Method for preparing denitration catalyst by utilizing stepped fibers and denitration catalyst

Through the stepped fiber preparation method, the problem of a single length of glass fiber in the existing technology is solved, the effective utilization of fibers of different lengths is realized, and the performance and resource utilization rate of the denitration catalyst are improved.

CN118719045AActive Publication Date: 2024-10-01CHINA ENERGY LONGYUAN ENVIRONMENTAL PROTECTION CO LTD +2

Patent Information

Application Number
CN202410786120.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-18
Publication Date
2024-10-01
Estimated Expiration
2044-06-18

AI Technical Summary

Technical Problem

The glass fibers in existing denitration catalysts have a single length and cannot effectively utilize fibers of different lengths, resulting in a waste of resources and insufficient performance.

Method used

Using a stepped fiber preparation method, glass fibers of different lengths are graded, and then aged, extruded, and sintered after pretreatment and mixing to prepare a denitrification catalyst with excellent denitrification performance and mechanical strength.

Benefits of technology

It realizes the gradient utilization of glass fibers of different lengths, improves the mechanical strength and denitration performance of the denitration catalyst, and promotes the resource utilization of glass fibers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004898665600000151
    Figure BDA0004898665600000151
  • Figure BDA0004898665600000161
    Figure BDA0004898665600000161
  • Figure BDA0004898665600000162
    Figure BDA0004898665600000162
Patent Text Reader

Abstract

The invention relates to the technical field of denitration, and discloses a method for preparing a denitration catalyst by using stepped fibers and the denitration catalyst. The method comprises the following steps: mixing titanium dioxide, pretreated glass fibers A and an organic solvent C to obtain modified titanium dioxide; mixing a tungsten source, the modified titanium dioxide, a vanadium source, a C1-C10 alcohol compound and an ammonia water solution to obtain a titanium-tungsten-vanadium mixture; and mixing the pretreated glass fiber B, the titanium-tungsten-vanadium mixture, a lubricant, the pretreated glass fiber C, the pretreated glass fiber D, a binder, a plasticizer and the pretreated glass fiber E, and then performing aging, extrusion forming and sintering. According to the method, gradient utilization of the glass fibers can be achieved, the glass fibers with different lengths are applied to preparation of the denitration catalyst at the same time, and a foundation can be laid for follow-up recovery of the glass fibers with different lengths.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of denitration, and in particular to a method for preparing a denitration catalyst by utilizing stepped fibers and the denitration catalyst. Background Art

[0002] Coal is the main energy source in my country. Nitrogen oxides in coal-fired flue gas are pollutants that need to be controlled. Among them, NH3-SCR is currently the most popular flue gas denitrification method.

[0003] Denitration catalyst is the key to SCR reaction. The commonly used denitration catalyst in industry is honeycomb vanadium-titanium denitration catalyst, which has high efficiency. The main components of the catalyst are metal oxides and a small amount of glass fiber. In the preparation method of traditional denitration catalyst, short-cut fibers of specific length are usually used, and the length is relatively uniform. At the same time, the existing technology lacks exploration of the influence of glass fiber length on the strength of denitration catalyst.

[0004] At present, the glass fibers obtained by recycling a large amount of waste are irregular in length and cannot reach uniform length. The existing technology can only use fibers of a specific length, and the recycled fibers are not fully utilized. Therefore, how to apply glass fibers of different lengths to the field of denitrification catalysts is the focus of current research. Summary of the invention

[0005] The purpose of the present invention is to overcome the problems that the glass fibers in the denitration catalyst in the prior art need to be of a single length, the utilization of fibers of different lengths is narrow, and the glass fibers obtained by recycling existing wastes are irregular in length and difficult to realize resource utilization. The present invention provides a method for preparing a denitration catalyst using stepped fibers and a denitration catalyst. The present invention can realize the utilization of glass fibers of various sizes by exploring the gradation of glass fibers of different lengths, thereby effectively expanding the application range of glass fibers and improving the overall performance of the product.

[0006] In order to achieve the above object, the present invention provides a method for preparing a denitration catalyst using stepped fibers, the method comprising the following steps:

[0007] (1) mixing glass fiber A, organic solvent A, water and polymer A to obtain pretreated glass fiber A; mixing glass fiber B, organic solvent B, water and polymer B to obtain pretreated glass fiber B; mixing glass fiber C with an organic acid aqueous solution to react to obtain pretreated glass fiber C; soaking glass fiber D in a first polyacrylamide aqueous solution to obtain pretreated glass fiber D; soaking glass fiber E in a second polyacrylamide aqueous solution to obtain pretreated glass fiber E;

[0008] (2) mixing titanium dioxide, pretreated glass fiber A and organic solvent C to obtain modified titanium dioxide; mixing a tungsten source, modified titanium dioxide, a vanadium source, a C1-C10 alcohol compound and an ammonia solution to obtain a titanium-tungsten-vanadium mixture;

[0009] (3) mixing the pretreated glass fiber B, the titanium-tungsten-vanadium mixture, the lubricant, the pretreated glass fiber C, the pretreated glass fiber D, the binder, the plasticizer and the pretreated glass fiber E, and then aging, extruding and sintering them;

[0010] Wherein, polymer A and polymer B are each independently selected from polyethylene oxide and / or polyacrylamide;

[0011] The length La of the glass fiber A is in the range of 0.5 mm ≤ La < 1 mm, the length Lb of the glass fiber B is in the range of 1 mm ≤ Lb < 3 mm, the length Lc of the glass fiber C is in the range of 3 mm ≤ Lc < 5 mm, the length Ld of the glass fiber D is in the range of 5 mm ≤ Ld < 7 mm, and the length Le of the glass fiber E is in the range of 7 mm ≤ Le ≤ 9 mm;

[0012] Based on the total weight of the glass fibers, the content of the glass fibers C is 45-70 wt %.

[0013] Preferably, based on the total weight of the glass fibers, the content of glass fiber A is 5-15wt%, the content of glass fiber B is 10-25wt%, the content of glass fiber C is 45-70wt%, the content of glass fiber D is 10-25wt%, and the content of glass fiber E is 5-15wt%.

[0014] Preferably, the ratio of the total weight of the glass fibers to the weight of the titanium dioxide is 5-15:100, wherein the glass fibers are calculated as SiO2.

[0015] Preferably, in step (1), the organic solvent A and the organic solvent B are independently selected from one or more of C1-C5 alcohol compounds, acetone and dimethyl ether.

[0016] Preferably, in step (1), the organic acid is selected from one or more of citric acid, tartaric acid, oxalic acid, acetic acid, ethylenediaminetetraacetic acid, hydroxyethylidene diphosphonic acid, aminotrimethylphosphinic acid and ethylenediaminetetramethylphosphinic acid; and / or

[0017] The concentration of the organic acid aqueous solution is ≤0.1 mol / L.

[0018] Preferably, the specific process of step (2) includes:

[0019] (2.1) mixing titanium dioxide, pretreated glass fiber A and organic solvent C to obtain modified titanium dioxide;

[0020] (2.2) mixing the tungsten source, the modified titanium dioxide and the first ammonia solution and then ball milling to obtain a titanium-tungsten mixture;

[0021] (2.3) Mixing the titanium-tungsten mixture, the vanadium source, the C1-C10 alcohol compound and the second ammonia solution to obtain a titanium-tungsten-vanadium mixture.

[0022] Preferably, in step (2.2), the weight ratio of the tungsten source to the titanium dioxide is 2.5-5wt:100, wherein the tungsten source is calculated as WO3; and / or

[0023] In step (2.3), the weight ratio of the vanadium source to the titanium dioxide is 0.8-1.5wt:100, wherein the vanadium source is calculated as V2O5; and / or

[0024] In step (2.3), the C1-C10 alcohol compound is selected from one or more of monoethanolamine, diethanolamine, triethanolamine, diethylene glycol, glycerol, dipropylene glycol, trimeryl glycol and triisopropanolamine.

[0025] Preferably, the specific process of step (3) includes:

[0026] (3.1) Mixing the pretreated glass fiber B, titanium-tungsten-vanadium mixture and part of the lubricant;

[0027] (3.2) mixing the material obtained in step (3.1), pretreated glass fiber C, pretreated glass fiber D, a binder, and a plasticizer;

[0028] (3.3) The material obtained in step (3.2), the pretreated glass fiber E and the remaining lubricant are mixed, and then aged, extruded and sintered.

[0029] Preferably, the lubricant is selected from one or more of glycerol, triethanolamine and stearic acid; and / or

[0030] The plasticizer is selected from phthalic acid and / or dioctyl phthalate; and / or

[0031] The binder is selected from one or more of polyvinyl alcohol, methyl cellulose, hydroxymethyl cellulose, polyacrylamide and polyethylene glycol.

[0032] The second aspect of the present invention provides a denitration catalyst prepared according to the method described above.

[0033] The method of the present invention can realize the gradient utilization of glass fibers, and glass fibers of different lengths can be simultaneously applied to the preparation of denitration catalysts, which can lay a foundation for the subsequent recovery of glass fibers of different lengths. At the same time, the denitration catalyst prepared by the method of the present invention has a certain improvement in mechanical strength on the basis of excellent denitration performance. DETAILED DESCRIPTION

[0034] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.

[0035] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0036] In one aspect, the present invention provides a method for preparing a denitration catalyst using stepped fibers, the method comprising the following steps:

[0037] (1) mixing glass fiber A, organic solvent A, water and polymer A to obtain pretreated glass fiber A; mixing glass fiber B, organic solvent B, water and polymer B to obtain pretreated glass fiber B; mixing glass fiber C with an organic acid aqueous solution to react to obtain pretreated glass fiber C; soaking glass fiber D in a first polyacrylamide aqueous solution to obtain pretreated glass fiber D; soaking glass fiber E in a second polyacrylamide aqueous solution to obtain pretreated glass fiber E;

[0038] (2) mixing titanium dioxide, pretreated glass fiber A and organic solvent C to obtain modified titanium dioxide; mixing a tungsten source, modified titanium dioxide, a vanadium source, a C1-C10 alcohol compound and an ammonia solution to obtain a titanium-tungsten-vanadium mixture;

[0039] (3) mixing the pretreated glass fiber B, the titanium-tungsten-vanadium mixture, the lubricant, the pretreated glass fiber C, the pretreated glass fiber D, the binder, the plasticizer and the pretreated glass fiber E, and then aging, extruding and sintering them;

[0040] Wherein, polymer A and polymer B are each independently selected from polyethylene oxide and / or polyacrylamide;

[0041] The length La of the glass fiber A is in the range of 0.5 mm ≤ La < 1 mm, the length Lb of the glass fiber B is in the range of 1 mm ≤ Lb < 3 mm, the length Lc of the glass fiber C is in the range of 3 mm ≤ Lc < 5 mm, the length Ld of the glass fiber D is in the range of 5 mm ≤ Ld < 7 mm, and the length Le of the glass fiber E is in the range of 7 mm ≤ Le ≤ 9 mm;

[0042] Based on the total weight of the glass fibers, the content of the glass fibers C is 45-70 wt %.

[0043] In a preferred embodiment, based on the total weight of the glass fibers, the content of glass fiber A is 5-15wt%, the content of glass fiber B is 10-25wt%, the content of glass fiber C is 45-70wt%, the content of glass fiber D is 10-25wt%, and the content of glass fiber E is 5-15wt%. In the present invention, the total weight of the glass fibers refers to the total weight of glass fiber A, glass fiber B, glass fiber C, glass fiber D and glass fiber E.

[0044] The method described in the present invention realizes the simultaneous use of glass fibers of different lengths in the preparation process of the denitration catalyst, which not only promotes the resource utilization of recycled glass fibers, but also further improves the mechanical properties of the prepared denitration catalyst by optimizing the ratio of glass fibers of different lengths.

[0045] More preferably, based on the total weight of the glass fibers, the content of the glass fibers A is less than or equal to the content of the glass fibers D.

[0046] More preferably, based on the total weight of the glass fibers, the content of the glass fibers E is less than or equal to the content of the glass fibers B.

[0047] In order to further improve the mechanical strength and denitrification performance of the denitrification catalyst, in a preferred embodiment, the ratio of the total weight of the glass fiber to the weight of the titanium dioxide is 5-15:100, wherein the glass fiber is calculated as SiO2; specifically, it can be 5:100, 6:100, 7:100, 8:100, 9:100, 10:100, 11:100, 12:100, 13:100, 14:100 or 15:100.

[0048] In the present invention, in step (1), non-acidic water-soluble organic matter and a small amount of polymer are added to glass fiber A and glass fiber B for treatment, respectively, so as to improve the overall dispersion of the fibers. Preferably, the weight average molecular weight of polyethylene oxide is 1000-20000; the weight average molecular weight of polyacrylamide is 500-20000. In a preferred case, organic solvent A and organic solvent B are independently selected from one or more of C1-C5 alcohol compounds, acetone and dimethyl ether; specifically, C1-C5 alcohol compounds can be methanol, ethanol, n-propanol, isopropanol, ethylene glycol, propylene glycol or glycerol.

[0049] In a preferred embodiment, in step (1), the process of obtaining the pretreated glass fiber A comprises: mixing the glass fiber A, the organic solvent A, water and the polymer A, and then performing solid-liquid separation, washing and drying. Further preferably, the liquid-solid ratio of the organic solvent A to the glass fiber A is 10-20 mL:1 g, the liquid-solid ratio of water to the glass fiber A is 5-20 mL:1 g; the weight ratio of the polymer A to the glass fiber A is 0.5-2:10; and the mixing conditions include: the temperature is 30-60°C and the time is 30-120 min.

[0050] In a preferred embodiment, in step (1), the process of obtaining the pretreated glass fiber B comprises: mixing the glass fiber B, water, organic solvent B and polymer B, and then performing solid-liquid separation, washing and drying. Further preferably, the liquid-solid ratio of the organic solvent B to the glass fiber B is 10-20 mL:1 g, the liquid-solid ratio of water to the glass fiber B is 5-20 mL:1 g; the weight ratio of the polymer B to the glass fiber B is 0.5-2:10, and the mixing conditions include: the temperature is 60-90°C and the time is 30-120 min.

[0051] In a preferred embodiment, in step (1), the organic acid is selected from one or more of citric acid, tartaric acid, oxalic acid, acetic acid, ethylenediaminetetraacetic acid, hydroxyethylidene diphosphonic acid, aminotrimethylphosphinic acid and ethylenediaminetetramethylphosphinic acid, more preferably citric acid, tartaric acid or oxalic acid. The concentration of the organic acid aqueous solution is ≤0.1 mol / L, more preferably 0.03-0.08 mol / L.

[0052] In a preferred embodiment, when the glass fiber C is mixed with the organic acid aqueous solution for reaction in step (1), the reaction temperature is ≤40°C, more preferably 20-30°C; the reaction time is 10-90min; and the liquid-to-solid ratio of the organic acid aqueous solution to the glass fiber C is 5-20mL:1g.

[0053] In a preferred embodiment, in step (1), the glass fiber D is immersed in the first polyacrylamide aqueous solution for 30-120 min, the concentration of the first polyacrylamide aqueous solution is 2-8 wt %; and the liquid-to-solid ratio of the first polyacrylamide aqueous solution to the glass fiber D is 5-20 mL:1 g.

[0054] In a preferred embodiment, in step (1), the glass fiber E is immersed in the second polyacrylamide aqueous solution for 30-120 min, the concentration of the second polyacrylamide aqueous solution is 2-8 wt %, and the liquid-to-solid ratio of the second polyacrylamide aqueous solution to the glass fiber D is 5-20 mL:1 g.

[0055] In a preferred embodiment, the specific process of step (2) includes:

[0056] (2.1) mixing titanium dioxide, pretreated glass fiber A and organic solvent C to obtain modified titanium dioxide;

[0057] (2.2) mixing the tungsten source, the modified titanium dioxide and the first ammonia solution and then ball milling to obtain a titanium-tungsten mixture;

[0058] (2.3) Mixing the titanium-tungsten mixture, the vanadium source, the C1-C10 alcohol compound and the second ammonia solution to obtain a titanium-tungsten-vanadium mixture.

[0059] In a preferred embodiment, in step (2), the weight ratio of the tungsten source to the titanium dioxide is 2.5-5:100, wherein the tungsten source is calculated as WO3; specifically, it can be 2.5:100, 3:100, 3.5:100, 4:100, 4.5:100 or 5:100. In the present invention, the tungsten source can be ammonium metatungstate or ammonium paratungstate.

[0060] Preferably, in step (2.1), the organic solvent C is a C1-C5 alcohol compound, such as ethylene glycol; the mixing temperature is 40-90°C, the mixing time is 30-60 min, and centrifugal separation is performed after the mixing is completed.

[0061] In a preferred embodiment, in step (2.2), the ball milling conditions include: a speed of 500-1000 r / min, a time of 20-40 min, and a concentration of the first ammonia solution of 3-7 wt %. There is no special requirement for the amount of the first ammonia solution, and it can be used according to the conventional amount in the art. Preferably, the liquid-solid ratio of the first ammonia solution to the solid material (tungsten source and modified titanium dioxide) is 5-10 mL: 1 g.

[0062] Preferably, in step (2), the weight ratio of the vanadium source to the titanium dioxide is 0.8-1.5:100, wherein the vanadium source is calculated as V2O5; specifically, it can be 0.8:100, 0.9:100, 1:100, 1.1:100, 1.2:100, 1.3:100, 1.4:100 or 1.5:100.

[0063] Preferably, in step (2.3), the concentration of the second aqueous ammonia solution is 3-7 wt %. Further preferably, the concentration and volume of the second aqueous ammonia solution are the same as those of the first aqueous ammonia solution.

[0064] In the present invention, the C1-C10 alcohol compound refers to a compound having 1 to 10 carbon atoms and having a hydroxyl group. Preferably, in step (2.3), the C1-C10 alcohol compound is selected from one or more of monoethanolamine, diethanolamine, triethanolamine, diethylene glycol, glycerol, dipropylene glycol, trimeryl glycol and triisopropanolamine. Preferably, the volume ratio of the C1-C10 alcohol compound to the first ammonia solution is 1:10-20.

[0065] In a preferred embodiment, the specific process of step (3) includes:

[0066] (3.1) Mixing the pretreated glass fiber B, titanium-tungsten-vanadium mixture and part of the lubricant;

[0067] (3.2) mixing the material obtained in step (3.1), pretreated glass fiber C, pretreated glass fiber D, a binder, and a plasticizer;

[0068] (3.3) The material obtained in step (3.2), the pretreated glass fiber E and the remaining lubricant are mixed, and then aged, extruded and sintered.

[0069] Preferably, in step (3.1), the amount of lubricant used is 5-10 wt % of the total amount of lubricant.

[0070] Preferably, in step (3.1), the mixing temperature is 150-200°C, and the mixing time is 0.5-3h.

[0071] Preferably, in step (3.2), the mixing temperature is 150-200° C., and the mixing time is 0.5-3 h.

[0072] Preferably, in step (3.3), the mixing temperature is 180-220° C., and the mixing time is 0.5-3 h.

[0073] In a preferred embodiment, the lubricant is selected from one or more of glycerol, triethanolamine and stearic acid; the plasticizer is selected from phthalic acid and / or dioctyl phthalate; and the binder is selected from one or more of polyvinyl alcohol, methyl cellulose, hydroxymethyl cellulose, polyacrylamide and polyethylene glycol.

[0074] In a preferred embodiment, the aging time is 20-30 hours.

[0075] In the present invention, in step (3.3), the extrusion molding and sintering can be carried out according to conventional conditions in the art. For example, the sintering temperature can be 400-600°C and the sintering time can be 2-5 hours.

[0076] In the present invention, there is no special requirement for the amount of lubricant, binder and plasticizer, and they can be used according to the conventional addition amount in the art. Specifically, the weight ratio of titanium dioxide, lubricant, binder and plasticizer is 1:0.05:0.1:0.06-0.1:0.07-0.1.

[0077] The second aspect of the present invention provides a denitration catalyst prepared according to the method described above.

[0078] The present invention will be described in detail below through examples, but the protection scope of the present invention is not limited thereto.

[0079] Example 1

[0080] (1) glass fiber A, organic solvent A (propylene glycol), water and polymer A (polyethylene oxide, weight average molecular weight of 1500-2000) are mixed, and then centrifuged, washed and dried to obtain pretreated glass fiber A; wherein the liquid-solid ratio of organic solvent A to glass fiber A is 10 mL:1 g, the liquid-solid ratio of water to glass fiber A is 10 mL:1 g, the weight ratio of polymer A to glass fiber A is 1:10, the mixing temperature is 50° C., and the mixing time is 60 min;

[0081] Glass fiber B, water, organic solvent B (propylene glycol) and polymer B (polyethylene oxide, weight average molecular weight of 1500-2000) are mixed, and then solid-liquid separation, washing and drying are performed to obtain pretreated glass fiber B; wherein the liquid-solid ratio of organic solvent B to glass fiber B is 10 mL:1 g, the liquid-solid ratio of water to glass fiber B is 10 mL:1 g, the weight ratio of polymer B to glass fiber B is 1:10, the mixing temperature is 70° C., and the mixing time is 60 min;

[0082] The glass fiber C is mixed with an organic acid aqueous solution (0.06 mol / L citric acid aqueous solution) to react, and then solid-liquid separation, washing and drying are performed to obtain a pretreated glass fiber C; wherein the mixing temperature is 25° C., the mixing time is 30 min, and the liquid-solid ratio of the organic acid aqueous solution to the glass fiber C is 15 mL:1 g mL:1 g;

[0083] The glass fiber D is immersed in the first polyacrylamide aqueous solution (with a concentration of 5 wt%) for 60 minutes, and then solid-liquid separation, washing and drying are performed to obtain a pretreated glass fiber D; wherein the liquid-solid ratio of the first polyacrylamide aqueous solution to the glass fiber D is 10 mL: 1 g;

[0084] The glass fiber E is immersed in the first polyacrylamide aqueous solution (with a concentration of 5 wt%) for 60 minutes, and then solid-liquid separation, washing and drying are performed to obtain a pretreated glass fiber E; wherein the liquid-solid ratio of the second polyacrylamide aqueous solution to the glass fiber D is 10 mL: 1 g;

[0085] (2) mixing titanium dioxide, pretreated glass fiber A and excess organic solvent C (ethylene glycol), and then performing solid-liquid separation, washing and drying to obtain modified titanium dioxide; wherein the mixing temperature is 60° C. and the mixing time is 30 min;

[0086] A tungsten source (ammonium metatungstate) and a first ammonia solution (with a concentration of 5 wt%) are mixed, and then modified titanium dioxide is added, followed by ball milling to obtain a titanium-tungsten mixture; wherein the ball milling rate is 800 r / min, and the ball milling time is 30 min; the weight ratio of the tungsten source to the titanium dioxide is 3:100, and the tungsten source is calculated as WO3; the ratio of the volume of the first ammonia solution to the sum of the weight of the tungsten source and the modified titanium dioxide is 10 mL: 1 g;

[0087] A titanium-tungsten mixture, a vanadium source (ammonium metavanadate), an alcohol compound (monoethanolamine) and a second ammonia solution (with a concentration of 5 wt%) are mixed, and then solid-liquid separation, washing and drying are performed to obtain a titanium-tungsten-vanadium mixture; wherein the weight ratio of the vanadium source to the titanium dioxide is 1.05:100, and the vanadium source is calculated as V2O5; the volume of the second ammonia solution is the same as that of the first ammonia solution; and the volume ratio of the alcohol compound to the first ammonia solution is 1:15;

[0088] (3.1) Pretreated glass fiber B, titanium-tungsten-vanadium mixture and 5 wt% of lubricant (triethanolamine) were mixed; wherein the mixing temperature was 180° C. and the mixing time was 1 h;

[0089] (3.2) mixing the material obtained in step (3.1), pretreated glass fiber C, pretreated glass fiber D, a binder (polyvinyl alcohol), and a plasticizer (phthalic acid); wherein the mixing temperature is 180° C. and the mixing time is 1 h;

[0090] (3.3) The material obtained in step (3.2), the pretreated glass fiber E and the remaining lubricant are mixed, and then aged, extruded and sintered; wherein the mixing temperature is 200° C., the mixing time is 1 h, the aging time is 24 h, the sintering temperature is 500° C., and the sintering time is 4 h;

[0091] The length La of the glass fiber A is in the range of 0.5 mm ≤ La < 1 mm, the length Lb of the glass fiber B is in the range of 1 mm ≤ Lb < 3 mm, the length Lc of the glass fiber C is in the range of 3 mm ≤ Lc < 5 mm, the length Ld of the glass fiber D is in the range of 5 mm ≤ Ld < 7 mm, and the length Le of the glass fiber E is in the range of 7 mm ≤ Le ≤ 9 mm;

[0092] Based on the total weight of the glass fibers, the content of the glass fibers A is 6 wt %, the content of the glass fibers B is 14 wt %, the content of the glass fibers C is 57 wt %, the content of the glass fibers D is 15 wt %, and the content of the glass fibers E is 8 wt %;

[0093] The ratio of the total weight of the glass fiber to the weight of the titanium dioxide is 11:100, wherein the glass fiber is calculated as SiO2;

[0094] The weight ratio of titanium dioxide, lubricant, binder and plasticizer is 1:0.08:0.08:0.09.

[0095] Example 2

[0096] The method described in Example 1 is used for implementation, except that, based on the total weight of the glass fibers, the content of glass fiber A is 10wt%, the content of glass fiber B is 15wt%, the content of glass fiber C is 55wt%, the content of glass fiber D is 14wt%, and the content of glass fiber E is 6wt%.

[0097] Example 3

[0098] The method described in Example 1 is used for implementation, except that, firstly, the pretreatment process of glass fiber A, glass fiber B and glass fiber C in step (1) is adjusted; and secondly, the content of each component in the glass fiber is adjusted.

[0099] Specific:

[0100] Glass fiber A, organic solvent A (ethylene glycol), water and polymer A (polyacrylamide, weight average molecular weight of 1500-2000) are mixed, and then centrifuged, washed and dried to obtain pretreated glass fiber A; wherein the liquid-solid ratio of organic solvent A to glass fiber A is 10 mL:1 g, the liquid-solid ratio of water to glass fiber A is 10 mL:1 g, the weight ratio of polymer A to glass fiber A is 1:10, the mixing temperature is 50° C., and the mixing time is 60 min;

[0101] Glass fiber B, water, organic solvent B (ethylene glycol) and polymer B (polyacrylamide, weight average molecular weight of 1500-2000) are mixed, and then solid-liquid separation, washing and drying are performed to obtain pretreated glass fiber B; wherein the liquid-solid ratio of organic solvent B to glass fiber B is 10 mL:1 g, the liquid-solid ratio of water to glass fiber B is 10 mL:1 g, the weight ratio of polymer B to glass fiber B is 1:10, the mixing temperature is 60° C., and the mixing time is 60 min;

[0102] Based on the total weight of the glass fibers, the content of the glass fibers A was 10 wt %, the content of the glass fibers B was 15 wt %, the content of the glass fibers C was 55 wt %, the content of the glass fibers D was 14 wt %, and the content of the glass fibers E was 6 wt %.

[0103] Comparative Example 1

[0104] The method described in Example 1 was used for implementation, except that the lengths of the glass fibers AE were 3-5 mm.

[0105] Comparative Example 2

[0106] The method described in Example 1 was followed, except that all glass fibers were used directly without any pretreatment.

[0107] Specifically, the preparation process of the catalyst is:

[0108] (1) titanium dioxide, glass fiber A and excess organic solvent C (ethylene glycol) are mixed, and then solid-liquid separation, washing and drying are performed to obtain modified titanium dioxide; wherein the mixing temperature is 60° C. and the mixing time is 30 min;

[0109] A tungsten source (ammonium metatungstate) and a first ammonia solution (with a concentration of 5 wt%) are mixed, and then modified titanium dioxide is added, followed by ball milling to obtain a titanium-tungsten mixture; wherein the ball milling rate is 800 r / min, and the ball milling time is 30 min; the weight ratio of the tungsten source to the titanium dioxide is 3:100, and the tungsten source is calculated as WO3; the ratio of the volume of the first ammonia solution to the sum of the weight of the tungsten source and the modified titanium dioxide is 10 mL: 1 g;

[0110] A titanium-tungsten mixture, a vanadium source (ammonium metavanadate), an alcohol compound (monoethanolamine) and a second ammonia solution (with a concentration of 5 wt%) are mixed, and then solid-liquid separation, washing and drying are performed to obtain a titanium-tungsten-vanadium mixture; wherein the weight ratio of the vanadium source to the titanium dioxide is 1.05:100, and the vanadium source is calculated as V2O5; the volume of the second ammonia solution is the same as that of the first ammonia solution; and the volume ratio of the alcohol compound to the first ammonia solution is 1:15;

[0111] (2.1) mixing glass fiber B, titanium-tungsten-vanadium mixture and 5 wt% of lubricant (triethanolamine) at a mixing temperature of 180° C. and a mixing time of 1 h;

[0112] (2.2) mixing the material obtained in step (2.1), glass fiber C, glass fiber D, a binder (polyvinyl alcohol), and a plasticizer (phthalic acid); wherein the mixing temperature is 180° C. and the mixing time is 1 h;

[0113] (2.3) The material obtained in step (2.2), glass fiber E and the remaining lubricant are mixed, and then aged, extruded and sintered; wherein the mixing temperature is 200° C., the mixing time is 1 h, the aging time is 24 h, the sintering temperature is 500° C., and the sintering time is 4 h;

[0114] The length La of the glass fiber A is in the range of 0.5 mm ≤ La < 1 mm, the length Lb of the glass fiber B is in the range of 1 mm ≤ Lb < 3 mm, the length Lc of the glass fiber C is in the range of 3 mm ≤ Lc < 5 mm, the length Ld of the glass fiber D is in the range of 5 mm ≤ Ld < 7 mm, and the length Le of the glass fiber E is in the range of 7 mm ≤ Le ≤ 9 mm;

[0115] Based on the total weight of the glass fibers, the content of the glass fibers A is 6 wt %, the content of the glass fibers B is 14 wt %, the content of the glass fibers C is 57 wt %, the content of the glass fibers D is 15 wt %, and the content of the glass fibers E is 8 wt %;

[0116] The ratio of the total weight of the glass fiber to the weight of the titanium dioxide is 11:100, wherein the glass fiber is calculated as SiO2;

[0117] The weight ratio of titanium dioxide, lubricant, binder and plasticizer is 1:0.08:0.08:0.09.

[0118] Comparative Example 3

[0119] The method described in Example 1 is used for implementation, except that, based on the total weight of the glass fibers, the content of glass fiber A is 55wt%, the content of glass fiber B is 15wt%, the content of glass fiber C is 10wt%, the content of glass fiber D is 14wt%, and the content of glass fiber E is 6wt%.

[0120] Comparative Example 4

[0121] The method described in Example 1 is used for implementation, except that, based on the total weight of the glass fibers, the content of glass fiber A is 10wt%, the content of glass fiber B is 15wt%, the content of glass fiber C is 6wt%, the content of glass fiber D is 14wt%, and the content of glass fiber E is 55wt%.

[0122] Test Case

[0123] 1. The axial compressive strength and longitudinal compressive strength of the denitration catalysts obtained in Examples 1-3 and the products obtained in Comparative Examples 1-7 were tested using a TYE-300 pressure testing machine. The range of the pressure testing machine was 300 KN, and the pressurization rate was 250 N / s. The test results are shown in Table 1.

[0124] 2. The wear resistance of the denitration catalysts obtained in Examples 1-3 and the products obtained in Comparative Examples 1-4 were tested; the results are shown in the table.

[0125] Test method: Divide the sample to be tested into two parts, as test sample and reference sample respectively, dry the test sample and reference sample in an oven at 105°C for 2 hours, weigh the test sample and reference sample after natural cooling; then place the test sample and reference sample in the test bin and reference bin of the wear test device respectively, the test sample and reference sample are completely sealed with ceramic fiber paper from the bin wall, then pass air containing abrasive agent through the test sample at a certain flow rate, and pass air through the reference sample at the same flow rate, after 2 hours of wear, weigh the test sample, reference sample and abrasive agent after wear to calculate the wear intensity.

[0126] The specific calculation method is as follows:

[0127]

[0128] Among them, ξ h Indicates wear intensity, % / kg;

[0129] W1 represents the weight of the test sample before the test, kg;

[0130] W2 represents the weight of the test sample after the test, kg;

[0131] W3 represents the weight of the reference sample before the test, kg;

[0132] W4 represents the weight of the reference sample after the test, kg;

[0133] W represents the recorded weight of the abrasive, kg.

[0134] 3. Testing the denitration rates of nitrogen oxides of the denitration catalysts obtained in Examples 1-3 and the products obtained in Comparative Examples 1-4;

[0135] Test method: Test the nitrogen oxide denitrification rate of the denitrification catalyst at different temperatures: The test method is to take a small sample of the denitrification catalyst and a small sample of the product and load them into the catalyst performance evaluation reaction device, and introduce simulated gas for activity evaluation. The composition of the simulated gas is similar to that of industrial boiler exhaust gas, and its composition is as follows: 500ppm of NO, 400ppm of NH3, 10.00% of O2, 12% of water, and the rest is nitrogen. The simulated gas is passed into the denitrification reactor for reaction at a reaction temperature of 210°C. The concentration of nitrogen oxides in the flue gas before and after the reaction is analyzed using a 42i-HL flue gas analyzer, and then the denitrification rate of the denitrification catalyst is calculated when the reaction temperature is 210°C. The test results are shown in Table 2;

[0136] The reaction temperature in the denitration reactor is adjusted to 270°C to obtain the denitration rate of the denitration catalyst when the reaction temperature is 270°C. The test results are shown in Table 2.

[0137] The calculation method of the denitration rate of the denitration catalyst is: η=(ab) / a×100%, where the concentration of nitrogen oxides in the flue gas before the reaction is a, the concentration of nitrogen oxides in the flue gas after the reaction is b, and the denitration rate of the denitration catalyst is η.

[0138] Table 1

[0139]

[0140] Table 2

[0141]

[0142]

[0143] Combining the data in Table 1 and Table 2, it can be seen that the method of the present invention can be used to prepare a denitration catalyst with high compressive strength, good wear resistance and high denitration efficiency.

[0144] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A method for preparing a denitration catalyst using stepped fibers, characterized in that: The method comprises the following steps: (1) mixing glass fiber A, organic solvent A, water and polymer A to obtain pretreated glass fiber A; mixing glass fiber B, organic solvent B, water and polymer B to obtain pretreated glass fiber B; mixing glass fiber C with an organic acid aqueous solution to react to obtain pretreated glass fiber C; soaking glass fiber D in a first polyacrylamide aqueous solution to obtain pretreated glass fiber D; soaking glass fiber E in a second polyacrylamide aqueous solution to obtain pretreated glass fiber E; (2) mixing titanium dioxide, pretreated glass fiber A and organic solvent C to obtain modified titanium dioxide; mixing a tungsten source, modified titanium dioxide, a vanadium source, a C1-C10 alcohol compound and an ammonia solution to obtain a titanium-tungsten-vanadium mixture; (3) mixing the pretreated glass fiber B, the titanium-tungsten-vanadium mixture, the lubricant, the pretreated glass fiber C, the pretreated glass fiber D, the binder, the plasticizer and the pretreated glass fiber E, and then aging, extruding and sintering them; Wherein, polymer A and polymer B are each independently selected from polyethylene oxide and / or polyacrylamide; The length La of the glass fiber A is in the range of 0.5 mm ≤ La < 1 mm, the length Lb of the glass fiber B is in the range of 1 mm ≤ Lb < 3 mm, the length Lc of the glass fiber C is in the range of 3 mm ≤ Lc < 5 mm, the length Ld of the glass fiber D is in the range of 5 mm ≤ Ld < 7 mm, and the length Le of the glass fiber E is in the range of 7 mm ≤ Le ≤ 9 mm; Based on the total weight of the glass fibers, the content of the glass fibers C is 45-70 wt %.

2. The method according to claim 1, characterized in that: Based on the total weight of the glass fibers, the content of glass fiber A is 5-15wt%, the content of glass fiber B is 10-25wt%, the content of glass fiber C is 45-70wt%, the content of glass fiber D is 10-25wt%, and the content of glass fiber E is 5-15wt%.

3. The method according to claim 1 or 2, characterized in that: The ratio of the total weight of the glass fiber to the weight of the titanium dioxide is 5-15:100, wherein the glass fiber is calculated as SiO2.

4. The method according to claim 1, characterized in that: In step (1), the organic solvent A and the organic solvent B are independently selected from one or more of a C1-C5 alcohol compound, acetone and dimethyl ether.

5. The method according to claim 1 or 4, characterized in that: In step (1), the organic acid is selected from one or more of citric acid, tartaric acid, oxalic acid, acetic acid, ethylenediaminetetraacetic acid, hydroxyethylidene diphosphonic acid, aminotrimethylphosphinic acid and ethylenediaminetetramethylphosphinic acid; and / or The concentration of the organic acid aqueous solution is ≤0.1 mol / L.

6. The method according to claim 1 or 2, characterized in that: The specific process of step (2) includes: (2.1) mixing titanium dioxide, pretreated glass fiber A and organic solvent C to obtain modified titanium dioxide; (2.2) mixing the tungsten source, the modified titanium dioxide and the first ammonia solution and then ball milling to obtain a titanium-tungsten mixture; (2.3) Mixing the titanium-tungsten mixture, the vanadium source, the C1-C10 alcohol compound and the second ammonia solution to obtain a titanium-tungsten-vanadium mixture.

7. The method according to claim 1 or 6, characterized in that: In step (2), the weight ratio of the tungsten source to the titanium dioxide is 2.5-5:100, wherein the tungsten source is calculated as WO3; and / or In step (2), the weight ratio of the vanadium source to the titanium dioxide is 0.8-1.5:100, wherein the vanadium source is calculated as V2O5; and / or In step (2), the C1-C10 alcohol compound is selected from one or more of monoethanolamine, diethanolamine, triethanolamine, diethylene glycol, glycerol, dipropylene glycol, trimeryl glycol and triisopropanolamine.

8. The method according to claim 1, characterized in that: The specific process of step (3) includes: (3.1) Mixing the pretreated glass fiber B, titanium-tungsten-vanadium mixture and part of the lubricant; (3.2) mixing the material obtained in step (3.1), pretreated glass fiber C, pretreated glass fiber D, a binder, and a plasticizer; (3.3) The material obtained in step (3.2), the pretreated glass fiber E and the remaining lubricant are mixed, and then aged, extruded and sintered.

9. The method according to claim 1 or 8, characterized in that: The lubricant is selected from one or more of glycerol, triethanolamine and stearic acid; and / or The plasticizer is selected from phthalic acid and / or dioctyl phthalate; and / or The binder is selected from one or more of polyvinyl alcohol, methyl cellulose, hydroxymethyl cellulose, polyacrylamide and polyethylene glycol.

10. A denitration catalyst prepared by the method according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Honeycomb type SCR denitration catalyst as well as preparation method thereof and equipment

    CN101474565A

  • SCR (Selective catalytic reduction) monolithic honeycombed catalyst for low-temperature flue gas de-nitrification and preparation method thereof

    CN103464194A

  • Low-cost denitration catalyst and preparation process thereof

    CN103495413A

  • Ceramic-based membrane type filter stick and preparation method thereof

    CN111548131A

  • Preparation method of integral honeycomb denitration catalyst

    CN114011401A

Cited By

  • Preparation method of regenerated glass fiber suitable for denitration catalyst and denitration catalyst

    CN121202460A

  • Preparation method of regenerated glass fiber suitable for denitration catalyst and denitration catalyst