive use of adsorbent will cause difficulties in solid-liquid separation after the adsorption. Therefore, 1.2 g / L is selected as the optimal dosage for the experiment.
[0090] Fig.16 is the adsorption rate of illite and FA-Fe-illite at different adsorption times.
[0091] Fig.16 In order to clarify the effect of contact time on europium adsorption, 0.05g of adsorbent was weighed to explore the removal variation in 30ml of solution containing 30mg / L europium. Fig.16 As shown in the figure, the adsorption rates of illite and FA-Fe-illite increase with time, showing a rapid growth trend within 30 minutes, and then slowly rising until the adsorption equilibrium is reached after 60 minutes. The adsorption removal rate basically does not change. This may be related to the presence of a large number of active sites on the surface of the adsorbent in the early stage, and as time goes on, the adsorption capacity gradually tends to saturation.
[0092] Figure 17 to Figure 19is the adsorption kinetics diagram of illite and FA-Fe-illite. Fig.17 This is the pseudo-first-order kinetic model diagram of illite and FA-Fe-illite. Fig.18 This is the pseudo-second-order kinetic model diagram of illite and FA-Fe-illite. Fig.19 This is the internal diffusion kinetic model diagram of illite and FA-Fe-illite.
[0093] Adsorption kinetics is an important characteristic of the adsorbent, which can reflect the adsorption rate and adsorption capacity of the adsorbent. The pseudo-first-order, pseudo-second-order and internal diffusion kinetic models were used to fit the kinetic equations of illite and FA-Fe-illite adsorption of Eu(III). The three kinetic model equations are as follows:
[0094] Ln(q e -q t )=Lnq e -k1t(4)
[0095]
[0096] q t =k d t 0.5 +C (6)
[0097] In the formula, k1(min -1 ) and k2(g·mg -1 ·min -1 ) are the adsorption rate constants of pseudo-first-order and pseudo-second-order kinetic equations, respectively, and q t and q e are the adsorption capacity of Eu(III) at time t and at adsorption equilibrium, respectively, and k d (mg·g -1 ·min -1 / 2 ) is the diffusion rate constant of the intraparticle diffusion, and C represents a constant related to the thickness and boundary layer.
[0098] Figure 17 to Figure 19 The linear fitting results of the above three models for Eu(III) adsorption are shown in Figure 2. The results show that the pseudo-first-order fitting coefficients R 2 are 0.969 and 0.835 respectively, and the quasi-second-order fitting coefficient R 2 are 0.998 and 0.999, respectively, which indicates that the adsorption of Eu(III) by illite and FA-Fe-illite is more consistent with the pseudo-second-order kinetic model, and the q e The value is very close to the experimentally measured q eValue (illite is 11.27 mg / g, FA-Fe-illite is 19.09 mg / g). In addition, according to Fig.19 The fitting results of the intra-particle diffusion kinetic model shown in the figure show that the fitting straight line does not coincide with the origin, indicating that internal diffusion is not the only factor controlling adsorption, which indicates that the adsorption of europium by illite and FA-Fe-illite is mainly controlled by chemical adsorption.
[0099] Fig. 20 The adsorption rates of illite and FA-Fe-illite at different initial europium concentrations. Figure 21-22 is the adsorption isotherm of illite and FA-Fe-illite. Fig.21 Langmuir adsorption isotherms of illite and FA-Fe-illite. Fig. 22 Freundlich adsorption isotherms of illite and FA-Fe-illite.
[0100] The adsorption equilibrium mechanism of illite and FA-Fe-illite at different initial europium concentrations was clarified. The Langmuir and Freundlich isothermal adsorption models were used to simulate the adsorption process of Eu(III) on illite and FA-Fe-illite. The initial europium concentration (10-210 mg·L -1 ) is used as a benchmark for adsorption experiments. The Langmuir isotherm model is reversible adsorption, the adsorbent surface is relatively uniform and the adsorption is monolayer adsorption, and one site can only accommodate one adsorbate. The Freundlich isotherm model is often used for multilayer adsorption. This model mainly describes the surface adsorption behavior of surfaces with uneven surfaces or interactions after surface adsorption of particles. The equations of the two models are shown below:
[0101]
[0102] In the formula, C e (mg·L -1 ) is the concentration of Eu(III) at equilibrium, q e is the adsorption capacity of Eu(III) at adsorption equilibrium, q m (mg·g -1 ) is the maximum adsorption capacity, K L is the Langmuir constant related to the heat of adsorption, K F is the Freundlich constant related to the adsorption capacity, and 1 / n is the Freundlich constant related to the adsorption intensity. The linear fitting results of the Langmuir isotherm model and the Freundlich isotherm model are shown in Fig.21 and Fig. 22 .
[0103] like Fig. 20As shown in the figure, the removal rates of illite and FA-Fe-illite for Eu(III) decrease with the increase of initial europium concentration. Fig.21 and Fig. 22 It can be seen that the Langmuir coefficients of illite and FA-Fe-illite for Eu(III) adsorption are 0.992 and 0.981, respectively, and the FreundLich coefficients are 0.971 and 0.988, respectively. In comparison, the Langmuir adsorption isotherm of illite has a better fitting effect, while the FreundLich coefficient of FA-Fe-illite is higher than the Langmuir coefficient, and its FreundLich adsorption isotherm has a better fitting effect, and the calculated q m Value (20.14 mg g -1 ) is very close to the experimentally measured q m Value (19.09 mg g -1 ), indicating that the adsorption of Eu(III) by illite is mainly monolayer adsorption, while that by FA-Fe-illite is mainly multilayer adsorption, which can be attributed to the fact that functional groups such as carboxyl groups loaded on the surface of FA-Fe-illite can chelate and coordinate with europium ions. Moreover, the FreundLich model fitting parameter of FA-Fe-illite is 1 / n<1 (between 0 and 1), indicating that the adsorption of europium by FA-Fe-illite is spontaneous.
[0104] Fig.23 is the adsorption rate of illite and FA-Fe-illite at different temperatures. Fig.24 These are the adsorption thermodynamic data of illite and FA-Fe-illite.
[0105] like Fig.23 As shown in the figure, when the temperature is 283-313K, as the temperature increases, the removal rate of Eu(III) by illite and FA-Fe-illite gradually increases, and the thermodynamic parameters ΔH, ΔS and ΔG are calculated by the following formula:
[0106] K d =q e / C e (9)
[0107] LqCy d =-ΔH 0 / R+ΔS 0 / R (10)
[0108] ΔG 0 =ΔH 0 - TΔS 0 (11)
[0109] In the formula, Kd is the adsorption distribution coefficient, q e is the adsorption capacity of Eu(III) at adsorption equilibrium, Ce is the equilibrium concentration of Eu(III) (mg·L -1 ), T is the adsorption temperature (K), R is the ideal gas constant (8.314 J·mol -1 ·K -1 ), thermodynamic parameter ΔH 0 (kJ·mol -1 ), ΔS 0 (J.mol -1 ·K -1 ) and ΔG 0 (kJ·mol -1 ) represent the changes in enthalpy, entropy and Gibbs free energy, respectively.
[0110] lnK after adsorption of Eu(III) on illite and FA-Fe-illite d The linear relationship between and 1 / T is as follows Fig.24 The enthalpy change ΔH reflects the endothermic nature of the adsorption process. The values of ΔH for illite and FA-Fe-illite to Eu(III) are 28.261 and 38.829 kJ / mol, respectively, indicating that the adsorption reaction is an endothermic process, which is consistent with the experimental results. The entropy change ΔS reflects the degree of disorder in the adsorption process. The ΔS in the process of illite and FA-Fe-illite adsorbing Eu(III) is 28.261 and 38.829 kJ / mol, respectively. 0 >0, indicating that the adsorption of the two is an entropy increase process, and the adsorption system moves in the direction of increasing disorder; Gibbs free energy reflects the spontaneity of the adsorption process, where ΔG 0 All of them are negative values, indicating that the adsorption of Eu(III) by illite and FA-Fe-illite can occur spontaneously at different temperatures, and increasing the temperature is conducive to their contact with Eu(III).
[0111] Fig.25 This is a comparison chart of the adsorption effects of recycled illite and FA-Fe-illite.
[0112] For the practical application of adsorbents, the recovery of adsorbents is crucial. In order to explore the stability of illite and FA-Fe-illite in adsorbing Eu(III), the present invention selected 0.1 mol / L HCl to elute and adsorb the adsorbed illite and FA-Fe-illite respectively, and repeated the adsorption steps several times after drying to compare the adsorption effect after elution. The results are shown in Figure 2. Fig.25As shown, hydrochloric acid has excellent desorption capacity for both illite and FA-Fe-illite. Although the removal rate of Eu(III) has a downward trend after 5 adsorption-desorption cycles, it can still reach about 75% of the original removal rate. This shows that the modified illite adsorbent provided by the present invention has good recycling performance. During the recycling process, the reason why the adsorbent's removal rate of europium is reduced may be that with the increase in the number of elutions, the minerals on the surface of the adsorbent are inevitably lost, which leads to a reduction in adsorption sites. In addition, the hydrochloric acid desorption may also change the related structure of the adsorbent material to a certain extent, causing the adsorption capacity of the adsorbent to decrease.
[0113] Figures 26 to 29 This is the XPS spectrum of the adsorbent FA-Fe-illite before and after the adsorption of europium. Fig.26 This is the XPS spectrum of the adsorbent FA-Fe-illite before and after the adsorption of europium, where the electron binding energy represented by the abscissa varies from 0 to 1200 eV. Fig. 27 for Fig.26 The locally enlarged XPS spectrum of the electron binding energy from 1130 to 1180 eV after the adsorbent FA-Fe-illite adsorbs europium. Fig.28 for Fig.26 Locally enlarged high-resolution XPS spectrum of O1S with electron binding energy ranging from 526 to 542 eV before adsorption of europium on the adsorbent FA-Fe-illite. Fig.29 for Fig.26 Locally enlarged high-resolution XPS spectrum of O1S of FA-Fe-illite-Eu(III) with the electron binding energy ranging from 526 to 542 eV after the adsorbent FA-Fe-illite adsorbs europium.
[0114] like Fig.26 As shown in Figure 2, after the adsorption of Eu(III), the material showed an obvious Eu 3d peak, indicating that europium was successfully adsorbed by the adsorbent FA-Fe-illite. Fig. 27 As shown, the high Eu 3d deconvolution after FA-Fe-illite adsorption was separated into two components (Eu 3d5 / 2 and Eu 3d3 / 2), which also indicated that europium was captured on the adsorbent.
[0115] like Fig.28 As shown in Figure 1, the 1s orbital of the O element can be divided into four peaks, corresponding to COOH at 533.16 eV, -OH at 532.23 eV, C=O at 531.68 eV, and COC at 531.07 eV. Fig.29It can be seen that after the adsorbent adsorbs Eu(III), the four peaks move to 533.78eV, 531.86eV, 531.13eV and 530.24eV respectively. Obviously, the peaks of COOH and COC become flat and the peak area decreases after the adsorption of europium. The electrons of carbon atoms are transferred to the single-bonded oxygen atoms of the carboxyl group, providing electrons for the single-bonded oxygen complexed metal atoms of the carboxyl group. At the same time, the relative area of OH increases, indicating that they participate in the removal of Eu(III) to a certain extent. Based on the above research, it can be found that the adsorption of Eu(III) by FA-Fe-illite is mainly controlled by oxygen-containing functional groups such as -OH and COOH, and a strong coordination chelation reaction is carried out with them, thereby achieving stable adsorption.
[0116] It will be easily understood by those skilled in the art that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. Application of a solid adsorption material for adsorbing metal elements, It is characterized in that The solid adsorption material is fulvic acid-modified hydroxy-iron pillared illite, and the solid adsorption material is used for adsorbing metal elements europium or americium.
2. The use according to claim 1, It is characterized in that The initial concentration of europium or americium in water is above 0.5 mg / L, preferably 2-180 mg / L, more preferably 10-60 mg / L; and the amount of solid adsorption material used is 0.5-4 g / L, preferably 1-3 g / L, more preferably 1.2-1.6 g / L.
3. The use according to claim 1, It is characterized in that The contact time between the solid adsorption material and the water containing europium or americium is more than 30 minutes, preferably more than 60 minutes.
4. The use according to claim 1, It is characterized in that The adsorption reaction temperature of the solid adsorption material and water containing europium or americium is above 10°C, preferably above 15°C, more preferably 20-40°C.
5. The use according to claim 1, It is characterized in that The pH value of the water containing europium or americium is 5-9, preferably 6-8.
6. The use according to claim 1, It is characterized in that After the adsorption is completed, the solid and liquid are separated first, and then the solid adsorption material is eluted with hydrochloric acid to obtain europium or americium, and the solid adsorption material is used for recycling.
7. The use according to claim 1, It is characterized in that The preparation method of the solid adsorption material comprises the following steps: Step A: First prepare Fe(OH) 3 The illite powder is stirred and dissolved in water to obtain an illite suspension, wherein the water is deionized water or ultrapure water; Step B, heating the illite suspension to 45-80° C., and at this temperature, adding the hydroxy iron pillaring liquid dropwise to the illite suspension with stirring, stirring at a constant temperature for a period of time, then standing at the temperature for aging, cooling and solid-liquid separation, washing the obtained solid with water, and obtaining hydroxy iron pillared illite after drying, grinding and sieving; Step C, adding the hydroxy-iron pillared illite and fulvic acid into an alkaline solution, reacting for a period of time under stirring and / or shaking conditions, washing the obtained solid with water after solid-liquid separation, and obtaining a solid adsorption material FA-Fe-illite, i.e. fulvic acid-modified hydroxy-iron pillared illite, after drying, grinding and sieving.
8. The use according to claim 7, It is characterized in that In step A of the preparation method, Fe(NO 3 ) 3 , water and sodium carbonate to prepare the Fe(OH) 3 The hydroxy-iron pillaring liquid is prepared by the step of stirring the reaction at a temperature of 50 to 70°C, and the mixture is allowed to stand for aging at the same temperature for more than 12 hours, preferably for more than 24 hours; and the weight ratio of water to illite powder used to form the illite suspension is 100:1 to 20, preferably 100:6 to 10; and the stirring is magnetic stirring, and the stirring time is more than 30 minutes.
9. The use according to claim 7, It is characterized in that In step B of the preparation method, the illite suspension is heated to 50-70°C, and after stirring the reaction at a constant temperature for 2-6 hours, it is allowed to stand and age for more than 12 hours; the solid-liquid separation is centrifugal separation, and the separated solid is washed with water for more than 3 times, and after drying and grinding, it is passed through a 200-400 mesh sieve to obtain the hydroxy-iron pillared illite.
10. The use according to claim 7, It is characterized in that In step C of the preparation method, the fulvic acid is solid fulvic acid, and the mass ratio of the fulvic acid to the hydroxy-iron pillared illite powder is 1:0.5-30, preferably 1:1-15; the alkali solution is a NaOH solution, and the concentration of the NaOH solution is 0.01-1 mol / L, preferably 0.05-0.2 mol / L; and the mass ratio of the solid to the alkali solution is 1:50-200; the reaction is carried out under stirring and / or shaking conditions for more than 12 hours, and the reaction temperature is 10-45°C, preferably 20-35°C; the solid-liquid separation is centrifugal separation, the drying is drying the solid in a vacuum drying oven at 70-100°C, and the screening is passing through a 100-200 mesh sieve; and the prepared adsorbent FA-Fe-illite is stored in the dark.
Citation Information
Patent Citations
Europium adsorbent based on cyclodextrin polycarboxylic acid polymer and application method of adsorbent
CN112934202A