Soft foam type lithium ion sieve composite adsorbent as well as preparation method and application thereof

By preparing a soft foam type lithium ion sieve composite adsorbent, the problems of high processing cost and slow adsorption rate of lithium ion sieve adsorbent in the liquid lithium extraction process are solved, and efficient and stable lithium ion adsorption effect is achieved, which is suitable for industrial applications. .

CN118719013APending Publication Date: 2024-10-01CENT SOUTH UNIV
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410762272.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-13
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing lithium ion screen adsorbents have problems in the process of liquid lithium extraction, such as high efficiency filtration and high processing costs, reduced adsorption effect caused by powder agglomeration, poor dispersion and slow adsorption rate, and traditional molding methods cannot meet industrial needs.

Method used

The preparation method of soft foam lithium ion sieve composite adsorbent is adopted, through the combination of organic matter such as hydroxyethyl cellulose, N, N-methylene bisacrylamide and Li4Ti5O12 powder, and through stirring, ultrasound, freezing gel and acid Washing treatment to form a soft foam adsorbent with high adsorption capacity and fast adsorption rate.

Benefits of technology

It achieves high adsorption capacity, fast adsorption rate and stability. The adsorbent reaches equilibrium within 1.5 hours, and the lithium ion adsorption capacity remains 97.8% after 8 cycles, which reduces production costs and simplifies the operating process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118719013A_ABST
    Figure CN118719013A_ABST
Patent Text Reader

Abstract

The invention provides a soft foam type lithium ion sieve composite adsorbent and a preparation method and application thereof.The method comprises the steps that an organic matter A and an organic matter B are taken and dissolved in deionized water, and an organic matter solution is obtained; adding Li4Ti5O12 (LTO) powder, stirring for multiple times, and carrying out ultrasonic treatment, so as to obtain an LTO-loaded adsorbent precursor solution; dropwise adding an initiator and a catalyst to obtain a mixed solution; injecting into a mold, freezing and drying to obtain LTO frozen gel; carrying out acid pickling treatment; the foam type composite adsorbent prepared by the invention has excellent hydrophilicity, is loose, porous and elastic, can increase the fluidity during lithium extraction and reduce loss, and has higher adsorption capacity and higher adsorption rate; the method can also be directly and industrially applied to salt lake brine, seawater, geothermal water, waste lithium battery leaching liquid and the like, and when the method is applied to lithium extraction of liquid lithium resources, adsorption equilibrium can be achieved only in 1-1.5 h. The method is easy to realize continuous industrial production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of separation and purification, and in particular to a soft foam type lithium ion sieve composite adsorbent and a preparation method and application thereof. Background Art

[0002] Lithium, known as "the important metal that drives the world", is widely used in various fields such as energy batteries, aerospace, nuclear power, and pharmaceuticals. With the rapid development of lithium-ion battery and electric vehicle industries, the demand for lithium continues to increase. However, traditional lithium extraction methods can no longer meet the requirements of cost reduction and energy saving, environmental protection, efficiency, and the increasing demand for lithium resources. The adsorption method is considered to be the most promising method for extracting lithium from liquid lithium resources due to its advantages of low energy consumption, high cost-effectiveness, and good environmental benefits.

[0003] At present, most adsorbents are powdered adsorbents. In the process of lithium extraction from liquid, the following defects make it difficult to apply them in practice. First, separating powdered adsorbents from liquids usually requires efficient filtration or centrifugal equipment, which increases processing costs and complexity. Secondly, powders are prone to agglomeration and accumulation, which will affect their effective specific surface area and thus reduce the actual adsorption effect. In addition, powdered adsorbents have poor dispersibility in liquid media, which will lead to a decrease in the lithium ion mass transfer rate, a slower adsorption process, and affect the overall lithium extraction efficiency. Therefore, the development of molding technology with commercial application value is of great significance to the future development of lithium resources.

[0004] The existing patent CN101955210B uses acrylic acid monomers to reversely suspend and polymerize to form a cross-linked polymer, and then the lithium ion sieve powder is coated in the polymer to obtain a granular lithium ion sieve. However, when it is used for lithium extraction from a mixed solution, the Li + The equilibrium adsorption capacity is only 6.8 mg g -1, the performance needs to be improved urgently. This is because the increase in mass transfer resistance during granulation, poor hydrophilicity of the binder and clogging of the adsorption sites cause a significant loss of adsorption capacity. At present, the foaming method is used to form the powder to improve the above problems. Foam-type adsorbents have many unique functions and advantages. First, the adsorbent is embedded in the foam system to obtain a foam-type adsorbent, which has high mechanical strength and stability, making it easier to handle and recycle in the liquid phase system, simplifying the operating process and equipment requirements. At the same time, it also solves the problem of easy agglomeration and accumulation between powders, and improves the adsorption rate and efficiency. In addition, the foam-type adsorbent has a good fluid channel, which reduces the risk of clogging during the adsorption process. At the same time, it has good water absorption, which is conducive to the diffusion of lithium-containing solutions into the expanded foam-type adsorbent, thereby promoting full contact between the solution and the adsorbent, and solving the problem of poor dispersibility of powder adsorbents in liquid media. Finally, the foam-type adsorbent also has a high total porosity, surface area and lithium ion sieve loading. For example, CN108046368 A discloses a lithium ion sieve filler loaded with open-cell foam glass using nano-titanium dioxide as a binder, but its adsorption rate is slow and it takes 6 hours to reach adsorption equilibrium, and its performance still needs to be improved.

[0005] Therefore, there is an urgent need to develop a new foam-type lithium ion sieve composite adsorbent with high adsorption capacity and fast adsorption rate in this field to meet the needs of continuous production in industry. Summary of the invention

[0006] The present invention provides a soft foam type lithium ion sieve composite adsorbent and a preparation method and application thereof, the purpose of which is to solve the above-mentioned problems existing in the background technology.

[0007] In order to achieve the above-mentioned purpose, the embodiments of the present invention provide a soft foam type lithium ion sieve composite adsorbent and a preparation method and application thereof. The soft foam type lithium ion sieve composite adsorbent can be directly industrially applied to lithium-containing solutions such as salt lake brine, seawater, geothermal water, and waste lithium battery leaching solution. The soft foam type lithium ion sieve composite adsorbent has the advantages of good hydrophilicity, less adsorption capacity than powdered lithium ion sieve adsorbent, simple operation, low cost, and easy industrial application.

[0008] An object of an embodiment of the present invention is to provide a method for preparing a soft foam type lithium ion sieve composite adsorbent, comprising the following steps:

[0009] S1: dissolving organic matter A and organic matter B in deionized water to obtain an organic solution;

[0010] S2: Take Li4Ti5O 12 The powder is added to the organic solution at a certain temperature, and subjected to multiple stirring and ultrasonic treatment to obtain a loaded LTO adsorbent precursor solution;

[0011] S3: adding an initiator and a catalyst dropwise to the LTO-loaded adsorbent precursor solution to obtain a mixed solution;

[0012] S4: injecting the mixed solution into a mold, freezing and drying to obtain LTO cryogel;

[0013] S5: The LTO cryogel is subjected to an acid washing treatment to obtain HTO cryogel.

[0014] According to one aspect of an embodiment of the present invention, in step S1, the organic substance A is any one of hydroxyethyl cellulose, resorcinol, and polyvinyl alcohol, and the added amount is 0.75 to 1.75 g; the organic substance B is any one of N,N-methylenebisacrylamide, urea formaldehyde, and glutaraldehyde, and the added amount is 0.75 to 1.75 g.

[0015] According to one aspect of the embodiment of the present invention, the content of LTO loaded in step S2 is 10% to 90%.

[0016] According to one aspect of an embodiment of the present invention, in step S2, the temperature is 0-10° C.; the stirring time is 10 min / time, at least 3 times; and the ultrasonic time is 10 min / time, at least 3 times.

[0017] According to one aspect of an embodiment of the present invention, in step S3, the initiator is any one of ammonium persulfate, hydrogen peroxide, and azobisisobutyronitrile, and the concentration is 3 to 13 wt.%; the catalyst is any one of N,N,N′,N′-tetramethylethylenediamine, N,N,N′,N′-tetraethylethylenediamine, and N,N,N′,N′-tetramethyl-1,3-propylenediamine, and the concentration is 1 to 7 wt.%.

[0018] According to one aspect of an embodiment of the present invention, the freezing time of step S4 is 4 to 8 hours; the drying temperature is -20°C, and the drying time is 12 to 24 hours.

[0019] According to one aspect of the embodiment of the present invention, the pickling time in step S5 is 5 hours, and the acid used is hydrochloric acid with a concentration of 0.05 to 0.5 mol / L. The different concentrations of hydrochloric acid are 0.05, 0.1, 0.2, 0.3, 0.4, and 0.5 mol / L.

[0020] Based on a general concept of the invention, an embodiment of the present invention provides a soft foam-type lithium ion sieve composite adsorbent obtained by the above-mentioned preparation method.

[0021] Another object of an embodiment of the present invention is to provide a lithium-extracting agent for lithium-containing solutions, including a soft foam-type lithium ion sieve composite adsorbent obtained by the above-mentioned preparation method.

[0022] According to one aspect of an embodiment of the present invention, the lithium-containing solution includes at least one of salt lake brine, seawater, geothermal water, and waste lithium battery leaching solution.

[0023] The above scheme of the present invention has the following beneficial effects:

[0024] (1) The structure of the soft foam lithium ion sieve adsorbent of the present invention is superior. It can be easily adsorbed and recycled through the "immersion and extrusion" mechanism. It is also lighter in weight and more convenient in transportation, handling and use. Compared with granular adsorbents, it has higher economy, sustainability and industrial application potential.

[0025] (2) The soft foam lithium ion sieve adsorbent of the present invention has better stability (compared with the granular lithium ion sieve of CN101955210B in the prior art, when used for lithium extraction from mixed solution, Li + The adsorption capacity was from 28.4 mg·g -1 Reduced to 6.8 mg g -1 , while the adsorbent of the present invention is almost unaffected), and a higher adsorption capacity (28.1 mg·g -1 ) and extremely fast adsorption rate, it only takes 1.5 hours to reach adsorption equilibrium, greatly shortening the adsorption time. After 8 cycles, the adsorption capacity of the soft foam lithium ion sieve adsorbent remains at 97.8% of the initial value, and it is reusable.

[0026] (3) The concentration of hydrochloric acid used in the pickling process of the preparation method of the present invention is small. The concentration of hydrochloric acid used in the present invention is much lower than 1 mol / L in CN101955210B, which is beneficial to saving production costs. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0028] Figure 1 This is a physical picture of the durability test process of the soft foam type lithium ion sieve composite adsorbent prepared in Example 1 of the present invention;

[0029] Figure 2 is a scanning electron microscope image of the soft foam type lithium ion sieve composite adsorbent of Example 1 of the present invention;

[0030] Figure 3 is a curve showing the adsorption capacity of the soft foam type lithium ion sieve composite adsorbent of Example 1 of the present invention changing with time;

[0031] Figure 4 This is a test diagram of the cycle performance of the soft foam type lithium ion sieve composite adsorbent of Example 1 of the present invention;

[0032] Figure 5 The soft foam type lithium ion sieve composite adsorbent of Example 1 of the present invention is respectively for Li + Mg 2+ 、Na + , K + , Ca 2+ The adsorption amount. DETAILED DESCRIPTION

[0033] In order to make the technical problems, technical solutions and advantages to be solved by the present invention more clear, a detailed description will be given below with reference to the accompanying drawings and specific embodiments.

[0034] Unless otherwise defined, all professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.

[0035] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.

[0036] In view of the existing problems, the present invention provides a method for preparing a soft foam type lithium ion sieve composite adsorbent, comprising the following steps:

[0037] S1: dissolving organic matter A and organic matter B in deionized water to obtain an organic solution;

[0038] S2: Take Li4Ti5O 12 The powder is added to the organic solution at a certain temperature, and subjected to multiple stirring and ultrasonic treatment to obtain a loaded LTO adsorbent precursor solution;

[0039] S3: adding an initiator and a catalyst dropwise to the LTO-loaded adsorbent precursor solution to obtain a mixed solution;

[0040] S4: injecting the mixed solution into a mold, freezing and drying to obtain LTO cryogel;

[0041] S5: The LTO cryogel is subjected to an acid washing treatment to obtain HTO cryogel.

[0042] According to one aspect of an embodiment of the present invention, in step S1, the organic substance A is any one of hydroxyethyl cellulose, resorcinol, and polyvinyl alcohol, and the added amount is 0.75 to 1.75 g; the organic substance B is any one of N,N-methylenebisacrylamide, urea formaldehyde, and glutaraldehyde, and the added amount is 0.75 to 1.75 g.

[0043] According to one aspect of the embodiment of the present invention, the content of LTO loaded in step S2 is 10% to 90%.

[0044] According to one aspect of an embodiment of the present invention, in step S2, the temperature is 0-10° C.; the stirring time is 10 min / time, at least 3 times; and the ultrasonic time is 10 min / time, at least 3 times.

[0045] According to one aspect of an embodiment of the present invention, in step S3, the initiator is any one of ammonium persulfate, hydrogen peroxide, and azobisisobutyronitrile, and the concentration is 3 to 13 wt.%; the catalyst is any one of N,N,N′,N′-tetramethylethylenediamine, N,N,N′,N′-tetraethylethylenediamine, and N,N,N′,N′-tetramethyl-1,3-propylenediamine, and the concentration is 1 to 7 wt.%.

[0046] According to one aspect of an embodiment of the present invention, the freezing time of step S4 is 4 to 8 hours; the drying temperature is -20°C, and the drying time is 12 to 24 hours.

[0047] According to one aspect of the embodiment of the present invention, the pickling time in step S5 is 5 hours, and the acid used is hydrochloric acid with a concentration of 0.05 to 0.5 mol / L. The different concentrations of hydrochloric acid are 0.05, 0.1, 0.2, 0.3, 0.4, and 0.5 mol / L.

[0048] Based on a general concept of the invention, an embodiment of the present invention provides a soft foam-type lithium ion sieve composite adsorbent obtained by the above-mentioned preparation method.

[0049] Another object of an embodiment of the present invention is to provide a lithium-extracting agent for lithium-containing solutions, including a soft foam-type lithium ion sieve composite adsorbent obtained by the above-mentioned preparation method.

[0050] According to one aspect of an embodiment of the present invention, the lithium-containing solution includes at least one of salt lake brine, seawater, geothermal water, and waste lithium battery leaching solution.

[0051] The following will be described in detail through specific examples. In the following examples, the pickling process adopts a conventional method, and the titanium-based lithium ion sieve precursor is pickled with a hydrochloric acid solution to elute part of the lithium therein to form a lithium ion sieve with a hole structure.

[0052] The following is a detailed description through specific embodiments.

[0053] Example 1

[0054] A method for preparing a soft foam type lithium ion sieve composite adsorbent comprises the following steps:

[0055] S1: Dissolve 1.75 g of hydroxyethyl cellulose (HEC) and 0.75 g of N,N-methylenebisacrylamide (MBA) in 45 mL of deionized water to obtain a HEC solution;

[0056] S2: 1.5 g Li4Ti5O 12 The powder was added into a viscous HEC solution at 5 °C, stirred for 10 min / time, and then ultrasonicated for 10 min / time, and repeated three times to obtain Li4Ti5O 12 LTO adsorbent precursor solution with 60% loading;

[0057] S3: 1.0 mL of 8 wt.% ammonium persulfate (APS) solution and 1.0 mL of 4 wt.% N,N,N′,N′-tetramethylethylenediamine (TEMED) solution were added dropwise to the LTO adsorbent precursor solution to obtain a mixed solution;

[0058] S4: The mixed solution was injected into a mold beaker and frozen for 8 hours, and then cooled to -20°C using a freeze dryer and kept at this temperature for 24 hours to obtain LTO-HEC cryogel;

[0059] S5: LTO-HEC cryogel was treated with 0.3 mol / L hydrochloric acid to obtain Li4Ti5O 12 The soft foam lithium ion sieve adsorbent has a loading of 60%. Figure 1 As shown, and subjected to durability test. Figure 1 The results show that after multiple cycles of testing, the foam can still recover to a similar height after multiple compressions. The similar foam height indicates that the sample has strong recovery and does not break after each compression. The results of the durability test confirm the stability of the foam and its potential for long-term application. The surface was characterized using SEM, and the results are as follows Figure 2 As shown, the foam samples have a similar white appearance. The mixed cavitation in the presence of surfactants produces spongy and porous foams with continuously interconnected macropores. The foams are highly porous and rigid in the dry state. The presence of lithium ion sieve particles leads to the production of irregularly shaped but interconnected macrovoids, showing a more rough and porous foam surface.

[0060] The present invention is the first to use hydroxyethyl cellulose (HEC) and N, N-methylenebisacrylamide (MBA) with Li4Ti5O 12Combined with ammonium persulfate (APS) and N, N, N', N'-tetramethylethylenediamine (TEMED), gel formation and solidification are promoted to improve the stability and adsorption performance of the material, forming a soft foam-type lithium ion sieve adsorbent, which has excellent hydrophilicity, can increase the fluidity during lithium extraction and reduce loss, thereby having a higher adsorption capacity and a faster adsorption rate. It is used in the extraction of lithium from liquid lithium resources, and only 1-1.5 hours are required to reach adsorption equilibrium. The foam-type composite adsorbent prepared by the present invention is loose, porous, elastic, and easy to realize continuous industrial production.

[0061] Example 2

[0062] 1.75 g of hydroxyethyl cellulose was replaced by 1.5 g of hydroxyethyl cellulose, and the other steps and parameters were the same as those in Example 1.

[0063] Example 3

[0064] The hydroxyethyl cellulose was replaced by polyvinyl alcohol, and the other steps and parameters were the same as those in Example 1.

[0065] Example 4

[0066] N,N-methylenebisacrylamide was replaced by urea formaldehyde, and other steps and parameters were the same as those in Example 1.

[0067] Example 5

[0068] 0.75 g of N,N-methylenebisacrylamide was replaced with 1.0 g of N,N-methylenebisacrylamide, and the other steps and parameters were the same as those in Example 1.

[0069] Example 6

[0070] 8 wt. % ammonium persulfate was replaced by 13 wt. % ammonium persulfate, and other steps and parameters were the same as in Example 1.

[0071] Example 7

[0072] The ammonium persulfate was replaced by azobisisobutyronitrile, and the other steps and parameters were the same as those in Example 1.

[0073] Example 8

[0074] The 0.3 mol / L hydrochloric acid was replaced by 0.1 mol / L hydrochloric acid, and the other steps and parameters were the same as those in Example 1.

[0075] Example 9

[0076] The 0.3 mol / L hydrochloric acid was replaced by 0.05 mol / L hydrochloric acid, and the other steps and parameters were the same as those in Example 1.

[0077] Application Example 1

[0078] The soft foam lithium ion sieve adsorbent prepared in Example 1 was placed in a solution having an initial lithium ion concentration of 150 mg·L -1 In the adsorption solution, under the conditions of pH = 12 and reaction temperature of 293K, it only takes 1 hour to reach adsorption equilibrium. The ICP test results show that the adsorption capacity of the soft foam lithium ion sieve adsorbent is 27.9 mg g -1 .

[0079] Application Example 2

[0080] The soft foam lithium ion sieve adsorbent prepared in Example 1 was placed in a solution having an initial lithium ion concentration of 150 mg·L -1 In the adsorption solution, at pH = 12, the reaction temperature is 293K, 303K, 313K, and the reaction time is 2h. The ICP test results show that the adsorption capacity of lithium ions is 28.1mg / g, 30.9mg / g and 33.5mg / g respectively.

[0081] Application Example 3

[0082] The soft foam lithium ion sieve adsorbent prepared in Example 1 was placed in a solution having an initial lithium ion concentration of 150 mg·L -1 The adsorption capacity of the adsorbent was 0.25, 0.5, 0.75, 1, 1.25, 1.5, 1.75, 2, 3, 5 and 6 h at pH = 12, reaction temperature 293 K and reaction time 0, 0.25, 0.5, 0.75, 1, 1.25, 1.5, 1.75, 2, 3, 5 and 6 h. The ICP test results show that the adsorption capacity of the adsorbent for lithium ions is 0. Figure 3 As shown, it was found that the adsorption equilibrium could be reached in 1-1.5 h, and the adsorption capacity was 27.9 mg / g.

[0083] Application Example 4

[0084] The soft foam lithium ion sieve adsorbent prepared in Example 1 was placed in a solution having an initial lithium ion concentration of 150 mg·L -1 The adsorption liquid was set at pH = 9, the reaction temperature was 293K, and the reaction time was 7h. Eight cycles of adsorption and desorption experiments were carried out. The ICP test results showed that the adsorption capacity of lithium ions increased from 27.9 mg·g -1 Decreased and stabilized at 27.3 mg·g -1 , remains at 97.8% of the initial value, as Figure 4 As shown, it can be seen that after 8 cycles, the lithium adsorption capacity of the soft foam lithium ion sieve adsorbent decreased slightly, but still remained at 97.8% of the initial value, which indicates that the prepared low-temperature gel foam has stable adsorption performance.

[0085] Application Example 5

[0086] The soft foam lithium ion sieve adsorbent prepared in Example 1 was placed in simulated brine (Li +:150mg·L -1 , Na + , K + , Ca 2+ and Mg 2+ :100mg·L -1 ), pH = 12, reaction temperature 293K, reaction time 2h. The ICP test results show that the adsorption capacity of the soft foam lithium ion sieve adsorbent for these cations is 28.1 mg·g -1 , 1.4mg·g -1 , 1.1mg·g -1 , 0.6mg·g -1 and 2.3 mg g -1 , Li + To Na + , K + , Ca 2+ and Mg 2+ The separation factors are 83.33, 70.67, 64.70, and 118.07, respectively. Figure 5 As shown, it can be seen that the distribution coefficient K of the soft foam lithium ion sieve adsorbent d The values ​​show the following pattern: Li + >>Ca 2+ >K + >Na + >Mg 2+ , indicating that the soft foam lithium ion sieve adsorbent has extremely high Li + Selective.

[0087] Comparative Example 1

[0088] A method for preparing a lithium ion sieve adsorbent comprises the following steps:

[0089] 3.0 g chitosan was dissolved in 2% glacial acetic acid to obtain 100 mL 3.0 wt.% CTS solution, and 3 g powdered lithium ion sieve H4Ti5O was added. 12 According to the molar ratio of polysaccharide solution to epichlorohydrin of 1, 1.72g epichlorohydrin was added to the suspension and reacted in a water bath at 323K for 2 hours. Then, 1mol·L - 1NaOH was added to obtain a spherical particle adsorbent, and the second step of crosslinking was carried out at 323K for 5 hours. Then it was frozen for 8 hours, and then cooled to -20°C using a freeze dryer and kept at this temperature for 24 hours. After freeze drying, the spherical desiccant was filtered out, and the surface was washed with distilled water and anhydrous ethanol for later use to obtain epichlorohydrin crosslinked chitosan granulated lithium ion sieve powder. The obtained granular lithium ion sieve was compared with Example 1. The granular lithium ion sieve was placed in an initial lithium ion concentration of 150 mg·L -1 The adsorption liquid was pH=12, the reaction temperature was 293K, and the equilibrium adsorption capacity was 24.7 mg·g -1 , the equilibrium time is 8h, and the performance is much lower than that of Example 1.

[0090] Comparative Example 2

[0091] The difference from Example 1 is that no lithium ion sieve is added, and other steps and parameters are the same to obtain pure HEC cryogel.

[0092] Put it into the initial lithium ion concentration of 150mg·L -1 The adsorption equilibrium was reached in the adsorption solution at pH = 12 and reaction temperature of 293 K. The ICP test results showed that its adsorption capacity for lithium ions was 0.1 mg / g.

[0093] Comparative Example 3

[0094] 1.75 g of hydroxyethyl cellulose was replaced by 0.5 g of hydroxyethyl cellulose, and the other steps and parameters were the same as those in Example 1.

[0095] Put it into the initial lithium ion concentration of 150mg·L -1 The adsorption was carried out in an adsorption solution at pH = 12, a reaction temperature of 293 K, and a balance time of 5 h. The ICP test results showed that the equilibrium adsorption capacity of lithium ions was 10.5 mg / g, which was far less than that of Example 1.

[0096] Comparative Example 4

[0097] 0.75 g of N,N-methylenebisacrylamide was replaced with 0.5 g of N,N-methylenebisacrylamide, and the other steps and parameters were the same as those in Example 1.

[0098] Put it into the initial lithium ion concentration of 150mg·L -1 The adsorption was carried out in an adsorption solution at pH = 12, a reaction temperature of 293 K, and a balance time of 4 hours. The ICP test results showed that the equilibrium adsorption capacity of lithium ions was 10.7 mg / g, which was far less than that of Example 1.

[0099] Comparative Example 5

[0100] The freezing for 8 h was replaced by freezing for 2 h, and the other steps and parameters were the same as in Example 1.

[0101] Put it into the initial lithium ion concentration of 150mg·L -1 The adsorption was carried out in an adsorption solution at pH = 12, a reaction temperature of 293 K, and a balance time of 4 hours. The ICP test results showed that the equilibrium adsorption capacity of lithium ions was 8.2 mg / g, which was far less than that of Example 1.

[0102] Comparative Example 6

[0103] The drying process for 24 h was replaced by drying for 10 h, and the other steps and parameters were the same as those in Example 1.

[0104] Put it into the initial lithium ion concentration of 150mg·L -1 The adsorption was carried out in an adsorption solution at pH = 12 and a reaction temperature of 293 K, and the equilibrium time was 5.5 h. The ICP test results showed that the equilibrium adsorption capacity of lithium ions was 10.2 mg / g, which was far less than that of Example 1.

[0105] Comparative Example 7

[0106] 1.5 g Li4Ti5O 12 The powder was added to the viscous HEC solution at 12°C, and the other steps and parameters were the same as in Example 1.

[0107] Put it into the initial lithium ion concentration of 150mg·L -1 The adsorption was carried out in an adsorption solution at pH = 12 and a reaction temperature of 293 K, and the equilibrium time was 4.5 h. The ICP test results showed that the equilibrium adsorption capacity of lithium ions was 7.9 mg / g, which was far less than that of Example 1.

[0108] The above is a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing a soft foam type lithium ion sieve composite adsorbent, characterized in that: The steps include: S1: dissolving organic matter A and organic matter B in deionized water to obtain an organic solution; S2: Take Li4Ti5O 12 The powder is added to the organic solution at a certain temperature, and subjected to multiple stirring and ultrasonic treatment to obtain a loaded LTO adsorbent precursor solution; S3: adding an initiator and a catalyst dropwise to the LTO-loaded adsorbent precursor solution to obtain a mixed solution; S4: injecting the mixed solution into a mold, freezing and drying to obtain LTO cryogel; S5: The LTO cryogel is subjected to an acid washing treatment to obtain HTO cryogel.

2. The method for preparing a soft foam type lithium ion sieve composite adsorbent according to claim 1, characterized in that: In step S1, the organic substance A is any one of hydroxyethyl cellulose, resorcinol, and polyvinyl alcohol, and the added amount is 0.75-1.75 g; the organic substance B is any one of N,N-methylenebisacrylamide, urea-formaldehyde, and glutaraldehyde, and the added amount is 0.75-1.75 g.

3. The method for preparing a soft foam type lithium ion sieve composite adsorbent according to claim 1, characterized in that: The content of LTO loaded in step S2 is 10% to 90%.

4. The method for preparing a soft foam type lithium ion sieve composite adsorbent according to claim 1, characterized in that: In step S2, the temperature is 0-10° C.; the stirring time is 10 min / time, at least 3 times; and the ultrasonic time is 10 min / time, at least 3 times.

5. The method for preparing a soft foam type lithium ion sieve composite adsorbent according to claim 1, characterized in that: In step S3, the initiator is any one of ammonium persulfate, hydrogen peroxide, and azobisisobutyronitrile, and the concentration is 3 to 13 wt.%; the catalyst is any one of N,N,N′,N′-tetramethylethylenediamine, N,N,N′,N′-tetraethylethylenediamine, and N,N,N′,N′-tetramethyl-1,3-propylenediamine, and the concentration is 1 to 7 wt.%.

6. The method for preparing a soft foam type lithium ion sieve composite adsorbent according to claim 1, characterized in that: The freezing time of step S4 is 4 to 8 hours; the drying temperature is -20°C, and the drying time is 12 to 24 hours.

7. The method for preparing a soft foam type lithium ion sieve composite adsorbent according to claim 1, characterized in that: The pickling time in step S5 is 5 hours, and the acid used is hydrochloric acid with a concentration of 0.05-0.5 mol / L.

8. A soft foam type lithium ion sieve composite adsorbent obtained by the preparation method according to any one of claims 1 to 7.

9. A lithium-extracting agent for lithium-containing solution, characterized in that: The invention relates to a soft foam type lithium ion sieve composite adsorbent obtained by the preparation method according to any one of claims 1 to 7.

10. A lithium-extracting agent for lithium-containing solution according to claim 9, characterized in that: The lithium-containing solution includes at least one of salt lake brine, seawater, geothermal water, and waste lithium battery leaching solution.

Citation Information

Cited By

  • Preparation method and application of lithium ion adsorption material

    CN118356918A

  • Preparation method of lithium ion adsorption material and application thereof

    CN118356918B