Titanium oxide / copper-indium-sulfur high-efficiency photocatalyst, preparation method and application thereof, immobilized gel ball, and preparation method and application thereof
A high-efficiency titanium oxide/copper indium sulfur photocatalyst was constructed through mercapto acid modification and microwave deposition technology, and alginate was used to form semi-interpenetrating network gel spheres, which solved the problems of low activity of the first-generation photocatalyst and high cost of the second-generation photocatalyst. , achieving efficient catalysis and good reusability.
Patent Information
- Application Number
- CN202410936398.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-10-01
AI Technical Summary
The existing first-generation photocatalyst TiO2 has low catalytic activity due to its wide bandgap and high electron-hole pair recombination rate; the second-generation photocatalyst suffers from high separation and recycling costs and attenuation of catalytic performance, and the immobilized carrier is mechanically Poor strength.
By modifying the TiO2 surface with mercapto acid modifiers and depositing CuInS2 nanoparticles under microwave radiation, we construct a titanium oxide/copper indium sulfur efficient photocatalyst, and use alginate and polymer cross-linking agents to form semi-interpenetrating network gel spheres. Immobilized catalyst to avoid falling off and improve mechanical strength.
It significantly improves the catalytic activity and reusability of the catalyst, improves the mechanical strength and light energy utilization, and enhances the stability and mass transfer performance of the catalyst.
Smart Images

Figure CN118719094A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field related to nano material preparation and immobilization technology, and specifically relates to a titanium oxide / copper indium sulfur high-efficiency photocatalyst and a preparation method and application thereof, and an immobilized gel ball and a preparation method and application thereof. Background Art
[0002] Semiconductor photocatalytic technology is a green and efficient way to solve environmental pollution. So far, the development of photocatalysts has gone through three generations. TiO2 is the most common first-generation photocatalyst due to its stable physical and chemical properties and non-toxicity. However, TiO2 with a wide band gap (3.2eV) has low photon utilization (about 5%) in the visible light range and a high recombination rate of photogenerated electron-hole pairs, which limits its catalytic activity. This is also the main problem of the first-generation single-component photocatalyst.
[0003] In order to solve these problems, TiO2 is coupled with narrow bandgap semiconductors to construct heterojunctions to form second-generation photocatalysts, which can not only increase the active sites and broaden the spectral response in the visible light region, but also inhibit the recombination of electron-hole pairs. CuInS2 is a narrow bandgap ternary semiconductor material with a bandgap of ~1.5eV, excellent stability and a large absorption coefficient (>10 5 cm -1 ). Due to the matching of the energy band structures between TiO2 and CuInS2, visible light can be effectively utilized and interfacial charge transfer can be achieved by constructing a TiO2 / CuInS2 heterojunction. However, conventional preparation methods can only deposit CuInS2 as a sensitizer on the surface of TiO2. The deposited CuInS2 particles tend to agglomerate due to similar forces, and it is difficult to form a uniform morphology and distribution between the two components, which directly affects the charge separation between the two components in the multiphase heterojunction system. The tightly coupled heterojunction based on chemical bonds can control the oriented growth of the interface components to achieve the stability of the interface material structure, improve the charge separation ability and thus enhance the catalytic activity. Mercapto acids contain carboxyl and mercapto groups, respectively, and have high covalent bonding affinity with both TiO2 and CuInS2; further, the "bulk heating" method of direct combination of microwaves and reactant molecules is conducive to the continuous epitaxial growth of CuInS2 in a short time, thereby reducing the surface defect concentration of the material, improving the charge separation efficiency and thus enhancing the catalytic activity of the second-generation photocatalyst. However, for the second-generation photocatalysts, high separation and recovery costs, catalyst leaching problems, and the decay of catalytic performance after recovery are the main drawbacks.
[0004] The third generation photocatalyst formed by fixing the second generation photocatalyst on a carrier can be easily separated from the reaction system. The choice of carrier is the key, not only to avoid the loss of light energy before and after immobilization and the reduction of mass transfer capacity, but also to prevent the catalyst from falling off. Alginate is a natural polysaccharide polymer formed by guluronic acid (G unit) and mannuronic acid (M unit) residues through a 1:4 glycosidic bond. It can be used to prepare transparent gels as catalyst immobilization carriers, effectively avoiding the loss of light energy. However, as a natural polymer, single alginate gel has poor mechanical strength.
[0005] It is very necessary to provide a photocatalyst with high catalytic performance, high mechanical strength and recyclability. Summary of the invention
[0006] The purpose of the present invention is to provide a titanium oxide / copper indium sulfur high-efficiency photocatalyst and a preparation method thereof. After the TiO2 surface is modified with a mercapto acid amphiphilic modifier (M-TiO2), CuInS2 nanoparticles are quickly deposited under microwave radiation in combination with the CuInS2 reaction raw material to prepare a titanium oxide / copper indium sulfur high-efficiency photocatalyst.
[0007] Another object of the present invention is to provide an application of titanium oxide / copper indium sulfur high-efficiency photocatalyst for photocatalytic degradation.
[0008] Another object of the present invention is to provide an immobilized gel ball and a preparation method thereof, wherein a semi-interpenetrating network pre-gel solution formed by alginate and a polymer cross-linking agent is used to disperse the titanium oxide / copper indium sulfur high-efficiency photocatalyst M-TiO2 / CuInS2, and carbonate acidification is used to produce gas and form pores to form channels that are beneficial to the mass transfer of organic pollutants. Finally, ionic cross-linking is performed to strengthen the gel shell to prevent the catalyst from falling off, thereby preparing M-TiO2 / CuInS2 immobilized gel balls.
[0009] The last object of the present invention is to provide an application of immobilized gel spheres for photocatalytic degradation, which not only has high catalytic efficiency but also has good reusability.
[0010] The specific technical solutions of the present invention are as follows:
[0011] A method for preparing a titanium oxide / copper indium sulfur high-efficiency photocatalyst comprises the following steps:
[0012] 1) Surface modification of mesoporous TiO2 by surface modifier;
[0013] 2) In situ preparation of titanium oxide / copper indium sulfur high-efficiency photocatalyst by microwave reflux method.
[0014] In step 1), the surface modifier is selected from ethanethiol, 2-mercaptoacetic acid, 3-mercaptopropionic acid, preferably 3-mercaptopropionic acid;
[0015] Step 1) is specifically as follows: dispersing mesoporous TiO2 in deionized water, adding a surface modifier and stirring, and washing to obtain surface-modified TiO2 (M-TiO2); wherein the concentration of mesoporous TiO2 in deionized water is 1-10 mg / mL, preferably 3.3 mg / mL; the dosage ratio of the surface modifier and deionized water is 5-20 μL / mL, preferably 10 μL / mL; adding the surface modifier and stirring at room temperature, the stirring time is 1-12 hours, preferably 6 hours.
[0016] The preparation method of mesoporous TiO2 is as follows: tetrabutyl titanate (TBOT) is added dropwise to deionized water, the product is washed, dried, ground, and calcined at high temperature to obtain mesoporous TiO2; the volume ratio of tetrabutyl titanate to deionized water is 1:10; the temperature of the high temperature calcination is 300°C, the calcination time is 1 hour, and the heating rate is 1.5°C / min; the high temperature calcination is carried out in an air atmosphere. The drying is natural drying, room temperature drying, and high temperature drying, preferably natural drying.
[0017] In step 2), the surface modified TiO2 (M-TiO2) is dispersed in an ethylene glycol solution, and after adding a copper source, an indium source and a sulfur source, the solution is stirred, subjected to microwave reaction, cleaned and dried to obtain a titanium oxide / copper indium sulfur high-efficiency photocatalyst M-TiO2 / CuInS2.
[0018] In step 2), the surface modified TiO2 (M-TiO2) and ethylene glycol solution are used in a ratio of 3-5 mg / mL;
[0019] In step 2), the mass ratio of the surface modified TiO2 (M-TiO2) to the copper source is 1:(0.0204-0.0684), preferably 1:0.0431;
[0020] In step 2), the molar ratio of the copper source, the indium source and the sulfur source is (0.9-1.1):1:(1-4), preferably 0.95:1:3;
[0021] In step 2), the copper source is CuCl; the indium source is InCl3·4H2O; the sulfur source is selected from thiourea, thioacetamide, L-cysteine hydrochloride, preferably L-cysteine hydrochloride;
[0022] The stirring time after adding the copper source, indium source and sulfur source was 30 min;
[0023] In step 2), the microwave reaction has a power of 200-1000 W, preferably 800 W; a reaction temperature of 180-200° C., preferably 190° C.; and a reaction time of 20-30 min, preferably 25 min.
[0024] After the microwave reaction, the product was washed three times with distilled water and then three times with anhydrous ethanol, and dried in a vacuum oven at 60°C for 6 h to obtain the titanium oxide / copper indium sulfur photocatalyst M-TiO2 / CuInS2.
[0025] The present invention provides a titanium oxide / copper indium sulfur high-efficiency photocatalyst, which is prepared by the above method; the titanium oxide / copper indium sulfur high-efficiency photocatalyst is an amorphous block structure with randomly stacked particles of 10-20nm, and the stacking gaps present a pore structure of 200-1000nm; the surface of the block structure is evenly covered by 50-100nm random spherical nanoparticles.
[0026] The invention provides an application of a titanium oxide / copper indium sulfur high-efficiency photocatalyst in the field of photocatalytic degradation.
[0027] The preparation method of surface-modified M-TiO2 / CuInS2 provided by the present invention utilizes the oxygen affinity of -COOH at one end of the mercapto acid modifier to bind TiO2, and the sulfur affinity of -SH at the other end to connect the sulfide precursor, and then utilizes the bulk heating effect of microwaves to rapidly decompose the sulfide precursor to form CuInS2 nanoparticles with uniform size and morphology deposited on the surface of M-TiO2, thereby constructing a uniform heterogeneous interface of M-TiO2 / CuInS2. The prepared material has an amorphous bulk structure, and the surface is uniformly covered with irregular spherical nanoparticles of about 50nm, which can be used for photocatalytic degradation of dyes.
[0028] The immobilized gel ball provided by the present invention is prepared by using the titanium oxide / copper indium sulfur high-efficiency photocatalyst.
[0029] The present invention provides a method for preparing immobilized gel spheres, comprising the following steps:
[0030] S1, dispersing titanium oxide / copper indium sulfur high-efficiency photocatalyst in water, adding pre-gel reagent and foaming agent to obtain pre-gel dispersion;
[0031] S2, mixing the metal ion aqueous solution and the acid solution to obtain a mixed solution;
[0032] S3. Place the mixed solution in a syringe and drip it into the pre-gel dispersion from a high place. After the mixture is formed into balls, it is solidified and freeze-dried to obtain immobilized gel balls.
[0033] In step S1, the ratio of titanium oxide / copper indium sulfur high-efficiency photocatalyst to water is 1-5 mg / mL, preferably 3 mg / mL;
[0034] In step S1, the mass ratio of the pre-gel reagent to the titanium oxide / copper indium sulfur high-efficiency photocatalyst is 3:1-7:1, preferably 5:1;
[0035] The pre-gel reagent includes alginate and a polymer cross-linking agent;
[0036] The mass ratio of the alginate to the polymer cross-linking agent is 1:1-4:1, preferably 4:1;
[0037] Preferably, the ratio of the alginate to water is 12 mg / mL; the ratio of the polymer cross-linking agent to water is 3 mg / mL;
[0038] The alginate is sodium alginate; the polymer cross-linking agent is selected from polyvinyl pyrrolidone (PVP) and polyvinyl alcohol (PVA), preferably PVP;
[0039] The dosage ratio of the foaming agent to water is 1-30 mg / mL, preferably 15 mg / mL;
[0040] The foaming agent is a carbonate; the foaming agent is preferably CaCO3 or NaHCO3, more preferably NaHCO3;
[0041] In step S2, the metal ion crosslinking agent is a metal ion crosslinking agent containing Ca 2+ , Cu 2+ 、Zn 2+ 、Ni 2+ , Fe 2+ , Mn 2+ An aqueous solution, preferably containing Zn 2+ The mixed solution comprises an aqueous solution of 5% to 15% by mass percentage of metal ions, preferably 10% by mass percentage; the acid solution comprises an acetic acid, citric acid, or gluconolactone solution, preferably an acetic acid solution; the volume concentration of the acid in the mixed solution is 5% to 15%, preferably 10%. The volume ratio of the mixed solution to the pregel dispersion is (3.33-10):1, and the optimal ratio is 5:1.
[0042] In step S2, the inner diameter of the syringe is 2 mm;
[0043] The height refers to a vertical distance of 10 cm from the surface of the pre-gel dispersion liquid;
[0044] The post-balling curing refers to soaking the balls in the pre-gel dispersion for 12 hours after the balls are formed;
[0045] The freeze drying temperature is (-30°C)-(-70°C), and the drying time is 12 hours.
[0046] The invention provides an application of immobilized gel balls in the field of photocatalytic degradation.
[0047] In the present invention, the preparation of M-TiO2 / CuInS2 heterojunction photocatalyst immobilized gel spheres is to disperse the photocatalyst in a semi-interpenetrating network pre-gel solution constructed by alginate and a polymer cross-linking agent, and then further use metal ions as cross-linking agents to strengthen the gel shell to prevent the photocatalyst from falling off; at the same time, a porous interconnected structure is constructed based on the CO2 gas generated by carbonate acidification to form a micro-reaction zone to enrich organic pollutants to increase the catalytic rate. The prepared M-TiO2 / CuInS2 heterojunction photocatalyst immobilized gel spheres can be used for the photocatalytic degradation of dyes.
[0048] The inventors found that by cross-linking with another polymer to form a semi-interpenetrating network gel, not only can the mechanical properties be effectively increased, but it is also beneficial to improve the strength of subsequent ionic cross-linking and prevent the catalyst from falling off. Furthermore, in order to improve the mass transfer performance of pollutants, a porous interconnected structure can be constructed inside the gel to improve the scattering and absorption of light, especially to achieve efficient transmission and enrichment of pollutants to provide active sites for catalytic reactions.
[0049] Compared with the prior art, the surface modification of TiO2 in the method of the present invention helps to construct a uniform M-TiO2 / CuInS2 heterojunction interface, improve the separation efficiency of electrons and holes, and electrons combine with O2 to form O2 - , holes and OH - Combined to form ·OH, resulting in a higher concentration of ·O2 - and ·OH can significantly improve its degradation effect on RhB under visible light irradiation; the immobilization matrix based on alginate is low-cost, green and environmentally friendly, and the hydrogen bonding between it and the polymer cross-linking agent can promote the formation of semi-interpenetrating network gel carrier, which not only improves the cross-linking degree of the gel and reduces the pore size of the gel network, but also facilitates the coordination of the two components with metal ions during the subsequent ionic cross-linking, which can not only improve the mechanical strength of the gel, but also strengthen the catalyst embedding effect and effectively avoid the catalyst from falling off; further, the internal porous interconnected structure formed by the gas production by the foaming method can realize multiple scattering and reflection of light, improve the utilization rate of light energy, and provide a mass transfer channel for organic matter, realizing high-concentration enrichment of organic matter. Compared with the unimmobilized photocatalyst, although the specific surface area is reduced, the semi-interpenetrating network gel carrier with a smaller network pore size combined with the "pore-in-pore" structure formed by the foaming method greatly increases the local organic concentration, effectively increases the substrate concentration, and thus significantly increases the catalytic reaction rate. In general, the prepared M-TiO2 / CuInS2 heterojunction photocatalyst immobilized gel spheres not only have high catalytic efficiency but also have good reusability. BRIEF DESCRIPTION OF THE DRAWINGS
[0050] Figure 1The SEM (a) and TEM (b) images of the M-TiO2 / CuInS2 heterojunction prepared in Example 1, wherein the SEM (c) and TEM (d) images of pure TiO2 and the SEM (e) and TEM (f) images of pure CuInS2 are used for comparison.
[0051] Figure 2 This is the XRD pattern of the M-TiO2 / CuInS2 heterojunction prepared in Example 1;
[0052] Figure 3 The UV-visible diffuse reflectance spectrum of the M-TiO2 / CuInS2 heterojunction prepared in Example 1, wherein the inset is the band gap calculated using the direct band gap method;
[0053] Figure 4 The transient photocurrent-time (It) curve (a) and electrochemical impedance spectroscopy EIS (b) of the M-TiO2 / CuInS2 heterojunction prepared in Example 1;
[0054] Figure 5 The photodegradation curve of RhB of the M-TiO2 / CuInS2 heterojunction prepared in Example 1 changes with time;
[0055] Figure 6 This is the XRD pattern of the M-TiO2 / CuInS2 immobilized gel spheres prepared in Example 1;
[0056] Figure 7 FT-IR image of the M-TiO2 / CuInS2 immobilized gel spheres prepared in Example 1;
[0057] Figure 8 The SEM surface (a) and cross-sectional (b) morphologies of the M-TiO2 / CuInS2 immobilized gel spheres prepared in Example 1;
[0058] Fig. 9 This is a curve diagram showing the photodegradation of RhB by the M-TiO2 / CuInS2 immobilized gel spheres prepared in Example 1 over time;
[0059] Fig.10 This is a curve diagram of repeated photodegradation of RhB by the M-TiO2 / CuInS2 immobilized gel spheres prepared in Example 1;
[0060] Fig.11 The SEM (a) and TEM (b) images of TiO2 / CuInS2 prepared in Comparative Example 1, wherein the SEM (c) and TEM (d) images of M-TiO2 / CuInS2 prepared in Example 1 are used for comparison;
[0061] Fig.12The transient photocurrent-time (It) curve (a) and electrochemical impedance spectroscopy EIS (b) of TiO2 / CuInS2 prepared in Comparative Example 1;
[0062] Fig.13 This is a curve diagram showing the change of RhB photodegradation over time at the TiO2 / CuInS2 heterojunction prepared in Comparative Example 1;
[0063] Fig.14 This is a curve diagram showing the photodegradation of RhB by the M-TiO2 / CuInS2 immobilized gel spheres prepared in Comparative Example 2 over time;
[0064] Fig.15 This is a curve chart of the repeated degradation of RhB by the M-TiO2 / CuInS2 immobilized gel spheres prepared in Comparative Example 3. DETAILED DESCRIPTION
[0065] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0066] Unless otherwise specified, the test materials and reagents used in the following examples can be obtained from commercial sources.
[0067] If no specific techniques or conditions are specified in the examples, they can be carried out according to the techniques or conditions described in the literature in the art or according to the product instructions.
[0068] The sodium alginate used in the present invention has a purity of CP (chemically pure), and the PVP has a purity of GR (super pure).
[0069] Example 1
[0070] A method for preparing a titanium oxide / copper indium sulfur high-efficiency photocatalyst comprises the following steps:
[0071] 1) Take 5mL of tetrabutyl titanate and add it dropwise to 50mL of water, age it for 24h, wash it repeatedly with deionized water and dry it naturally, and finally calcine it at 300℃ for 1h with a heating rate of 1.5℃ / min to obtain mesoporous TiO2. Disperse 0.1g of mesoporous TiO2 in 30mL of deionized water solution, add 300μL of 3-mercaptopropionic acid and stir for 6h, centrifuge the product at 10000rpm for 5min, wash the obtained product once with deionized water and then once with ethylene glycol to obtain surface-modified TiO2 (M-TiO2).
[0072] 2) 0.1g M-TiO2 was dispersed in 30mL ethylene glycol solution, and CuCl, InCl3·4H2O and L-cysteine hydrochloride were added in the molar ratio of 0.95:1:3, and the mass ratio of surface-modified TiO2 (M-TiO2) and CuCl was 1:0.0431, so that the theoretically generated CuInS2 accounted for 10% of the total mass of M-TiO2 / CuInS2. After being fully stirred for 30min, the mixed solution was transferred to a microwave reactor and reacted at a power of 800W and a temperature of 190°C for 25min. The obtained product was centrifuged at 10000rpm for 5min, and the obtained product was first washed three times with distilled water, then washed three times with anhydrous ethanol, and dried in a vacuum oven at 60°C for 6h to obtain M-TiO2 / CuInS2.
[0073] For comparison, pure TiO2 and pure CuInS2 were synthesized separately. The synthesis method of pure TiO2 is as follows: 5 mL of tetrabutyl titanate was added dropwise to 50 mL of water, aged for 24 h, washed repeatedly with deionized water and dried naturally, and calcined at 300 °C for 1 h at a heating rate of 1.5 °C / min.
[0074] The synthesis method of pure CuInS2 is as follows: CuCl, InCl3·4H2O and L-cysteine hydrochloride in a molar ratio of 0.95:1:3 are fully stirred for 30 minutes and then transferred to a microwave reactor to react for 25 minutes at a power of 800 W and a temperature of 190°C. The product is obtained after centrifugation, washing and drying.
[0075] A method for preparing immobilized gel spheres using the above-mentioned M-TiO2 / CuInS2, specifically: taking 30 mg of M-TiO2 / CuInS2 and adding it to 10 mL of water, after uniform dispersion by ultrasonication for 10 minutes, adding a mixture of 120 mg of sodium alginate (SA), 30 mg of polyvinyl pyrrolidone (PVP) and 150 mg of NaHCO3 to the above-mentioned dispersion, and continuously stirring for 2 hours to form a uniform pre-gel dispersion. Also prepare 50 mL of a mixed solution of ZnCl2 and CH3COOH, with a ZnCl2 mass ratio of 10% and a CH3COOH volume ratio of 10%, and transfer the mixture to a syringe with an inner diameter of 2 mm. The mixed solution is dripped into the pre-gel dispersion at a height of 10 cm, and the volume ratio of the mixed solution to the pre-gel dispersion is 5:1. After forming the spheres, they are immersed in the pre-gel dispersion for curing for 12 hours. After the surface of the gel spheres is fully rinsed with deionized water, the gel spheres are transferred to a low-temperature freeze dryer and freeze-dried at -70°C for 12 hours to obtain M-TiO2 / CuInS2 heterojunction immobilized gel spheres.
[0076] SEM ( Figure 1 a) and TEM( Figure 1 As shown in the figure (b), the prepared material is a giant amorphous block structure, and the surface of the structure is evenly covered with irregular spherical nanoparticles of about 50nm. For comparison, the SEM ( Figure 1 c) and TEM( Figure 1 d) shows that it is composed of 10-20nm spherical particles randomly stacked, and the stacking gap is a pore structure of 200-1000nm; SEM ( Figure 1 e) and TEM( Figure 1 (f) shows that the particles are 50 nm in diameter and are distributed in a stacked manner. Obviously, the formation of the heterojunction achieves close contact between the two components and uniform distribution of the components.
[0077] Figure 2 This is the XRD diffraction spectrum of the M-TiO2 / CuInS2 sample. From the XRD spectrum, it can be seen that obvious diffraction peaks appear at 2θ=25.20°, 37.94°, 48.05°, 53.89°, 55.01° and 62.62°, corresponding to the (101) plane, (004) plane, (200) plane, (105) plane, (211) plane and (204) plane of anatase TiO2 (JCPDS21-1272), and at 2θ=27.88°, 46.31°, corresponding to the (112) and (204) crystal planes of chalcopyrite CuInS2 (JCPDS 32-0339). The presence of TiO2 and CuInS2 components in XRD confirms the successful synthesis of the heterojunction.
[0078] Figure 3 This is the UV-visible diffuse reflectance spectrum of the M-TiO2 / CuInS2 sample. The absorption range of M-TiO2 / CuInS2 is 200-800nm, and the band edge is at 500-510nm, which is wider than that of pure TiO2 and pure CuInS2. The inset is the optical band gap calculated using the Tauc plot method, which is 2.20eV for M-TiO2 / CuInS2, between pure TiO2 (3.14eV) and pure CuInS2 (1.50eV). Obviously, the construction of the M-TiO2 / CuInS2 heterojunction expands the light absorption range.
[0079] Figure 4Figure a is the transient photocurrent (It) curve of TiO2, CuInS2 and M-TiO2 / CuInS2, which clearly shows the current changes of each sample under light and dark environments. Whenever the xenon lamp is turned on, all samples can quickly generate significant transient photocurrent, and when the light source is turned off, the photocurrent drops rapidly. Compared with TiO2 and CuInS2, M-TiO2 / CuInS2 shows the highest photocurrent intensity, indicating that the material can efficiently separate photogenerated electrons and holes under light conditions. Figure 4 Figure b shows the electrochemical impedance spectra (EIS) of TiO2, CuInS2 and M-TiO2 / CuInS2. The diameter of the semicircle (or arc) in the figure provides information on charge transfer. Generally speaking, a small diameter represents a low charge transfer resistance (R ct ). Compared with TiO2 and CuInS2, M-TiO2 / CuInS2 has the smallest arc radius in EIS, which indicates that the lifetime of photogenerated carriers in this sample is longer. The equivalent circuit was drawn by ZView fitting, and the impedance of TiO2 was calculated to be 37478Ω, the impedance of CuInS2 was 44214Ω, and the impedance of M-TiO2 / CuInS2 was 12747Ω. This shows that the construction of heterojunction can effectively reduce the charge transfer resistance and improve the charge separation ability.
[0080] An application of titanium oxide / copper indium sulfur high-efficiency photocatalyst, the specific photodegradation experiment is carried out according to the following steps: 30 mg of the synthesized M-TiO2 / CuInS2 heterojunction photocatalyst, pure TiO2 and pure CuInS2 are suspended in 50 mL of 60 mg / L RhB solution. Stir and ultrasonicate for 10 minutes to obtain a homogeneous dispersion. Take out 3 mL of the suspension from the system at regular intervals, centrifuge to remove the photocatalyst particles, and use a UV-visible spectrophotometer to detect the maximum absorbance change of RhB (λ=554 nm). With the reaction time as the horizontal axis, the absorbance value (C t ) and the absorbance of the system before the reaction (C0) were plotted as the ordinate. Before photodegradation, the suspension was placed in the dark for 30 min to reach adsorption-desorption equilibrium. The photoreaction was carried out under AM1.5 sunlight emitted by a 300W xenon lamp equipped with a CUT420 filter. The adsorption rate and degradation rate were calculated by the ratio of (C0-C0) under dark reaction and photoreaction, respectively. t The distance between the xenon lamp and the reaction cell is 10 cm, and the intensity is about 220 mW / cm 2 To prevent the temperature from rising, the system was cooled with circulating water. The photocatalytic performance of the prepared samples can be evaluated by the degradation degree of RhB. Figure 5This is the photodegradation curve of M-TiO2 / CuInS2 for RhB. The adsorption rate is about 50% in the dark reaction for 30 minutes (of which the adsorption equilibrium is basically reached in about 10 minutes), and the total degradation rate is 99.9% in 40 minutes under light. Compared with the total degradation rate of 25% for pure TiO2 and pure CuInS2, its degradation rate is significantly improved.
[0081] Figure 6 This is the XRD of the M-TiO2 / CuInS2 immobilized gel sphere. From the XRD spectrum, it can be seen that SA and PVP both have broad diffraction peaks at 2θ=11~37° and 38~47°, which are derived from the amorphous state formed by SA and PVP. When M-TiO2 / CuInS2 is immobilized, the diffraction peak at 2θ=25.20° corresponds to the (101) plane of anatase TiO2, while the diffraction peaks at 2θ=27.88°, 46.31°, and 54.94° correspond to the (112), (204), and (312) crystal planes of chalcopyrite CuInS2, indicating that M-TiO2 / CuInS2 is successfully immobilized on the SA / PVP gel.
[0082] Figure 7 This is the diffuse reflectance infrared spectrum of M-TiO2 / CuInS2 immobilized gel spheres. It can be observed that 3519cm -1 The broad peak near 2931cm -1 、1608cm -1 、1417cm -1 、1034cm -1 The characteristic peaks of SA correspond to the stretching vibration of -OH, CH, asymmetric stretching vibration and symmetric stretching vibration of C=O in the carboxyl group, and stretching vibration of CO. -1 ,2973cm -1 ,1635cm -1 ,1423cm -1 and 1292cm -1 The peaks at 1656 cm correspond to the stretching vibration of -OH, the stretching vibration of CH, the stretching vibration of C=O in the pyrrole ring, the bending vibration of CH and the bending vibration of CN in the pyrrole ring. The stretching vibration of the carboxyl group in the SA / PVP mixed gel shifts to a high wavenumber of 1656 cm -1 , and the -OH stretching vibration peak is 3446cm -1 narrowed, indicating that hydrogen bonds were formed between SA and PVP. -1 The Ti-O stretching vibration peak appeared at , indicating the successful immobilization of M-TiO2 / CuInS2 on SA / PVP gel.
[0083] Figure 8 The surface (a) and cross-section (b) morphologies of the M-TiO2 / CuInS2 immobilized gel spheres. Many particles can be observed attached to the surface, which are M-TiO2 / CuInS2 photocatalysts. In addition, there are many dispersed pores ( Figure 8 In a), the cross section shows a highly dispersed porous structure that is well connected to each other, with the diameter of the macropores formed being about 100-500 μm ( Figure 8 (b)
[0084] Fig. 9 The photocatalytic degradation performance of M-TiO2 / CuInS2 immobilized gel spheres on RhB in water under visible light was shown. The adsorption rate of the immobilized gel spheres in the dark reaction for 30 minutes was 28%, which was lower than the adsorption rate of the M-TiO2 / CuInS2 heterojunction (50%). However, the degradation rate of RhB after 20 minutes of illumination reached 99.9%, which was significantly improved compared with the degradation rate of the M-TiO2 / CuInS2 heterojunction for 20 minutes (88.8%), and the time for complete degradation was almost halved. This is mainly due to the "pore-in-pore" structure formed by the simultaneous acidification and gasification of SA and PVP cross-linking, which is conducive to the transfer and transportation of organic matter, achieving pollutant concentration enrichment and increasing substrate concentration, thereby improving the photocatalytic efficiency.
[0085] Fig.10 This is the absorbance change curve of the nine-time repeated degradation of RhB by M-TiO2 / CuInS2 immobilized gel spheres. The repeated degradation experiment was carried out according to the following steps: After each photodegradation, the immobilized gel spheres were placed in distilled water and soaked for 6 hours to remove the dye molecules adsorbed on the surface. After freeze-drying for 12 hours, the photocatalytic degradation reaction was carried out again. As can be seen from the figure, the degradation rate of the first eight times under light irradiation can reach 99.9%. After the ninth repeated degradation, the degradation efficiency can still be maintained at 99.34% (the adsorption rate of the dark reaction for 60 minutes is maintained between 25-35%), indicating that the immobilized gel spheres have good reusability.
[0086] Comparative Example 1
[0087] A method for preparing a photocatalyst comprises the following steps:
[0088] 5 mL of tetrabutyl titanate was added dropwise to 50 mL of water, aged for 24 h, washed repeatedly with deionized water and dried naturally, and finally calcined at 300 ° C for 1 h, with a heating rate of 1.5 ° C / min to obtain mesoporous TiO2. 0.1 g of mesoporous TiO2 was dispersed in 30 mL of ethylene glycol solution, and CuCl, InCl3·4H2O and L-cysteine hydrochloride were added in a molar ratio of 0.95:1:3 in sequence, and the mass ratio of mesoporous TiO2 to CuCl was 1:0.0431. After being fully stirred for 30 min, the mixed solution was transferred to a microwave reactor and reacted at a power of 800 W and a temperature of 190 ° C for 25 minutes. The obtained product was centrifuged at 10000 rpm for 5 min, washed three times with distilled water, and then washed three times with anhydrous ethanol, and dried in a vacuum oven at 60 ° C for 6 h to obtain TiO2 / CuInS2.
[0089] Fig.11 This is the SEM of TiO2 / CuInS2 ( Fig.11 In the SEM (a) and TEM (b) of Example 1, the prepared TiO2 is a giant block structure with holes distributed on the surface. CuInS2 is 50nm nanoparticles randomly accumulated on the surface of the block structure, partially aggregated, and some areas are not effectively covered. Compared with the SEM ( Fig.11 c) and TEM( Fig.11 Compared with (d), the deposition of CuInS2 on the TiO2 surface is less uniform.
[0090] Fig.12 Figure a is the It curve of TiO2 / CuInS2, and its photocurrent intensity is significantly lower than that of M-TiO2 / CuInS2; Fig.12 Figure b is the EIS spectrum of TiO2 / CuInS2. Compared with M-TiO2 / CuInS2, M-TiO2 / CuInS2 has a larger arc radius, indicating that the lifetime of photogenerated carriers in this sample is shorter. The impedance of TiO2 / CuInS2 obtained by ZView fitting of the equivalent circuit is 16309Ω, which is larger than the impedance of M-TiO2 / CuInS2 (12747Ω), indicating that the charge transfer resistance of TiO2 / CuInS2 is large and the charge separation ability is weak. Fig.13 This is the photodegradation curve of TiO2 / CuInS2 for RhB, and the degradation rate is 99.9% after 60 minutes of illumination. Obviously, the photocatalytic degradation ability of TiO2 / CuInS2 for RhB is significantly weaker than that of M-TiO2 / CuInS2 heterojunction (the degradation rate is 99.9% after 40 minutes), which may be due to the fact that the randomly stacked CuInS2 on the TiO2 surface fails to form an effective and uniform interface between the two, resulting in a lower charge separation ability.
[0091] Comparative Example 2
[0092] A method for preparing immobilized gel spheres comprises the following steps:
[0093] Take 30mg of the M-TiO2 / CuInS2 synthesized in Example 1 and add it to 10mL of water. After uniform dispersion by ultrasonic treatment for 10min, add 120mg of SA and 30mg of PVP mixture to the above dispersion and continue stirring for 2h to form a uniform gel dispersion. Prepare 50mL of 10% ZnCl2 solution by mass and transfer it to a syringe. Take the volume ratio of ZnCl2 solution to pre-gel dispersion as 5:1, drop the ZnCl2 solution into the pre-gel dispersion at a height of 10cm, and solidify for 12h. Rinse the surface of the gel ball with deionized water and transfer it to a low-temperature freeze dryer and freeze-dry at -70℃ to obtain M-TiO2 / CuInS2 heterojunction immobilized gel ball.
[0094] Fig.14 This is the photodegradation curve of RhB by the non-gas-producing pore-forming gel ball prepared in Example 2. The adsorption rate in the dark reaction for 30 minutes is 10%, and the degradation rate in the light reaction for 20 minutes is only 38%. Compared with the catalytic performance of the gas-producing pore-forming gel ball in Example 1 (the degradation rate in 20 minutes is 99.99%), it is significantly reduced, indicating that acidification gas production and pore formation play a vital role in the catalytic performance.
[0095] Comparative Example 3
[0096] A method for preparing immobilized gel spheres comprises the following steps:
[0097] Take 30mg of the M-TiO2 / CuInS2 synthesized in Example 1 and add it to 10mL of water. After uniform dispersion by ultrasonic treatment for 10min, add 120mg of SA and 150mg of NaHCO3 to the above dispersion and continue stirring for 2h to form a uniform gel dispersion. Prepare 50mL of a mixed solution of ZnCl2 and CH3COOH, with a ZnCl2 mass ratio of 10% and a CH3COOH volume ratio of 10%. After mixing, transfer to a syringe. The volume ratio of the mixed solution to the pre-gel dispersion is 5:1. Drop the mixed solution into the pre-gel dispersion at a height of 10cm and solidify for 12h. Rinse the surface of the gel ball with deionized water and transfer it to a low-temperature freeze dryer and freeze-dry at -70℃ to obtain the M-TiO2 / CuInS2 heterojunction immobilized gel ball.
[0098] Fig.15This is the repeated photodegradation curve of RhB by the gel ball prepared in comparative example 3, the first photodegradation rate is 93.41% (dark reaction adsorption rate is 47.09%), the second photodegradation rate is 93.57% (dark reaction adsorption rate is 50.78%), the third photodegradation rate is 97.08% (dark reaction adsorption rate is 54.58%), the fourth photodegradation rate is 85.01% (dark reaction adsorption rate is 40.83%), and the fifth photodegradation rate is 69.69% (dark reaction adsorption rate is 34.65%). Obviously, with the increase of degradation times, the degradation performance is significantly reduced, indicating that the reusability of the SA-immobilized gel ball alone is not ideal.
[0099] The present invention utilizes a mercapto acid amphiphilic modifier to functionalize the surface thiol of TiO2, and based on covalent action and combined with the microwave "bulk heating" characteristics, homogeneously and in situ grows CuInS2 nanoparticles on the surface of TiO2 to construct a uniform and closely contacted M-TiO2 / CuInS2 heterojunction. The heterojunction with a uniform interface can effectively improve the charge separation efficiency and accelerate the photodegradation reaction rate. After M-TiO2 / CuInS2 is dispersed by a semi-interpenetrating network pre-gel solution constructed by alginate and a polymer cross-linking agent, the gel shell is further strengthened by cross-linking with metal ions to prevent the photocatalyst from falling off; at the same time, a porous interconnected structure is constructed based on the CO2 gas generated by carbonate acidification to form a micro-reaction zone to enrich organic pollutants to improve the catalytic rate. The equipment used in the method of the present invention to prepare the photocatalyst material is simple and the reaction is rapid. The interface between the two materials is evenly distributed, which significantly improves the photodegradation effect of a single material under visible light irradiation; the matrix used for the immobilization of the photocatalyst is green and environmentally friendly, and the prepared gel ball not only improves the reusability of the catalyst, but also greatly improves the catalytic efficiency of the powder catalyst.
[0100] The description of the above embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the protection scope of the present invention.
Claims
1. A method for preparing a titanium oxide / copper indium sulfur high-efficiency photocatalyst, characterized in that: The steps include: 1) Surface modification of mesoporous TiO2 by surface modifiers; 2) In-situ preparation of titanium oxide / copper indium sulfur high-efficiency photocatalyst by microwave reflux method; The surface modifier is selected from ethanethiol, 2-mercaptoacetic acid, and 3-mercaptopropionic acid, preferably 3-mercaptopropionic acid.
2. The preparation method according to claim 1, characterized in that: Step 1) is specifically as follows: dispersing mesoporous TiO2 in deionized water, adding a surface modifier, stirring, and washing to obtain surface-modified TiO2 (M-TiO2); wherein the concentration of mesoporous TiO2 in deionized water is 1-10 mg / mL, and the dosage ratio of the surface modifier to deionized water is 5-20 μL / mL.
3. The preparation method according to claim 1, characterized in that: In step 2), the surface-modified TiO2 (M-TiO2) is dispersed in an ethylene glycol solution, and after adding a copper source, an indium source and a sulfur source, the solution is stirred, subjected to microwave reaction, cleaned and dried to obtain a titanium oxide / copper indium sulfur high-efficiency photocatalyst M-TiO2 / CuInS2; in step 2), the microwave reaction has a power of 200-1000 W, a reaction temperature of 180-200°C and a reaction time of 20-30 min.
4. A titanium oxide / copper indium sulfur high-efficiency photocatalyst prepared according to any one of claims 1 to 3, characterized in that: The titanium oxide / copper indium sulfur high-efficiency photocatalyst is an amorphous block structure with randomly stacked particles of 10-20nm, and the stacking gaps present a pore structure of 200-1000nm; the surface of the block structure is evenly covered by randomly stacked spherical nanoparticles of 50-100nm.
5. An application of the titanium oxide / copper indium sulfur high-efficiency photocatalyst according to claim 4, characterized in that: Used for photocatalytic degradation.
6. An immobilized gel ball, characterized in that: The method is prepared using the titanium oxide / copper indium sulfur high-efficiency photocatalyst described in claim 4.
7. A method for preparing the immobilized gel spheres according to claim 6, characterized in that: The preparation method comprises the following steps: S1, dispersing titanium oxide / copper indium sulfur high-efficiency photocatalyst in water, adding pre-gel reagent and foaming agent to obtain pre-gel dispersion; S2, mixing the metal ion aqueous solution and the acid solution to obtain a mixed solution; S3. Place the mixed solution in a syringe and drip it into the pre-gel dispersion from a high place. After the mixture is formed into balls, it is solidified and freeze-dried to obtain immobilized gel balls.
8. The preparation method according to claim 7, characterized in that: In step S1, the mass ratio of the pregel reagent to the titanium oxide / copper indium sulfur high-efficiency photocatalyst is 3:1-7:1, and the pregel reagent includes alginate and a polymer cross-linking agent; the mass ratio of the alginate to the polymer cross-linking agent is 1:1-4:
1.
9. The preparation method according to claim 8, characterized in that: The foaming agent is carbonate.
10. An application of the immobilized gel spheres according to claim 6, characterized in that: Used for photocatalytic degradation.
Citation Information
Patent Citations
Nano composite photochemical catalyst and application thereof
CN102091643A
Photocatalytic composite gel bead and preparation method as well as application thereof
CN103170373A
Flaky titanium dioxide / bismuth oxybromide composite photocatalyst and preparation method thereof
CN104785280A
Biomass nanomaterial porous microsphere and preparation method thereof
CN113368830A
Nano-selenium sodium alginate composite gel, preparation method therefor and use thereof
WO2023082218A1