Octahedral hollowed-out prismatic MnxCoy / MIL-100 (Fe) catalyst for cooperatively controlling NO and Hg < 0 > as well as preparation method and application of octahedral hollowed-out prismatic MnxCoy / MIL-100 (Fe) catalyst
By introducing Mn and Co into the MIL-100 (Fe) material, a catalyst with an octagonal hollow prismatic structure is formed, which solves the problem of low removal efficiency of NOx and Hg0 in low-temperature flue gas in the existing technology and achieves efficient catalytic effect. and reduced biological toxicity.
Patent Information
- Application Number
- CN202410893606.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-04
- Publication Date
- 2024-10-01
AI Technical Summary
Existing catalysts are difficult to efficiently remove NOx and Hg0 in low-temperature sintering flue gas, and are biologically toxic, making them unable to meet the ultra-low emission requirements of the steel industry.
The octahedral hollow prism MnxCoy/MIL-100(Fe) catalyst was synthesized using a non-corrosive acid hydrothermal method and an equal-volume impregnation method. The MIL-100(Fe) material was modified with Mn and Co to form a rich pore structure and high specific surface area. Catalyst, enhances redox performance and active sites, and synergistically controls NO and Hg0 emissions.
It improves the redox capacity and surface acidic site distribution of the catalyst, achieves efficient removal of NO and Hg0, is suitable for use in low-temperature sintering flue gas, and avoids the use of highly toxic vanadium oxide.
Smart Images

Figure CN118719155A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of metal organic framework catalyst preparation, and specifically relates to a method for synergistically controlling NO and Hg 0 The eight-sided hollow square Mn x Co y / MIL-100(Fe) catalyst and its preparation method and application. Background Art
[0002] In recent years, the harm of pollutants from non-power industries has become increasingly prominent, among which pollutants emitted by the steel industry have attracted much attention. The Ministry of Ecology and Environment and five other national ministries jointly issued the "Opinions on Promoting the Implementation of Ultra-low Emissions in the Steel Industry", which put forward specific requirements for ultra-low emissions of steel enterprises. x and heavy metal mercury (Hg), poses a great threat to environmental air quality and human health. x It is easy to cause pollution problems such as photochemical smog, acid rain and haze; Hg is highly volatile, highly toxic, easy to migrate and has high bioaccumulation. It is often emitted into the air along with particulate matter in sintering flue gas, affecting the world through atmospheric circulation and affecting water and soil through dry and wet deposition. Therefore, it is necessary to study the control of NO in sintering flue gas. x The emission of Hg is of great significance to achieve ultra-low emissions in the steel industry and improve the quality of ambient air. Currently, ammonia selective catalytic reduction technology (NH3-SCR) is widely used in NO x However, the commercial V2O5-WO3(MoO3) / TiO2 catalyst has the disadvantages of narrow temperature window, poor low temperature activity, high toxicity of vanadium oxide, etc., which makes it unsuitable for sintering flue gas with low flue temperature and difficult to achieve NO and Hg 0 Therefore, a new NH3-SCR catalyst suitable for the emission characteristics of sintering flue gas is developed to remove NO and control Hg 0 Emissions have become an urgent problem that needs to be solved, which has important social value and significant environmental benefits.
[0003] MOFs materials have attracted wide attention from researchers due to their high porosity, large specific surface area, adjustable pore structure and unsaturated metal sites, and are used in the fields of adsorption, energy storage and catalysis. Among them, MIL-100(Fe) synthesized with trivalent iron ions as the center and trimesic acid as the ligand has the characteristics of low biological toxicity, developed pores, large specific surface area and rich active sites, which enables it to synergistically control NO and Hg in sintering flue gas. 0However, the function of a single metal in the synergistic control reaction is too limited. Studies have shown that binary metal loading can enhance the interaction between electrons, help improve redox performance and oxygen mobility, enrich active sites and form more active oxygen species, which is conducive to the synergistic reaction. The researchers prepared a high concentration of Co 3+ The catalyst was shown to induce more chemically adsorbed oxygen and oxygen defects, improve the electron shift in the presence of O2, and increase the Hg 0 The oxidation efficiency of these substances in Hg 0 Mn plays an important role in the oxidation process. Mn has attracted wide attention due to its good low-temperature catalytic ability. Mn ions can exist on the catalyst in a multivalent form, which can bring good redox performance. 4+ , Fe 3+ The electronegativity difference between C and O will lead to a charge-deficient state in the charge transport process, which can regulate the active sites so that the catalyst can enhance the selective adsorption of NH3 and NO and enrich the surface acidic sites to improve the denitrification efficiency and Hg 0 Oxidation efficiency. It can be inferred that the metal organic framework catalyst modified with Mn and Co bimetallic oxides can improve the shortcomings of poor single metal activity and functional limitations, enrich active oxygen species and enhance redox performance, and avoid the use of highly toxic vanadium, which is beneficial for the coordinated control of NO and Hg in sintering flue gas. 0 It has great potential. Summary of the invention
[0004] The selective catalytic reduction of NO and the synergistic catalytic oxidation of Hg 0 The present invention provides a catalyst for synergistically controlling NO and Hg 0 The eight-sided hollow square Mn x Co y / MIL-100(Fe) catalyst and its preparation method, the catalyst is prepared by non-corrosive acid hydrothermal method and equal volume impregnation method.
[0005] In order to achieve the above object, the technical solution provided by the present invention is:
[0006] A synergistic control of NO and Hg 0 The eight-sided hollow square Mn x Co y / MIL-100(Fe) catalyst, composed of MnCo modified MIL-100(Fe) metal organic framework material, the octagonal hollow square Mn x Co y / MIL-100(Fe) catalyst is denoted as Mn x Co y / MIL-100(Fe), wherein x is the molar ratio of Mn to MIL-100(Fe), 0≤x≤0.26, preferably 0.2≤x≤0.26, and y is the molar ratio of Co to MIL-100(Fe), 0≤x≤0.26, preferably 0≤x≤0.1
[0007] Further, the porous catalyst is composed of the following components in molar ratio:
[0008] Mn: 0 to 0.26 (more preferably 0.2 to 0.26), Co: 0 to 0.26 (more preferably 0 to 0.1).
[0009] Furthermore, the eight-sided hollow square Mn x Co y / MIL-100(Fe) catalyst has a rich pore structure and a specific surface area of 200-260m 2 / g, total pore volume is 0.3~0.5cm 3 / g, and the average pore size is 6-8nm.
[0010] The above synergistic control of NO and Hg 0 The eight-sided hollow square Mn x Co y / A method for preparing a MIL-100(Fe) catalyst comprises the following steps:
[0011] (1) The MIL-100(Fe) metal organic framework material was synthesized by a non-corrosive acid hydrothermal method;
[0012] (2) Pour manganese nitrate and cobalt nitrate hexahydrate into a beaker with ultrapure water as solvent, and mix them evenly under the action of magnetic stirring;
[0013] (3) pouring the MIL-100(Fe) metal organic framework material obtained in step (1) into the mixed solution obtained in step (2) and performing magnetic stirring, evaporating the solvent in a water bath, and finally forming an octahedral hollow square Mn x Co y / MIL-100(Fe) catalyst.
[0014] Furthermore, in step (1), the preparation method of the MIL-100 (Fe) metal organic framework material is specifically as follows: 0.02-0.04 mol of ferric nitrate nonahydrate is added to 1.12-2.24 mol of deionized water and stirred evenly, 0.0134-0.0268 mol of trimesic acid is added to the above solution, stirred for 25-35 min in a water bath at 55-65° C., the mixed solution is transferred to a stainless steel autoclave lined with polytetrafluoroethylene, and placed in an oven at 150-170° C. and maintained at 70 The method comprises the following steps: cooling the solid-liquid mixture and placing it in ultrapure water at 75 to 85° C. and stirring it for 160 to 200 min. The obtained solid-liquid mixture is divided into several portions and centrifuged to remove the supernatant. The orange precipitate is dispersed with anhydrous ethanol and poured into a conical flask and stirred in a water bath at 55 to 65° C. for 160 to 200 min. The obtained solid-liquid mixture is divided into several portions and centrifuged to remove the supernatant. The orange precipitate is placed in an oven at 150 to 170° C. and maintained for 700 to 740 min to obtain a MIL-100 (Fe) metal organic framework material.
[0015] Furthermore, step (2) is specifically as follows: adding manganese nitrate and cobalt nitrate hexahydrate into 80-120 mL of ultrapure water, and stirring in a water bath at 80° C. to form a mixed solution.
[0016] Further, step (3) is specifically as follows: 2.8 to 3.2 g of MIL-100 (Fe) metal organic framework material is poured into the mixed solution described in step (2), stirred in a water bath at 80° C. until the solution is dry, placed in an oven at 100 to 110° C. and kept for 700 to 740 min, the dried solid material is transferred to a crucible and then placed in a muffle furnace for calcination, the temperature is raised from room temperature to 250 to 350° C. at a rate of 4 to 6° C. / min and kept for 5 to 7 h, and then cooled to room temperature to obtain an octahedral hollow square Mn x Co y / MIL-100(Fe) catalyst.
[0017] The present invention will be further described below:
[0018] The present invention adopts non-corrosive acid hydrothermal method and equal volume impregnation method to synthesize a series of catalysts made of MnCo modified MIL-100 (Fe) with good pore structure and high specific surface area, which are used for synergistic control of NO and Hg 0 The introduction of Mn and Co can introduce more Mn and Co ions into the Fe lattice in the form of Fe-O-Mn and Fe-O-Co solid solutions, and induce the formation of structural defects and a large number of oxygen vacancies, resulting in higher active oxygen concentration and better active oxygen mobility, which is very important for achieving NO and Hg 0 The electronic induction effect between Mn, Co and Fe is crucial for the synergistic control of NO and Hg0 It can be inferred that these catalysts modified with Mn and Co in MIL-100(Fe) have a positive effect in synergistically controlling NO and Hg 0 This may be a promising approach to developing efficient synergistic control of NO and Hg 0 An effective way to develop new catalysts.
[0019] The technical effects of the present invention are:
[0020] The catalyst prepared by the present invention has a rich pore structure, which promotes the good dispersion of surface active components and the exposure of active sites, effectively improves the redox ability, enriches the distribution of surface acid sites, and can efficiently and synergistically control NO and Hg 0 . BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is a flow chart for the preparation of the metal organic framework MIL-100 (Fe) material prepared in Example 1.
[0022] Figure 2 This is a preparation flow chart of the octagonal hollow square Mn4Co1 / MIL-100(Fe) catalyst prepared in Example 2.
[0023] Figure 3 This is a scanning electron microscope image of the octahedral hollow-edge square Mn4Co1 / MIL-100(Fe) catalyst tested in Example 4.
[0024] Figure 4 This is the adsorption-desorption curve of the octahedral hollow square Mn4Co1 / MIL-100(Fe) catalyst tested in Example 4.
[0025] Figure 5 This is the pore size distribution diagram of the octahedral hollow square Mn4Co1 / MIL-100(Fe) catalyst tested in Example 4. DETAILED DESCRIPTION
[0026] The present invention is further described in detail below with reference to specific embodiments, but the present invention is not limited thereto.
[0027] Example 1
[0028] 16.0714g of ferric nitrate nine hydrate was added to 40mL of deionized water, stirred evenly in a water bath at 60°C, and 5.7009g of trimesic acid was added and stirred for 30min. The mixed solution was transferred to a stainless steel reactor lined with polytetrafluoroethylene, and then placed in an oven at 160°C for 720min. After cooling, the solid-liquid mixture was taken out and placed in ultrapure water at 80°C for 180min, and the obtained solid-liquid mixture was divided into centrifuge tubes, centrifuged at 8000rpm for 10min to remove the supernatant, and the orange precipitate was dispersed with anhydrous ethanol and poured into a conical flask and stirred at 60°C for 180min. The obtained solid-liquid mixture was divided into centrifuge tubes, centrifuged at 8000rpm for 10min to remove the supernatant, and the orange precipitate was placed in an oven at 105°C for 720min to obtain the MIL-100 (Fe) metal organic framework material.
[0029] Example 2
[0030] The synergistic control of NO and Hg 0 The eight-sided hollow square Mn x Co y The preparation method of the MIL-100(Fe) catalyst comprises the following steps:
[0031] (1) 0.8396 g of 50 wt% manganese nitrate solution and 0.1707 g of cobalt nitrate hexahydrate were placed in 100 mL of ultrapure water and fully mixed under magnetic stirring;
[0032] (2) adding 3 g of MIL-100(Fe) to the mixed solution obtained in step (1) under stirring in a water bath at 80° C., and stirring for 6 h until the solvent evaporates and the solid is dry;
[0033] (3) drying the solid obtained in step (2) in an oven at 105° C. for 720 min;
[0034] (4) The dried solid was transferred into a crucible, placed in a muffle furnace, and calcined at a rate of 5°C / min from room temperature to 300°C and maintained for 6 h. After cooling to room temperature, an octagonal hollow square Mn4Co1 / MIL-100(Fe) catalyst was obtained.
[0035] Example 3
[0036] The octagonal hollow square Mn4Co1 / MIL-100 (Fe) catalyst of the present invention synergistically controls NO and Hg 0 The performance test was carried out in a fixed bed reactor. The catalyst in Example 2 was loaded into the catalytic reactor, and the simulated flue gas of the gas distribution system consisted of 300ppm NO, 300ppm NH3, 16vol.% O2, 80μg / m3 Hg 0 The total gas flow rate was maintained at 200 mL / min and the gas volume space velocity (GHSV) was 40 000 h -1 The reaction temperature was controlled in the range of 50-300°C, and the catalyst was tested to synergistically control NO and Hg 0 conversion efficiency.
[0037] Example 4
[0038] BET and SEM tests of the catalyst of the present invention
[0039] In the present invention, the specific surface area, pore volume and pore size of the synthesized catalyst are tested using an America Micromeritics-3Flex analyzer (Micromeritics, USA). After taking 0.1g of sample and degassing at 150°C for 12h, N2 is used as an adsorbent and the experimental measurement is carried out at a temperature of 77K. According to the Brunauer-Emmett-Teller (BET) and Barrett-Joyner-Halenda (BJH) methods, the specific surface area, total pore volume and average pore size are obtained. In addition, the MIRA3 LMU (TESCAN, Czech Republic) field emission scanning electron microscope system is used in the present invention to photograph the morphology and structure of the catalyst.
[0040] The results show that the eight-sided hollow square Mn x Co y / MIL-100(Fe) catalyst uses MnCo to regulate the coordination environment of Fe ions, making the catalyst present an octahedral hollow square structure with a large specific surface area and rich pore structure, which can promote the dispersion of active components, expose more active sites, improve electron transfer and redox ability, enrich surface acid sites, enhance oxygen mobility and utilization, and thus make NO and Hg 0 Efficient removal.
Claims
1. A synergistic control of NO and Hg 0 The eight-sided hollow square Mn x Co y / MIL-100(Fe) catalyst, characterized in that The eight-sided hollow square Mn x Co y / MIL-100(Fe) catalyst is composed of transition metal Mn and Co modified MIL-100(Fe), wherein the octagonal hollow square Mn x Co y / MIL-100(Fe) catalyst is denoted as Mn x Co y / MIL-100(Fe).
2. The coordinated control of NO and Hg according to claim 1 0 The eight-sided hollow square Mn x Co y / MIL-100(Fe) catalyst, characterized in that The eight-sided hollow square Mn x Co y / MIL-100(Fe) catalyst is composed of components in the following molar ratios: Mn:MIL-100(Fe)=0~0.26, Co:MIL-100(Fe)=0~0.
26.
3. The coordinated control of NO and Hg according to claim 1 0 The eight-sided hollow square Mn x Co y / MIL-100(Fe) catalyst, characterized in that The eight-sided hollow square Mn x Co y / MIL-100(Fe) catalyst has a rich pore structure and a specific surface area of 200-260m 2 / g, total pore volume is 0.3~0.5cm 3 / g, and the average pore size is 6-8nm.
4. The synergistic control of NO and Hg according to any one of claims 1 to 3 0 The eight-sided hollow square Mn x Co y / A method for preparing a MIL-100(Fe) catalyst, characterized in that: The steps include: (1) trimesic acid and ferric nitrate nonahydrate were fully mixed in ultrapure water for 25 to 35 minutes, then added into a stainless steel autoclave lined with polytetrafluoroethylene, synthesized by a non-corrosive acid hydrothermal method, and washed and purified with ultrapure water and anhydrous ethanol and dried to obtain MIL-100(Fe); (2) adding manganese nitrate and cobalt nitrate hexahydrate into ultrapure water, and mixing them thoroughly under the action of magnetic stirring; (3) adding the MIL-100 (Fe) material obtained in step (1) to the mixed solution obtained in step (2), stirring until the solid-liquid mixture is dry, drying in an oven, and calcining in a muffle furnace to obtain a composite material, i.e., octagonal hollow square Mn x Co y / MIL-100(Fe) catalyst.
5. The preparation method according to claim 4, characterized in that: In step (1), the preparation method of the MIL-100 (Fe) metal organic framework material is specifically as follows: 0.02-0.04 mol of ferric nitrate nonahydrate is added to 1.12-2.24 mol of deionized water and stirred evenly, 0.0134-0.0268 mol of trimesic acid is added to the above solution, stirred for 25-35 min in a water bath at 55-65° C., the mixed solution is transferred to a stainless steel autoclave lined with polytetrafluoroethylene, and placed in an oven at 150-170° C. and maintained at 700-74 0min, after cooling, take out the solid-liquid mixture and put it into ultrapure water at 75-85°C and stir it for 160-200min, divide the obtained solid-liquid mixture into portions and centrifuge to remove the supernatant, transfer the orange precipitate into anhydrous ethanol for dispersion and pour it into a conical flask and stir it for 160-200min in a water bath at 55-65°C, divide the obtained solid-liquid mixture into portions and centrifuge to remove the supernatant, put the orange precipitate into an oven at 100-110°C and keep it for 700-740min to obtain the MIL-100(Fe) metal organic framework material.
6. The preparation method according to claim 4, characterized in that: Step (2) is specifically as follows: pouring manganese nitrate and cobalt nitrate hexahydrate into 80-120 mL of ultrapure water, and stirring in a water bath at 75-85° C. to form a mixed solution.
7. The preparation method according to claim 4, characterized in that: Step (3) is specifically as follows: 2.8 to 3.2 g of MIL-100 (Fe) metal organic framework material is poured into the mixed solution described in claim 6, stirred in a water bath at 75 to 85 ° C until the solvent evaporates and becomes relatively dry, placed in an oven at 100 to 110 ° C and kept for 700 to 740 min, the dried solid material is transferred to a crucible and then placed in a muffle furnace for calcination, the temperature is raised from room temperature to 250 to 350 ° C at a rate of 4 to 6 ° C / min and kept for 5 to 7 h, and then cooled to room temperature to obtain an octahedral hollow square Mn x Co y / MIL-100(Fe) catalyst.
Citation Information
Cited By
MOF-derived Fe / Mn composite material as well as preparation method and application thereof
CN120094617A