Shell powder adsorbent as well as preparation method and application thereof
By mixing and calcining shell powder with inorganic salts of magnesium, stanninite and dixonite with high adsorption capacity are formed. Combined with the coating agent, the problem of shell powder's limited adsorption capacity for nitrogen and phosphorus is solved and the problem is achieved. It provides efficient nitrogen and phosphorus removal and is suitable for treating eutrophic water bodies.
Patent Information
- Application Number
- CN202410916030.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-09
- Publication Date
- 2024-10-01
AI Technical Summary
Existing shell powder has limited adsorption capacity for nitrogen and phosphorus, and cannot simultaneously remove nitrogen and phosphorus, which limits its application in the treatment of eutrophic water bodies.
Shell powder is mixed with inorganic salts of magnesium (such as magnesium chloride, magnesium oxide, and magnesium carbonate) and calcined at high temperatures to form precipitates such as stanninite and diphosphonite, which increase the adsorption capacity and combine bentonite and silicon. Sodium acid acid is used as a coating agent to improve the adsorption effect.
It achieves high-efficiency adsorption of nitrogen and phosphorus, improves the adsorption capacity of shell powder, is suitable for the treatment of eutrophic water bodies, and reduces preparation costs and operation complexity.
Smart Images

Figure CN118719008A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of water purification, and in particular to a shell powder adsorbent and a preparation method and application thereof. Background Art
[0002] Eutrophication refers to the phenomenon of excessive accumulation of nutrients (such as nitrogen and phosphorus) in water or soil. It is mainly caused by human activities, including chemical emissions, wastewater discharge, pesticide and fertilizer use in agriculture, industry and urbanization. After these nutrients enter the water or soil, they will accelerate the growth of plants and plankton, causing the balance of the ecosystem to be broken. At present, the main treatment method is to suppress eutrophication by double recovery of nitrogen and phosphorus. In particular, phosphorus is a non-renewable resource, which will disappear in 100 years according to statistics. Therefore, recovering phosphorus from sewage is still a top priority for maintaining global economic development.
[0003] Shells are a daily consumable for people because they are rich in protein, but this also produces a large amount of shell waste, causing environmental pollution. Therefore, many applications of shells have been developed. It is reported that shell powder can remove 99% of low-concentration phosphates in water, but the nitrogen removal rate is unsatisfactory. There are many reports on adsorption materials for simultaneous denitrification and phosphorus removal, but the preparation of the above-mentioned denitrification and phosphorus removal materials is complex and their adsorption capacity for nitrogen and phosphorus is limited.
[0004] In summary, there is an urgent need for a shell powder with high adsorption capacity and the ability to remove nitrogen and phosphorus at the same time, which can be used for the treatment of eutrophic water bodies. Summary of the invention
[0005] The main purpose of the present invention is to propose a shell powder adsorbent and its preparation method and application, aiming to solve the problem that the existing shell powder has limited nitrogen and phosphorus adsorption capacity and cannot remove nitrogen and phosphorus at the same time, which limits the application of shell powder.
[0006] To achieve the above objectives, the present invention provides a shell powder adsorbent, which comprises shell powder and an inorganic salt of magnesium.
[0007] Optionally, the inorganic salt of magnesium includes at least one of magnesium chloride, magnesium oxide and magnesium carbonate.
[0008] Optionally, the mass ratio of the shell powder to the inorganic salt of magnesium is 1:(0.6-1.2).
[0009] Optionally, the shell powder adsorbent further includes a coating agent, and the coating agent includes bentonite and sodium silicate.
[0010] The present invention also provides a method for preparing a shell powder adsorbent, comprising the following steps: S10, providing shell powder;
[0011] S20. Mix and grind the shell powder and the inorganic salt of magnesium, and then calcine them under the protection of an inert gas to obtain a shell powder adsorbent.
[0012] Optionally, in the steps of washing, drying, crushing and sieving shells of shellfish to obtain shell powder: the drying temperature is 50-70° C.; and / or the drying time is 5 hours.
[0013] Optionally, in the steps of washing, drying, crushing and sieving the shells of shellfish to obtain shell powder, the mesh number of the sieving sieve is 30 to 50 meshes.
[0014] Optionally, in step S20, the grinding method includes ball milling:
[0015] The ball mill has a rotation speed of 500 to 700 rpm; and / or,
[0016] The ball milling time is 1.5 to 2.5 hours.
[0017] Optionally, in step S20, the calcination temperature is 700-900° C.; and / or the calcination time is 1.5-2.5 h.
[0018] The present invention also provides a dephosphorization and denitrification agent, comprising any of the shell powder adsorbents described above, or a shell powder adsorbent prepared by the preparation method of any of the shell powder adsorbents described above.
[0019] The present invention proposes a shell powder adsorbent, which uses shell powder as one of the raw materials. The shell powder has a relatively high calcium content and is therefore better in absorbing phosphorus. After being mixed with an inorganic salt of magnesium, it reacts with nitrogen and phosphorus in water to form struvite and diphosphate magnesium ammonium ammonium and is accompanied by the precipitation of struvite. This allows the shell powder adsorbent to absorb nitrogen as well as phosphorus, and can be used in the control of eutrophication of water bodies. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying creative work.
[0021] Figure 1 This is an XPS graph of the shell powder adsorbent prepared in one embodiment of the present invention after adsorbing nitrogen and phosphorus.
[0022] The realization of the purpose, functional features and advantages of the present invention will be further explained in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION
[0023] To make the purpose, technical scheme and advantages of the embodiment of the present invention clearer, the technical scheme in the embodiment of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiment, it is carried out according to the normal conditions or the conditions recommended by the manufacturer. If the reagents or instruments used do not specify the manufacturer, they are all conventional products that can be purchased commercially. In addition, the meaning of "and / or" appearing in the full text includes three parallel schemes, taking "A and / or B" as an example, including scheme A, or scheme B, or schemes that A and B meet at the same time. In addition, the technical schemes between the various embodiments can be combined with each other, but must be based on the ability of ordinary technicians in the field to achieve. When the combination of technical solutions is contradictory or cannot be achieved, it should be considered that the combination of such technical solutions does not exist, and is not within the scope of protection required by the present invention. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work belong to the scope of protection of the present invention.
[0024] Shells are a daily consumable for people because they are rich in protein, but this also produces a large amount of shell waste, causing environmental pollution. Therefore, many applications of shells have been developed. It is reported that shell powder can remove 99% of low-concentration phosphates in water, but the nitrogen removal rate is unsatisfactory. There are many reports on adsorption materials for simultaneous denitrification and phosphorus removal, but the preparation of the above-mentioned denitrification and phosphorus removal materials is complex and their adsorption capacity for nitrogen and phosphorus is limited.
[0025] In view of this, the present invention provides a shell powder adsorbent and a preparation method and application thereof, which can improve the shell powder adsorbent's effect of adsorbing nitrogen and phosphorus at the same time and can be applied to the treatment of water eutrophication.
[0026] In an embodiment of the present invention, the shell powder adsorbent includes shell powder and an inorganic salt of magnesium.
[0027] In the technical solution of the present invention, shell powder is used as one of the raw materials. The calcium content of shell powder is relatively high, so it has a better effect on adsorbing phosphorus. After mixing with inorganic salts of magnesium, the shell powder adsorbent can adsorb nitrogen while adsorbing phosphorus, and can be used in the control of eutrophication of water bodies.
[0028] Furthermore, the inorganic salt of magnesium includes at least one of magnesium chloride, magnesium oxide and magnesium carbonate, that is, the inorganic salt of magnesium can be one of magnesium chloride, magnesium oxide and magnesium carbonate, or a combination of any two, or a combination of three. In the present invention, there can be many inorganic salts of magnesium, as long as they can be dehydrated at high temperature to form magnesium oxide. Magnesium oxide and calcium oxide at high temperature react with nitrogen and phosphorus in water to produce struvite, diphosphate magnesium ammonium ammonium and struvite. In particular, the formation of struvite helps to improve the dephosphorization and denitrification effect of the shell powder adsorbent. Magnesium chloride, magnesium oxide and magnesium carbonate have low costs.
[0029] Furthermore, the mass ratio of the shell powder and the inorganic salt of magnesium is 1:(0.6-1.2). It can be understood that, for example, it is 1:0.6, 1:0.8, 1:1, 1:1.2, etc. The mass ratio of the shell powder and the inorganic salt of magnesium is within the above range. In actual production, 1:1 is preferred. Shell powder has the best effect in treating high nitrogen and high phosphorus.
[0030] Furthermore, the shell powder adsorbent also includes a coating agent, and the coating agent includes bentonite and sodium silicate. Preferably, the mass ratio of the bentonite to the sodium silicate is 1:2. Within this range, the coating effect is better.
[0031] It should be noted here that bentonite and sodium silicate are mixed to form a polymer solution, which can be subsequently mixed with shell powder to prepare microspheres coated with inorganic salts of magnesium, which have a sustained release effect and are more effective in adsorbing nitrogen and phosphorus in water bodies.
[0032] Specifically, the preparation process includes: first, stirring and dissolving bentonite and sodium silicate in a water bath, cooling to room temperature to obtain a polymer solution, then adding shell powder to mix to obtain microspheres, and then mixing with an inorganic salt of magnesium, coating the inorganic salt of magnesium, grinding and calcining to obtain a shell powder adsorbent.
[0033] The present invention also provides another method for preparing a shell powder adsorbent, comprising the following steps:
[0034] S10, providing shell powder;
[0035] S20. Mix and grind the shell powder and the inorganic salt of magnesium, and then calcine them under the protection of an inert gas to obtain a shell powder adsorbent.
[0036] Specifically, the operating steps of this embodiment are: put the shell powder into a grinding machine, mix it with an inorganic salt of magnesium, and calcine it at high temperature under oxygen-isolated conditions. After calcination, cool the sample to room temperature, take it out and put it into a sealed container.
[0037] The preparation method is simple, easy to operate, and has low production cost. The grinding method is adopted to make the calcium ions and magnesium ions better and more evenly mixed together. At the same time, the shell powder is mixed with the magnesium source and then calcined at a high temperature to modify it to obtain modified shell powder. In the calcination process, the calcium carbonate in the shell powder is converted into calcium oxide, and the inorganic salt of magnesium is converted into magnesium oxide, which can increase the specific surface area of the shell powder and make it have stronger adsorption capacity. The modified shell powder not only has the ability to adsorb phosphorus, but also has the ability to adsorb nitrogen. In the process of water treatment, it can react with nitrogen and phosphorus in the water, thereby forming struvite, diphosphate magnesium ammonium stone and struvite precipitation, and further improve the adsorption capacity for nitrogen and phosphorus.
[0038] When there is Ca in the wastewater 2+ / Mg 2+ NH4 + and PO4 3- When the concentration product of the above three ions is greater than the solubility product constant Ksp, struvite will spontaneously form and precipitate, thereby achieving NH4 + and PO4 3- Remove at the same time, the reaction formula is:
[0039] Ca 2+ +NH4 + +PO4 3- +H2O→(NH4)2Ca(PO3OH)2.H2O↓
[0040] Mg 2+ +NH4 + +PO4 3- +6H2O→NH4MgPO4.H2O↓
[0041] Mg 2+ +NH4 + +PO4 3- +6H2O→MgNH4PO4.6H2O↓.
[0042] Furthermore, before step S10, the process also includes: washing, drying, crushing and sieving the shells of the shellfish to obtain shell powder.
[0043] It should be noted that there are many options for shellfish, such as clams, scallops, clams, etc. They only need to have a relatively high calcium content and be easily available. They can be prepared by yourself or purchased on the market. In this embodiment, clams are preferred, and shell powder that has been ground and processed has a better effect.
[0044] Specifically, the operating steps of step S10 are: first, clean the shells with deionized water, and put them into a blast drying oven to dry; then, put the dried shells into a high-speed grinder to crush them, and after crushing, grind them through a mortar until they pass through a sieve to prepare shell powder.
[0045] Further, in the step of washing, drying, crushing and sieving the shells of the shellfish to obtain shell powder:
[0046] The drying temperature is 50-70°C and the drying time is 5 hours. Within this temperature range and time range, the drying effect is best. Drying the cleaned shells also facilitates subsequent processing of the shells.
[0047] It can be understood that the above-mentioned restrictions on reaction temperature and reaction time can be satisfied by both or only one of them. In a preferred embodiment of the present invention, the above-mentioned two conditions are satisfied at the same time, so that the drying effect is better.
[0048] Furthermore, in the steps of washing, drying, crushing and sieving the shells of shellfish to obtain shell powder, the mesh size of the sieve is 30 to 50 meshes, for example, it can be 30 meshes, 40 meshes or 50 meshes, etc. Within these mesh size ranges, the shell powder adsorbent of the present invention is better integrated with the subsequent magnesium inorganic salt, and the final dephosphorization and denitrification effect is better.
[0049] Furthermore, in step S20, the grinding method includes ball milling: the rotation speed of the ball mill is 500-700 rpm, and the time of the ball milling is 1.5-2.5 hours.
[0050] It should be noted that there are many ways to grind. The method used here is to put it in a ball mill jar and use a planetary ball mill, which has a better ball milling effect. The ball mill speed can be 500rpm, 600rpm or 700rpm, and the ball milling time is 1.5h, 2h or 2.5h. Among them, the preferred speed is 600rpm, maintained for 2h, which can make the calcium ions and magnesium ions better and more evenly mixed together.
[0051] Furthermore, in step S20, the calcination temperature is 700-900° C.; and / or the calcination time is 1.5-2.5 h.
[0052] It should be noted that the calcination temperature can be 700°C, 800°C or 900°C, and the calcination time can be 1.5h, 2h or 2.5h. In practice, the preferred calcination temperature is 800°C. At this temperature, the best effect is achieved when calcined for 2h. Within this temperature and time range, the calcium carbonate in the shell powder is converted into calcium oxide, and the inorganic salt of magnesium is converted into magnesium oxide, which can increase the specific surface area of the modified shell powder and make it have a stronger adsorption capacity. When the modified shell powder adsorbs nitrogen and phosphorus elements in water, it will form struvite (NH4MgPO4·6H20) precipitation, so that the adsorbent of the present invention has the ability to adsorb not only phosphorus but also nitrogen, and the adsorption capacity is greatly improved.
[0053] It can be understood that the above-mentioned limitations on the reaction calcination temperature and the calcination reaction time can be met at the same time, or only one of them can be met. In a preferred embodiment of the present invention, the above-mentioned two conditions are met at the same time, so that the obtained shell powder has a better adsorption effect.
[0054] The present invention also proposes a dephosphorization and denitrification agent, including any of the above-mentioned shell powder adsorbents, or a shell powder adsorbent prepared by the preparation method of any of the above-mentioned shell powder adsorbents. Therefore, it also has all the beneficial effects brought by the above-mentioned technical solutions, which will not be repeated here one by one.
[0055] The technical solution of the present invention is further described in detail below in conjunction with specific embodiments and drawings. It should be understood that the following embodiments are only used to explain the present invention and are not used to limit the present invention.
[0056] Example 1
[0057] A shell powder adsorbent comprises clam powder and magnesium chloride, wherein the mass ratio of the clam powder to the magnesium chloride is 1:2.
[0058] Example 2
[0059] A shell powder adsorbent comprises scallop powder and magnesium oxide, wherein the mass ratio of the scallop powder to the magnesium oxide is 1:0.6.
[0060] Example 3
[0061] A shell powder adsorbent comprises clam powder and magnesium carbonate, wherein the mass ratio of the clam powder to the magnesium carbonate is 1:1.
[0062] Example 4
[0063] A shell powder adsorbent comprises shell powder and an inorganic salt of magnesium, wherein the mass ratio of the shell powder to the inorganic salt of magnesium is 1:1.2.
[0064] Example 5
[0065] A method for preparing a shell powder adsorbent comprises the following steps:
[0066] S10, washing the clam shells with deionized water and drying them in a forced air drying oven at 60° C.;
[0067] S20, crushing the dried clam shells, grinding them with a mortar until they pass through a 40-mesh sieve, and preparing sieve-filtered shell powder;
[0068] S30, mixing the shell powder filtered through the sieve with magnesium chloride in a mass ratio of 1:1 to obtain a mixture, wherein each portion is 1 g;
[0069] S40, placing the mixture into a ball milling jar, and ball milling the mixture in a planetary ball mill at a rate of 600 rpm for 2 h to obtain ball-milled shell powder.
[0070] S50. The ball-milled shell powder was placed in a muffle furnace. In the absence of oxygen, it was heated to 800°C at a rate of 10°C / min and kept at 800°C for 2h. After heating, the sample was cooled to room temperature, taken out and placed in a sealed container to obtain shell powder. Its properties were tested and the results are shown in Table 1.
[0071] Example 6
[0072] A method for preparing a shell powder adsorbent comprises the following steps:
[0073] S10, washing the clam shells with deionized water and drying them in a blast drying oven at 50° C.;
[0074] S20, crushing the dried clam shells, grinding them with a mortar until they pass through a 50-mesh sieve, and preparing sieve-filtered shell powder;
[0075] S30, mixing the shell powder filtered through the sieve with magnesium chloride in a mass ratio of 1:1.2 to obtain a mixture, wherein each portion is 1 g;
[0076] S40, placing the mixture into a ball milling jar, and ball milling the mixture in a planetary ball mill at a rate of 500 rpm for 2 h to obtain ball-milled shell powder.
[0077] S50. The ball-milled shell powder was placed in a muffle furnace. In the absence of oxygen, it was heated to 700°C at a rate of 10°C / min and kept at 700°C for 2.5 hours. After the heating was completed, the sample was cooled to room temperature, taken out and placed in a sealed container to obtain shell powder. Its various properties were tested and the results are shown in Table 1.
[0078] Example 7
[0079] A method for preparing a shell powder adsorbent comprises the following steps:
[0080] S10, washing the clam shells with deionized water and drying them in a forced air drying oven at 70° C.;
[0081] S20, crushing the dried clam shells, grinding them with a mortar until they pass through a 30-mesh sieve, and preparing sieve-filtered shell powder;
[0082] S30, mixing the shell powder filtered through the sieve with magnesium chloride in a mass ratio of 1:0.6 to obtain a mixture, wherein each portion is 1 g;
[0083] S40, placing the mixture into a ball milling jar, and ball milling the mixture in a planetary ball mill at a rate of 700 rpm for 2 h to obtain ball-milled shell powder.
[0084] S50. Put the ball-milled shell powder into a muffle furnace, and heat it to 900°C at a rate of 10°C / min under the condition of isolating oxygen, and keep it at 900°C for 1.5 hours. After the heating is completed, cool the sample to room temperature, take it out and put it into a sealed container to obtain shell powder. Test its various properties and get the results shown in Table 1.
[0085] Example 8
[0086] Step S50 is omitted. Except for not performing sintering, other steps are the same as those in Example 5. Various properties are tested, and the results are shown in Table 1.
[0087] Example 9
[0088] Steps S40 and S50 are omitted. Except for not performing sintering and grinding, other steps are the same as those in Example 5. Various properties are tested, and the results are shown in Table 1.
[0089] Example 10
[0090] Step S40 is omitted. Except for not grinding, other steps are the same as those in Example 5. Various properties are tested, and the results are shown in Table 1.
[0091] Embodiment 11
[0092] Add a coating agent, wherein the step of adding the coating agent is: the mass ratio of the bentonite and sodium silicate is 1:2, stirring and dissolving, cooling to room temperature to obtain a polymer solution, and then mixing with shell powder and magnesium chloride in a mass ratio of 1:0.6 to obtain a mixture. The other steps are the same as in Example 5. The various properties are tested and the results are shown in Table 1.
[0093] Comparative Example 1
[0094] A shell powder adsorbent, comprising only shell powder.
[0095] Comparative Example 2
[0096] A shell powder adsorbent comprising only magnesium chloride.
[0097] Performance Testing
[0098] 1) The shell powder adsorbent prepared in Example 5 was analyzed by X-ray photoelectron spectroscopy after adsorbing nitrogen and phosphorus. The results are as follows: Figure 1 As shown: it shows that the shell powder adsorbent prepared by the present invention will generate three substances, namely, struvite, diphosphate magnesium ammonium and struvite precipitation, after adsorbing nitrogen and phosphorus.
[0099] 2) The shell powder adsorbent prepared in Examples 5 to 10 and the shell powder adsorbent prepared in Comparative Examples 1 to 2 were respectively placed in a glass bottle containing 50 ml of 100 mg / L NH4Cl or 100 mg / L KH2PO4 solution and a glass bottle containing a mixed solution of 50 ml of 100 mg / L NH4Cl and 100 mg / L KH2PO4, wherein the solution of 50 ml 100 mg / L NH4Cl and 100 mg / L KH2PO4 simulates the concentrations of nitrogen and phosphorus in water. After sealing, they were placed in a desktop constant temperature oscillator and oscillated continuously for 16 hours. The test was carried out at a temperature of 30°C and a speed of 180 rpm / min. The test results are shown in Table 1, wherein the phosphorus content test adopted the method specified in the national standard GB11893-89, and the ammonia nitrogen content was determined by the method specified in the national standard HJ 535-2009.
[0100] Continue to adjust the ratio of nitrogen and phosphorus in the water body, set three concentrations, respectively, in Example 5
[0101] Concentration 1: 50ml 100mg / L NH4Cl and 1g / L KH2PO4 solution in a glass bottle for simulation experiment,
[0102] Concentration 2: Simulation experiment in a glass bottle with 50ml 1g / L NH4Cl and 100mg / L KH2PO4 solution,
[0103] Concentration 3: Simulation experiment in a glass bottle with 50 ml of 1 g / L NH4Cl and 1 g / L KH2PO4 solution. The experimental results correspond to Table 2.
[0104] Table 1 Determination of the performance of shell powder adsorbents for adsorption of nitrogen and phosphorus in Examples 5 to 10 and Comparative Examples 1 to 2
[0105]
[0106] It can be seen from Table 1 that compared with Examples 5 to 7, Example 8 lacks the calcination step, and the resulting shell powder adsorbent has greatly reduced adsorption capacity for nitrogen and phosphorus compared with Examples 5 to 7. This shows that calcination can improve its adsorption capacity, indicating that calcination can not only make the shell powder produce calcium oxide at high temperature, but also make the inorganic salt of magnesium produce magnesium oxide. The mixture of the two generates struvite, diphosphate magnesium ammonium stone and struvite after adsorption of nitrogen and phosphorus, so that the adsorption amount of nitrogen and phosphorus reaches the highest.
[0107] Compared with Examples 5 to 7, Example 9 only crushes the shell powder and performs preliminary treatment without calcination and grinding. However, compared with Example 8, grinding is added. Therefore, the adsorption effect is better than that of Example 8, but worse than that of Examples 5 to 7. This shows that the calcination and ball milling processes can further make the shell powder finer and more uniform, activate the active substances in the shell powder, and further improve the adsorption capacity of the shell powder.
[0108] Compared with Examples 5 to 7, Example 10 only calcined the shell powder but did not go through the grinding process. The effect was poor compared with Examples 5 to 7. This shows that after grinding, the shell powder particles can be made more uniform and have a larger specific surface area, thereby enhancing the ability of the shell powder to adsorb nitrogen and phosphorus.
[0109] Compared with Examples 5 to 7, after adding the coating agent in Example 11, shell powder can be added and mixed to prepare microspheres, which are coated with inorganic salts of magnesium and can achieve a sustained-release adsorption effect, thereby enhancing the ability of the shell powder to adsorb nitrogen and phosphorus.
[0110] Compared with Comparative Examples 1 and 2, the effects of Examples 5 to 7 are better than those of the Comparative Examples, indicating that the addition of inorganic salts of magnesium can greatly improve the adsorption capacity of nitrogen and phosphorus in water.
[0111] Table 2 Performance test of shell powder corresponding to Example 5 for simultaneous adsorbent of nitrogen and phosphorus in water with different concentrations
[0112] Nitrogen adsorption (mg / g) Phosphorus adsorption (mg / g) Water concentration 1 52.01 632.77 Water concentration 2 433.14 98.89 Water concentration 3 416.52 620.35
[0113] It can be seen from Table 2 that, faced with water bodies with high concentrations of nitrogen and phosphorus, the shell powder adsorbent prepared in this embodiment still has a high adsorption capacity.
[0114] The above are only preferred embodiments of the present invention, and do not limit the patent scope of the present invention. For those skilled in the art, the present invention may have various changes and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the patent protection scope of the present invention.
Claims
1. A shell powder adsorbent, characterized in that: The shell powder adsorbent comprises shell powder and an inorganic salt of magnesium.
2. The shell powder adsorbent according to claim 1, characterized in that: The inorganic salt of magnesium includes at least one of magnesium chloride, magnesium oxide and magnesium carbonate.
3. The shell powder adsorbent according to claim 1, characterized in that: The mass ratio of the shell powder to the inorganic salt of magnesium is 1:(0.6-1.2).
4. The shell powder adsorbent according to claim 1, characterized in that: The shell powder adsorbent also includes a coating agent, and the coating agent includes polybentonite and sodium silicate.
5. A method for preparing a shell powder adsorbent according to any one of claims 1 to 4, characterized in that: The following steps are involved: S10, providing shell powder; S20. Mix and grind the shell powder and the inorganic salt of magnesium, and then calcine them under the protection of an inert gas to obtain a shell powder adsorbent.
6. The method for preparing the shell powder adsorbent according to claim 5, characterized in that: The steps of washing, drying, crushing and sieving shells of shellfish to obtain shell powder: The drying temperature is 50-70°C; and / or, The drying time is 5h.
7. The method for preparing the shell powder adsorbent according to claim 5, characterized in that: In the step of washing, drying, crushing and sieving the shells of shellfish to obtain shell powder, The mesh number of the sieve is 30 to 50 meshes.
8. The method for preparing the shell powder adsorbent according to claim 4, characterized in that: In step S20, the grinding method includes ball milling: The ball mill has a rotation speed of 500 to 700 rpm; and / or, The ball milling time is 1.5 to 2.5 hours.
9. The method for preparing the shell powder adsorbent according to claim 4, characterized in that: In step S20, the calcination temperature is 700-900° C.; and / or, The calcination time is 1.5 to 2.5 hours.
10. A dephosphorization and denitrification agent, characterized in that: It includes the shell powder adsorbent as described in any one of claims 1 to 3, or a shell powder adsorbent prepared by the preparation method of the shell powder adsorbent as described in any one of claims 4 to 9.
Citation Information
Cited By
Fruit sunscreen additive as well as preparation method and application thereof
CN118725741A