Magnetic copper alginate composite microsphere as well as preparation method and application thereof
By designing the core-shell structure of magnetic copper alginate composite microspheres and using copper alginate and chitosan layers to coat ABTS, the problem of ABTS toxicity in pollutant detection and the insufficient mechanical strength of alginate microspheres was solved, achieving Efficient catalytic degradation and recycling.
Patent Information
- Application Number
- CN202410724831.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-05
- Publication Date
- 2024-10-01
AI Technical Summary
In the existing technology, ABTS easily re-enters the environment due to its toxicity during the pollutant detection process, causing secondary environmental pollution. Moreover, simple alginic acid microspheres have insufficient mechanical strength in the catalytic degradation reaction and have a low recycling rate.
Design a magnetic copper alginate composite microsphere, which has a core-shell structure. The core is Fe3O4, and the outer shell is a layer of copper alginate and chitosan. It is prepared by magnetic stirring and curing agent dropping method to form magnetic alginate coated with ABTS. copper microspheres, and a chitosan layer is formed on the surface to enhance strength and protect the microspheres.
It improves the catalytic degradation efficiency, realizes efficient recycling and protection of microspheres, avoids the outflow of magnetic materials and ABTS caused by damage of microspheres, and expands the application scope of ABTS.
Smart Images

Figure CN118719150A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of composite material preparation, and in particular to magnetic copper alginate composite microspheres and a preparation method and application thereof. Background Art
[0002] ABTS (2,2'-azino-bis-3-ethylbenzothiazoline-6-sulfonic acid) is widely used in aqueous dyes (such as reactive blue 19) and oxidants (such as H2O) because it can be oxidized to ABTS radicals via single electron transfer, and because of its excellent spectral properties, solubility in organic and aqueous media, and stability over a wide pH range. 2 O 2 Numerous studies have shown that ABTS exhibits excellent reactivity to a variety of pollutants and is highly reactive in the presence of horseradish peroxidase / H 2 O 2 / ABTS system and laccase / O 2 In the / ABTS system, ABTS·+ has been confirmed to be the main active substance for pollutant degradation in the ABTS-enhanced enzyme catalysis system. Although ABTS shows unique reactivity in pollutant detection, due to its own toxicity, it is very easy to re-enter the environment during use, causing secondary pollution to the environment.
[0003] Chitosan and sodium alginate are natural biopolymer materials that have been widely used in the fields of biomedicine and tissue engineering in recent years. They have good compatibility and degradability, and have little toxicity to the human body. Pure alginate microspheres have weak mechanical strength and are used as carriers of laccase / ABTS mediators in catalytic degradation reactions, but their recycling rate is low.
[0004] In view of this, it is necessary to design an improved magnetic copper alginate composite microsphere and its preparation method and application to solve the above problems. Summary of the invention
[0005] The purpose of the present invention is to provide a magnetic copper alginate composite microsphere and a preparation method and application thereof.
[0006] In order to achieve the above-mentioned object of the invention, on the one hand, the present invention provides a magnetic copper alginate composite microsphere, wherein the composite microsphere is a core-shell structure, wherein the core is Fe 3 O 4 and ABTS, with an outer shell consisting of alginate and chitosan layers;
[0007] The Fe in the composite microspheres 3 O 4 The chitosan layer is coated with ABTS, the copper alginate layer in the shell is close to the ABTS, and the chitosan layer is formed on the outside of the copper alginate layer.
[0008] On the other hand, the present invention also provides a method for preparing the magnetic copper alginate composite microspheres, comprising the following steps:
[0009] S1, adding magnetic soil and ABTS solution to sodium alginate colloid, mixing evenly, to obtain a mixed sol; using a syringe to absorb the mixed sol, dripping it into a curing agent, and under magnetic stirring conditions, obtaining magnetic copper alginate microspheres coated with ABTS;
[0010] S2. Adding the ABTS-coated magnetic copper alginate microspheres obtained in step S1 into a chitosan solution to form a chitosan layer on the surface of the magnetic copper alginate microspheres to obtain magnetic copper alginate composite microspheres.
[0011] As an embodiment of the present invention, in step S2, the chitosan solution is prepared by dissolving chitosan in acetic acid solution, the mass concentration of which is 0.1-0.5%, the molecular weight of chitosan is 100,000-300,000, and the volume concentration of the acetic acid solution is 0.25-3%.
[0012] As an embodiment of the present invention, in step S1, the rotation speed of the magnetic stirring is 200-1000 rpm.
[0013] As an embodiment of the present invention, in step S1, the sodium alginate colloid is formed by dispersing sodium alginate in water, and the mass concentration thereof is 1.5-3%.
[0014] As an embodiment of the present invention, in step S1, the mass concentration of the ABTS solution is 0.1-10%.
[0015] As an embodiment of the present invention, the volume ratio of the added amount of the magnetic soil to the ABTS solution is 1:10-1:60.
[0016] As an embodiment of the present invention, in step S1, the curing agent is CuSO 4 The solution has a concentration of 0.1-1.5M; preferably, the process of adding the mixed sol to the curing agent is carried out at a rate of one drop per second.
[0017] In particular, the magnetic copper alginate composite microspheres prepared by the preparation method of the present invention can be used as a catalyst, and are particularly suitable as a catalyst for a laccase-mediator system.
[0018] The beneficial effects of the present invention are:
[0019] 1. The preparation method of the magnetic copper alginate composite microspheres provided by the present invention comprises the following steps: firstly preparing a copper alginate-coated magnetic material (Fe 3 O 4) and ABTS magnetic copper alginate microspheres, and then a layer of chitosan is loaded on the surface, and finally a magnetic copper alginate composite microsphere is obtained. The above process can use chitosan to enhance the strength of the microspheres, and at the same time use it to protect the copper alginate layer, so as to avoid the composite microspheres from being damaged during use, causing the magnetic material and ABTS inside the microspheres to flow out, affecting the use of the composite microspheres. Through the above method, a magnetic copper alginate composite microsphere with high catalytic degradation efficiency, recyclable and reusable is obtained, which not only solves many defects in the prior art when using ABTS, but also further expands the application range of ABTS.
[0020] 2. The preparation method of the magnetic copper alginate composite microspheres provided by the present invention accurately controls the morphology and composition of the composite microspheres by regulating the concentrations of sodium alginate colloid, ABTS solution and chitosan solution, and the amount of magnetic material added during the preparation process, and finally obtains round composite microspheres in the form of a core-shell structure. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is an optical photograph of ABTS-loaded magnetic copper alginate composite microspheres prepared in Example 1 of the present invention;
[0022] Figure 2 This is a SEM image of the magnetic copper alginate composite microspheres prepared in Example 1 of the present invention;
[0023] Figure 3 is the SEM image of magnetic copper alginate microspheres without ABTS;
[0024] Figure 4 FTIR image of the magnetic copper alginate composite microspheres prepared in Example 1 of the present invention;
[0025] Figure 5 This is an EDS image of the surface of the magnetic copper alginate composite microspheres prepared in Example 1 of the present invention;
[0026] Figure 6 for Figure 5 EDS image of the cross section of magnetic copper alginate composite microspheres;
[0027] Figure 7 : is a hysteresis loop diagram of the magnetic copper alginate composite microspheres prepared in Example 1 of the present invention;
[0028] Figure 8 This is a standard curve of ABTS peak area-concentration of magnetic copper alginate composite microspheres prepared in Example 1 of the present invention;
[0029] Fig. 9 This is a graph showing the cyclic degradation of Reactive Blue 19 by the magnetic copper alginate composite microspheres prepared in Example 1 of the present invention;
[0030] Fig.10 These are optical photographs of the magnetic copper alginate composite microspheres prepared in Examples 1 and 7 of the present invention. DETAILED DESCRIPTION
[0031] In order to make the purpose, technical solutions and advantages of the present invention more clear, the present invention is described in detail below with reference to the accompanying drawings and specific embodiments.
[0032] It should also be noted that, in order to avoid obscuring the present invention due to unnecessary details, only structures and / or processing steps closely related to the scheme of the present invention are shown in the drawings, while other details that are not closely related to the present invention are omitted.
[0033] In addition, it should be noted that the terms "comprises", "includes" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or apparatus that includes a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or apparatus.
[0034] The present invention provides a magnetic copper alginate composite microsphere, which has a core-shell structure and a core of Fe 3 O 4 The outer shell is a copper alginate layer and a chitosan layer; the center of the composite microsphere is Fe 3 O 4 , the copper alginate cavity in the shell is coated with ABTS, the thickness of the chitosan layer is less than 5 μm, and the thickness of the copper alginate layer is about 0.5-1.5 mm.
[0035] Furthermore, the present invention also provides a method for preparing the magnetic copper alginate composite microspheres, comprising the following steps:
[0036] S1. Preparation of magnetic copper alginate microspheres coated with ABTS: adding magnetic soil and ABTS solution to sodium alginate colloid, mixing evenly, and preparing a mixed sol; using a syringe to absorb the mixed sol, dripping it into a curing agent, and preparing magnetic copper alginate microspheres coated with ABTS under magnetic stirring conditions;
[0037] S2. Preparation of magnetic copper alginate composite microspheres: adding the ABTS-coated magnetic copper alginate microspheres prepared in step S1 into a chitosan solution to form a chitosan layer on the surface of the magnetic copper alginate microspheres to prepare magnetic copper alginate composite microspheres.
[0038] As an embodiment of the present invention, in step S1, the mass concentration of the ABTS solution is 0.1-10% (w / v); the magnetic soil is a self-made magnetic material, which is obtained by ball milling chromium slag and disintegrant with water and then separating the magnetic material with an electromagnet, and its main component is Fe3 O 4 The ratio of the amount of magnetic soil added (g) to the volume of ABTS solution (mL) is 1:10-1:60. By controlling the magnetic soil within the above range, it is not only beneficial to give the composite microspheres magnetic properties, but also does not affect the formation of microspheres. When the amount of magnetic soil added is too large, there are too many particulate substances in the mixed sol, which is not conducive to the formation of microspheres.
[0039] As an embodiment of the present invention, in step S1, the sodium alginate colloid is formed by dispersing sodium alginate in water, and its mass concentration is 1.5-3% (w / v). In the above process, by adjusting the concentration of the sodium alginate colloid, the size of the microspheres can be precisely controlled, and at the same time, by controlling the amount of magnetic soil added, its distribution state in the microspheres is ensured.
[0040] As an embodiment of the present invention, in step S1, the mixed sol is dripped into the curing agent at a rate of one drop per second; the curing agent is CuSO 4 The solution has a concentration of 0.1-1.5 M. The mixed sol is dropped into CuSO 4 After being in the solution, the Na ions in the sodium alginate exchange with the Cu ions and solidify to form the cavity structure of copper alginate. ABTS is likely to remain on the copper alginate due to electrostatic effects or other chemical bonds, and is not just wrapped around the outside of the magnetic material. ABTS and copper alginate are equivalent to being compounded together to form an ABTS@copper alginate layer and a chitosan layer.
[0041] As an embodiment of the present invention, in step S1, the speed of magnetic stirring is 200-1000rpm, and the stirring time is 0.5-3h. In this way, after the mixed sol is dripped into the curing agent, the mixed sol and the curing agent are in contact more fully, which is conducive to promoting the rapid formation of gel, and is also conducive to the formation and solidification of microspheres; secondly, under the condition of magnetic stirring, the morphology of the microspheres can be regulated, and the magnetic soil can be agglomerated and nucleated in the microspheres. On the other hand, the magnetic materials themselves will attract each other, and the conditions of magnetic stirring can accelerate the occurrence of the above process. At a specific speed, it is not only conducive to the formation of microspheres, but also can regulate the position of the magnetic material in the microspheres. It is found in the experimental process that when the magnetic material is located at the center of the microsphere, the contact probability and contact area of ABTS in the microsphere with the external catalytic substance to be catalyzed are increased, which is conducive to improving the catalytic efficiency; in addition, when the magnetic material is distributed in the center of the microsphere, the agglomeration between the microspheres can be avoided to the greatest extent. Furthermore, since magnetic soil is introduced into the microspheres, there is attraction between the microspheres and between the microspheres and the external environment. Therefore, the microspheres are prone to aggregate or be attracted by substances such as iron in the environment during use, which affects their normal use. By regulating the microsphere formation process, the magnetic soil can be promoted to agglomerate and nucleate in the microspheres, which can weaken the mutual attraction between the magnetic soils in adjacent microspheres to a certain extent, avoiding the introduction of magnetic materials into the microspheres, which will affect their normal use.
[0042] As an embodiment of the present invention, in step S2, the chitosan solution is prepared by dissolving chitosan in acetic acid solution, the mass concentration of the chitosan solution is 0.1-0.5% (w / v), the time the microspheres are in the chitosan solution is 15-50 min, the molecular weight of chitosan is 100,000-300,000, and the volume concentration of the acetic acid solution is 0.25-3% (v / v).
[0043] In the above process, by forming a layer of chitosan on the surface of the microspheres, not only can the adsorption of reactive blue 19 be utilized to increase the contact of the mediator ABTS with the reactive dye, thereby accelerating the catalytic efficiency, but also the microspheres can be protected to prevent the microspheres from being damaged during use, causing the internal ABTS and magnetic materials to flow out, affecting the normal use of the composite microspheres. When the concentration of chitosan is too high, the chitosan layer is too thick, which is not conducive to the contact between ABTS and the reactive dye, affecting the degradation efficiency; when the concentration is too low, the chitosan layer is not thick enough, which is not conducive to protecting the ABTS and magnetic materials inside the microspheres.
[0044] As an embodiment of the present invention, in step S2, in order to make the magnetic copper alginate microspheres fully contact with the chitosan solution and ensure the uniformity of the chitosan layer, it can be carried out under the condition of mechanical stirring or magnetic stirring. Preferably, the stirring time is 10-50 minutes. In other embodiments, the stirring time can also be adjusted as needed, as long as it is set according to the needs, and this is not limited here.
[0045] Furthermore, the magnetic copper alginate composite microspheres prepared by the preparation method of the present invention can be used as a catalyst, and are particularly suitable as a catalyst for a laccase-mediator system.
[0046] The following is a further description of the magnetic copper alginate composite microspheres and their preparation method and application provided by the present invention in conjunction with specific embodiments:
[0047] Example 1
[0048] This embodiment prepares a magnetic copper alginate composite microsphere, and its specific preparation method includes the following steps:
[0049] S1. Add 2.5 g of light yellow sodium alginate powder into 100 mL of deionized water several times, stir mechanically for 2 h, and then ultrasonicate for 10 min to accelerate the dissolution of the sodium alginate powder and promote the discharge of bubbles generated during the dissolution process. The temperature of the ultrasonication process is 25 ° C and the frequency is 50 Hz; then, let it stand at 5 ° C to ensure that the bubbles in the sodium alginate colloid are completely removed;
[0050] 50 mg of magnetic clay and 2 mL of 2.2 mg / mL ABTS solution were added to 8 mL of the above sodium alginate colloid in several portions, mechanically stirred until the particles were evenly dispersed, and ultrasonicated at 50 Hz for 10 min to remove bubbles, to prepare a mixed sol;
[0051] Use a 5 mL syringe to draw the mixed sol and add it to the 1 M CuSO solution at a rate of one drop per second. 4 The solution was stirred magnetically at 340 rpm for 1 h at a power of 10 W to obtain magnetic copper alginate microspheres coated with ABTS;
[0052] S2. Add the ABTS-coated magnetic copper alginate microspheres prepared in step S1 to a chitosan solution with a mass concentration of 0.24%, and stir for 30 minutes to form a chitosan layer on the surface of the magnetic copper alginate microspheres. Then, separate the microspheres with the chitosan layer formed on the surface by filtering, and wash them with deionized water for 5 times to obtain magnetic copper alginate composite microspheres, wherein the thickness of the chitosan layer in the microspheres is less than 5 μm, and the thickness of the copper alginate layer is about 0.5-1.5 mm.
[0053] The chitosan solution is obtained by dissolving 0.12g chitosan in 50mL 1% acetic acid solution, and the molecular weight of chitosan is 100,000-300,000. The filtrate and washing liquid of this process are used for the subsequent determination of the immobilization rate of ABTS in the composite microspheres. It should be noted that the magnetic stirring process of this embodiment is carried out using a digital display constant temperature magnetic stirrer model B11-3 purchased from Shanghai Si Le Instrument Co., Ltd. In addition, the reagents used in the embodiments of the present invention can be purchased on the market unless otherwise specified.
[0054] The optical photograph of the magnetic copper alginate composite microspheres prepared in this example is as follows: Figure 1 As shown in the figure, it can be observed that the microspheres are core-shell structures, and the center is black Fe 3 O 4 , the microspheres are spherical with uniform size. Composite microspheres (Fe 3 O 4 -CS-SA@ABTS) Figure 2 As shown in a, it can be clearly seen that the composite microspheres are core-shell structures, and Fe 3 O 4 Located in the center of the sphere, copper alginate serves as the shell of the sphere, and ABTS is coated in the cavity of copper alginate. Its specific position in the microsphere is as follows Figure 2 As shown in b; SEM image of microspheres without ABTS Figure 3 As shown, Figure 2 By comparison, it can be found that the Fe content in the microspheres prepared under the two experimental conditions is 3 O 4 can nucleate, but Figure 2 There are wrinkles on the surface of the composite microspheres. This is because ABTS is uncharged. The ABTS on the surface of copper alginate hinders the electrostatic interaction between copper alginate and chitosan, thus forming wrinkles. The appearance of wrinkles effectively increases the surface area of the microspheres, which is beneficial to improving their catalytic properties. The FTIR image of the composite microspheres is shown in Figure 2. Figure 4 As shown, the results showed that ABTS, Fe 3 O 4 , sodium alginate, and chitosan are compounded together; the EDS images of the surface and cross section of the composite microspheres are shown as follows Figure 5 and 6 As shown in the figure, the Fe content of the cross section is significantly higher than that of the surface, which further confirms that Fe 3 O 4 Located in the center of the microsphere.
[0055] In order to explore the Fe 3 O 4 Whether there is an interaction between Fe and ABTS, this example determines 3 O 4-CS-SA@ABTS and Fe 3 O 4 -CS-SA hysteresis loop, such as Figure 7 As shown, the results show that whether ABTS is loaded will not affect the magnetic properties of the composite microspheres, and the composite microspheres can be enriched under the action of an external magnetic field (such as a magnet), which is convenient for recovery and removal from the application environment. In particular, this example also determines the immobilization rate of ABTS in the composite microspheres. The specific determination method is as follows: The peak area corresponding to different concentrations of ABTS is measured by high pressure liquid chromatography, and the obtained Figure 8 The ABTS peak area-concentration standard curve shown in the figure is as follows; the filtrate and the washing liquid in Example 1 are subjected to high pressure liquid phase determination to obtain the peak area corresponding to ABTS, which is brought into the standard curve to obtain the content of ABTS in the filtrate and the 5 washing liquids. The results are shown in the table. After calculation, the immobilization rate of ABTS is 44.34%. The calculation formula of the immobilization rate is as follows: Among them A 0 is the amount of ABTS added during preparation, in mg; C 1 is the concentration of the filtrate and washing liquid measured by high pressure liquid phase during preparation, in ppm; 0.05 is the volume of the filtrate and washing liquid, in L.
[0056]
[0057] Furthermore, this example also explores the catalytic degradation and recyclability of the composite microspheres for reactive blue 19 in the laccase-mediator system. The specific test process is as follows: 2g of the composite microspheres prepared in Example 1 were added with 50mL of reactive blue 19 with an initial concentration of 75ppm, and the reactive blue 19 was catalytically degraded under magnetic stirring conditions until it was nearly colorless when observed with the naked eye, and the absorbance of reactive blue 19 at the characteristic peak of 592nm was measured with an ultraviolet spectrophotometer. After the degradation was completed, the composite microspheres were taken out, washed with deionized water for 3-5 times, and the surface moisture was wiped with filter paper. The catalytic degradation experiment was carried out again. Under the same experimental conditions, the degradation cycle was repeated 5 times. The results are as follows: Figure 8 As shown, the degradation rate of the first time is 95.97%, and the degradation rate of the fifth time is 90.46%. The results show that the composite microspheres prepared in this example can effectively degrade reactive blue 19, and the degradation rate after multiple cycles is still at a high level.
[0058] Examples 2 to 4
[0059] The difference between Examples 2 to 4 and Example 1 is only that: in step S2, the concentration of the chitosan solution is different from that in Example 1, and the other steps are the same as those in Example 1, which will not be repeated here. The performance comparison of the concentration of the chitosan solution used in Examples 1 to 4 and the composite microspheres obtained under the corresponding conditions is shown in Table 2. It can be seen from the data in the table that the catalytic degradation of the composite microspheres is affected by the concentration of the chitosan solution, and under the chitosan concentration given by the present invention, magnetic copper alginate composite microspheres with excellent catalytic degradation efficiency for active blue 19 can be obtained. The catalytic degradation rate in Table 2 is the experimental data of the first round of reaction for 2.5h, and the degradation rate is calculated by measuring the absorbance value of the unknown liquid and the active blue 19 before degradation. It can be seen from the table that the number of cycles in Example 1 and Example 4 of chitosan concentration is better, and the catalytic degradation efficiency of the two is close. Since CS is lighter and not easy to dissolve, a lower concentration of chitosan solution can be appropriately selected in the preparation process.
[0060] Table 2 Concentration of chitosan solution used in Examples 1 to 4 and performance comparison of composite microspheres prepared under corresponding conditions
[0061] project Chitosan solution concentration (%) Degradation rate of reactive blue 19 Number of cycles Example 1 0.24 87.6% ≥5 Example 2 0.12 87.3% ≤4 Example 3 0 93.5% ≤2 Example 4 0.5 87.8% ≥5
[0062] Examples 5 to 7
[0063] The difference between Examples 5 to 7 and Example 1 is that the speed of magnetic stirring is different. The other steps and experimental parameters are the same as those of Example 1 and will not be repeated here. The speed settings of Examples 1 and 5 to 6 and the distribution of magnetic materials in the microspheres prepared under the corresponding conditions are shown in Table 3. The SEM image of the composite microspheres prepared in Example 7 is shown in Fig.10 b, and Fig.10 Compared with the composite microspheres of Example 1 shown in a, it can be found that Fig.10 The nucleation effect of the composite microspheres in b is poor, and the magnetic material is mainly dispersed in the microspheres. The results show that magnetic copper alginate composite microspheres with magnetic material nucleation can be obtained under the given rotation speed conditions of the present invention.
[0064] Table 3 Distribution of magnetic materials in microspheres obtained under the rotation speed settings of Example 1 and Examples 5 to 7 and the corresponding conditions
[0065] project Speed (rpm) Distribution of magnetic materials in microspheres Example 1 340 nucleation Example 5 600 nucleation Example 6 200 nucleation Example 7 1200 No nucleation
[0066] The above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention may be modified or replaced by equivalents without departing from the spirit and scope of the technical solution of the present invention.
Claims
1. A magnetic copper alginate composite microsphere, characterized in that: The composite microsphere is a core-shell structure, wherein the core is Fe3O4 and the shell is a copper alginate layer and a chitosan layer; The Fe3O4 in the composite microspheres is coated with ABTS, the copper alginate layer in the shell is close to ABTS, and the chitosan layer is formed on the outside of the copper alginate layer.
2. A method for preparing magnetic copper alginate composite microspheres, characterized in that: The steps include: S1, adding magnetic soil and ABTS solution to sodium alginate colloid, mixing evenly, to obtain a mixed sol; using a syringe to absorb the mixed sol, dripping it into a curing agent, and under magnetic stirring conditions, obtaining magnetic copper alginate microspheres coated with ABTS; S2. Adding the ABTS-coated magnetic copper alginate microspheres obtained in step S1 into a chitosan solution to form a chitosan layer on the surface of the magnetic copper alginate microspheres to obtain magnetic copper alginate composite microspheres.
3. The method for preparing magnetic copper alginate composite microspheres according to claim 2, characterized in that: In step S2, the chitosan solution is prepared by dissolving chitosan in acetic acid solution, the mass concentration of which is 0.1-0.5%, the molecular weight of chitosan is 100,000-300,000, and the volume concentration of the acetic acid solution is 0.25-3%.
4. The method for preparing magnetic copper alginate composite microspheres according to claim 2, characterized in that: In step S1, the rotation speed of the magnetic stirring is 200-1000 rpm.
5. The method for preparing magnetic copper alginate composite microspheres according to claim 2, characterized in that: In step S1, the sodium alginate colloid is formed by dispersing sodium alginate in water, and its mass concentration is 1.5-3%.
6. The method for preparing magnetic copper alginate composite microspheres according to claim 2, characterized in that: In step S1, the mass concentration of the ABTS solution is 0.1-10%.
7. The method for preparing magnetic copper alginate composite microspheres according to claim 2, characterized in that: The volume ratio of the added amount of the magnetic soil to the ABTS solution is 1:10-1:
60.
8. The method for preparing magnetic copper alginate composite microspheres according to claim 2, characterized in that: In step S1, the curing agent is a CuSO4 solution with a concentration of 0.1-1.5M; preferably, the process of adding the mixed sol to the curing agent is carried out at a speed of one drop per second.
9. Use of magnetic copper alginate composite microspheres prepared by the preparation method described in any one of claims 2 to 8 in the field of catalysts.
10. Use of magnetic copper alginate composite microspheres prepared by the preparation method according to any one of claims 2 to 8 in a laccase-mediator system.
Citation Information
Patent Citations
Method for immobilizing phaffia rhodozyma and preparing neokestose and application of method
CN104450665A
Preparation method of copper alginate loaded laccase and mediator ABTS composite biocatalyst
CN112877320A
Laccase encapsultaed magnetic Cu-alginate beads and the method of bioremediation of water pollutants using the same
KR1020170143114A
Cited By
Anti-inflammatory hemostatic composite gel microsphere and preparation method thereof
CN121041228A