A coal flotation aid and its application method

By compounding coal flotation additives and emulsifying them, the hydrophobicity and reagent dispersibility of low-rank coal are improved, solving the problem of low flotation efficiency of low-rank coal and achieving high-efficiency flotation effect and improved economy.

CN118719330BActive Publication Date: 2026-11-17CHINA COAL (TIANJIN) UNDERGROUND ENG INTELLIGENCE RES INST CO LTD +2
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410961606.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2026-11-17
Estimated Expiration
2044-07-18

AI Technical Summary

Technical Problem

Low-rank coal slime has poor floatability, leading to resource waste. Existing methods are either uneconomical or unstable, and the reagents lack dispersibility and selectivity.

Method used

The coal flotation aid consists of cocamidopropyl betaine, fatty alcohol polyoxyethylene ether, soluble sodium carboxymethyl cellulose, fatty acid ester and Span 80. Through a primary emulsification, settling and secondary emulsification steps, a water-in-oil-in-water emulsion is formed, which improves the hydrophobicity of coal particle surface and the dispersibility of the reagent.

Benefits of technology

It improved the flotation clean coal yield and improved the indicators of low-rank coal, reduced the amount of reagents and clean coal ash, and enhanced the flotation effect and economic benefits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004950436360000041
    Figure BDA0004950436360000041
Patent Text Reader

Abstract

This invention discloses a coal flotation aid and its application method, applicable to solving the problems of low clean coal yield, high clean coal ash content, and poor flotation performance in low-rank coal slime flotation. The reagent raw materials, by mass, are: 1-90 parts water, 5-20 parts cocamidopropyl betaine, 5-30 parts fatty alcohol polyoxyethylene ether, 1-5 parts soluble sodium carboxymethyl cellulose, 1-5 parts Span 80, and 5-25 parts fatty acid esters. These components are added to the same container in any order and stirred thoroughly before use. This coal flotation aid, by compounding cocamidopropyl betaine, fatty alcohol polyoxyethylene ether, and fatty acid esters, provides a surface-modifying effect, significantly improving the hydrophobicity of low-rank coal. Soluble sodium carboxymethyl cellulose effectively reduces the adsorption of reagents by the pore structure of coal, promoting coal particle agglomeration and thus reducing reagent dosage. The addition of Span 80 enhances the emulsification effect and emulsion stability in the secondary emulsification process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of coal flotation technology, specifically to a coal flotation aid and its application method. Background Technology

[0002] my country has abundant reserves of low-rank coal, but its slime has poor floatability, making it difficult to wash and process. Therefore, resource waste is common in low-rank coal separation. Due to the large number of oxygen-containing functional groups and strong hydrophilicity on the surface of low-rank coal, non-polar hydrocarbon oils used as collectors are difficult to spread on the coal particle surface, making it difficult to use conventional methods for efficient flotation of low-rank coal slime. Furthermore, low-rank coal contains well-developed pores; when adding reagents using conventional methods, a large amount of flotation reagent enters the pores, leading to increased reagent consumption.

[0003] Domestic and international scholars have proposed many methods to solve the above problems. Some scholars have used pretreatment methods to reduce the porosity of coal particles while exposing the fresh coal surface to the flotation environment, thereby improving the flotation effect. However, this method is not economical and is difficult to implement industrially. Other scholars have improved the flotation effect by adding active substances such as esters and ethers to increase the hydrophobicity of coal slime. However, these substances have poor stability and are prone to deterioration during storage, affecting their performance. Adding surfactants soluble in conventional coal flotation collectors to prepare composite coal flotation reagents is an effective way to solve the flotation problem of low-rank coal, and can, to some extent, address the issues of low yield and combustible recovery rate of low-rank coal. However, there are few types of oil-soluble surfactants, and because surfactants have low selectivity for coal, their use in coal flotation often increases the ash content of clean coal while increasing the yield. Since the reagent is still an oily liquid, it also suffers from poor dispersibility during use. Summary of the Invention

[0004] The purpose of this invention is to provide a coal flotation aid and its application method to solve the problems mentioned in the background art.

[0005] To achieve the above objectives, the present invention provides the following technical solution:

[0006] A coal flotation aid, comprising the following components by mass: 1-90 parts water, 5-20 parts cocamidopropyl betaine, 5-30 parts fatty alcohol polyoxyethylene ether, 1-5 parts soluble sodium carboxymethyl cellulose, 1-5 parts Span 80, and 5-25 parts fatty acid esters. The above components are poured into the same container in any order and stirred evenly before use.

[0007] A method for using a coal flotation aid, wherein the coal flotation aid is used to surface modify coal in specific steps, including primary emulsification, settling, secondary emulsification, and surface modification, the specific steps of which are as follows:

[0008] A primary emulsion is obtained by emulsifying and dispersing water and non-polar hydrocarbon oil in a certain proportion in a primary emulsification device.

[0009] After the primary emulsion is allowed to stand for a period of time, the primary emulsion and the coal flotation aid are added into the secondary emulsification equipment for secondary emulsification and dispersion to obtain the secondary emulsion.

[0010] The secondary emulsion is mixed with the coal flotation frother and fed into the surface modifier to perform surface modification on the coal slime fed into the flotation process.

[0011] As a further aspect of the present invention, the non-polar hydrocarbon oil is kerosene or diesel oil.

[0012] As a further aspect of the present invention: the flotation frother for coal is 2-octanol, fusel oil, or No. 2 oil.

[0013] As a further aspect of the present invention, the shear rate provided by the primary emulsification equipment and the secondary emulsification equipment is not less than 1.0-5.0 m / s.

[0014] As a further aspect of the present invention: the time for the first emulsification dispersion is 1-30 minutes, and the time for the second emulsification dispersion is 1-20 minutes.

[0015] As a further aspect of the present invention: the proportion of water during a single emulsification is not higher than 50%.

[0016] As a further aspect of the present invention, the proportion of coal flotation aid during secondary emulsification is not less than 50%.

[0017] As a further aspect of the present invention, the standing time of the emulsion is 1-30 minutes.

[0018] As a further aspect of the present invention: the flotation feed coal slime is low-rank coal, and the amount of coal flotation aid per ton of dry coal slime is no more than 2 kg / t, and is less than or equal to the amount of non-polar hydrocarbon oil.

[0019] Compared with the prior art, the beneficial effects of the present invention are:

[0020] The coal flotation aid of this invention combines cocamidopropyl betaine, fatty alcohol polyoxyethylene ether, fatty acid esters, and other substances to give the flotation aid a surface-modifying effect, significantly improving the hydrophobicity of low-rank coal. Soluble sodium carboxymethyl cellulose can effectively reduce the adsorption of reagents by the pore structure of coal, promote the agglomeration of coal particles, and thus reduce the dosage. The addition of Span 80 improves the emulsification effect and emulsion stability in the secondary emulsification process, thereby increasing reagent dispersibility and reducing the dosage.

[0021] The method of use of this invention involves emulsifying non-polar hydrocarbon oil and water in a single emulsification process to form a water-in-oil emulsion, reducing the amount of non-polar hydrocarbon oil used. A settling process allows the oil and water phases of the primary emulsion to reach equilibrium and stability, providing a qualified water-in-oil emulsion for a secondary emulsification process. The secondary emulsification process further transforms the emulsion into a water-in-oil emulsion, allowing the non-polar groups of fatty alcohol polyoxyethylene ethers and fatty acid esters to align with the oil phase inside the emulsion droplets, thus exposing the polar groups on the surface of the droplets. This facilitates the adsorption of oxygen-containing functional groups on the coal surface by the droplets. Furthermore, the water-in-oil emulsion increases the dispersibility and selectivity of the reagent during the surface modification process. Detailed Implementation

[0022] Preferred embodiments of the present invention are described in detail below.

[0023] 70 parts water, 10 parts cocamidopropyl betaine, 5 parts fatty alcohol polyoxyethylene ether, 5 parts soluble sodium carboxymethyl cellulose, 5 parts Span 80, and 5 parts fatty acid esters are added to the same container in any order and stirred evenly before being used as a coal flotation aid.

[0024] Properties of coal slime: Low-rank coal slime from Pingshuo, Shanxi Province, with an ash content of 25%-27% and a yield of over 50% for particles smaller than 0.045mm.

[0025] Preparation conditions of the secondary emulsion: Pour 40 ml of ultrapure water and 60 ml of kerosene into a 500 ml beaker and perform a primary emulsification operation using a high-shear emulsification device for 2.5 minutes at a shear rate of 3.0 m / s to obtain the primary emulsion. Allow the primary emulsion to stand for 5 minutes. Add 150 ml of coal flotation aid to the primary emulsion and perform a secondary emulsification operation for 2.5 minutes at a shear rate of 3.0 m / s to obtain the secondary emulsion.

[0026] Flotation test conditions: A laboratory 1.5L hanging-cell flotation machine was used for flotation. Since surface modification can be completed during the pulp conditioning process in laboratory flotation equipment, no separate surface modification operation was performed in this embodiment. The flotation machine speed was 1800 r / min, and the flotation concentration was 80 g / L. The flotation first performed a 3-minute pre-conditioning of the pulp. After the pre-conditioning, a secondary emulsion was added at a dosage of 1500 g / t, and the mixture was stirred for 2 minutes. Then, 500 g / t of octanol, a coal flotation frother, was added, and the mixture was stirred for 30 seconds. After that, the air valve was opened, and the flotation flow rate was 0.25 m 3 Aeration was carried out at a rate of / h. After 10 seconds of aeration, foam scraping began and lasted for 3 minutes. The scraped foam was the flotation concentrate, and the slurry in the tank after the foam scraping period was completed was the flotation tailings. The flotation concentrate and flotation tailings were filtered, dried, and analyzed to calculate the yield, ash content, and flotation performance indicators. The data were recorded in Table 1 and named Experiment 1.

[0027] Comparative test conditions:

[0028] Comparative Experiment 1: Other flotation test conditions were the same as before, but kerosene was added after pre-conditioning the slurry at a dosage of 1500 g / t. The data are recorded in Table 1 and named Experiment 2.

[0029] Comparative Experiment 2: 40 ml of ultrapure water, 60 ml of kerosene, and 150 ml of the aforementioned coal flotation aid were simultaneously added to a beaker. Emulsification was performed using a high-shear emulsification device for 5 minutes at a shear rate of 3.0 m / s. After emulsification, the mixture was allowed to stand for 5 minutes. The emulsion was then used for flotation. The flotation test conditions were the same as before, with an emulsion dosage of 1500 g / t. The data are recorded in Table 1 and named Experiment 3.

[0030] Comparative Experiment 3: A secondary emulsion was prepared according to the method described in this invention and subjected to flotation tests. The flotation test conditions were the same as before, but the amount of secondary emulsion added was 1275 g / t. The data are recorded in Table 1 and named Experiment 4.

[0031]

[0032] Table 1 Comparison of Flotation Test Results

[0033] Comparing the data from Experiment 1 and Experiment 2 in Table 1, it can be seen that, compared with conventional kerosene and 2-octanol, when using the coal flotation aid and its application method described in this invention for flotation, under the same dosage, the yield of flotation clean coal increases by 4.17%, the ash content of flotation clean coal decreases by 2.26%, and the flotation improvement index increases by 8.84%.

[0034] Comparing the data from Experiment 1 and Experiment 3 in Table 1, it can be seen that, compared with performing emulsification only once, the method of using the coal flotation aid described in this invention can reduce the ash content of the flotation clean coal by 1.58% and increase the flotation perfection index by 6.01% under the same emulsification shear rate, total emulsification time and settling time.

[0035] Comparing the data from Experiments 2 and 4 in Table 1, it can be seen that the coal flotation aid and its application method described in this invention can achieve a flotation clean coal yield similar to that of conventional flotation reagents while reducing the dosage by 15%, and reduce the ash content of the flotation clean coal by 2.28% and increase the flotation perfection index by 8.22%.

[0036] In summary, the coal flotation additives and their application methods used in this embodiment can improve the yield of flotation clean coal and the flotation perfection index for low-rank coal flotation, while reducing the ash content of flotation clean coal and the amount of reagents used. This is of great significance for improving the economic benefits of coal enterprises and has broad application prospects.

[0037] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above, and that the invention can be implemented in other specific forms without departing from the spirit or essential characteristics of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description. Thus, it is intended that all variations falling within the meaning and scope of equivalents of the claims be included within the present invention.

[0038] Furthermore, it should be understood that although this specification describes embodiments, not every embodiment contains only one independent technical solution. This narrative style is merely for clarity. Those skilled in the art should consider the specification as a whole, and the technical solutions in each embodiment can also be appropriately combined to form other embodiments that can be understood by those skilled in the art.

Claims

1. A method for using a coal flotation aid, wherein the raw materials of the flotation aid, by mass, are: 1-90 parts water, 5-20 parts cocamidopropyl betaine, 5-30 parts fatty alcohol polyoxyethylene ether, 1-5 parts soluble sodium carboxymethyl cellulose, 1-5 parts Span 80, and 5-25 parts fatty acid esters. The above components are poured into the same container in any order, stirred evenly, and then it is ready for use; characterized in that… The coal flotation aid described above is used to perform surface modification of coal in specific steps, including primary emulsification, settling, secondary emulsification, and surface modification. The specific steps are as follows: Water and non-polar hydrocarbon oils are emulsified and dispersed in a primary emulsification device at a certain ratio to obtain a primary emulsion. After the primary emulsion is left to stand for a period of time, the primary emulsion and the coal flotation aid are added into the secondary emulsification equipment for secondary emulsification and dispersion to obtain the secondary emulsion. The secondary emulsion is mixed with the coal flotation frother and fed into the surface modifier to perform surface modification on the coal slime fed into the flotation process.

2. The method of using the coal flotation aid according to claim 1, characterized in that, Non-polar hydrocarbon oils are kerosene or diesel oil.

3. The method of using the coal flotation aid according to claim 1, characterized in that, The flotation frother for coal is octanol, fusel oil, or No. 2 oil.

4. The method of using the coal flotation aid according to claim 1, characterized in that, The shear rate provided by the primary emulsification equipment and the secondary emulsification equipment shall not be less than 1.0-5.0 m / s.

5. The method of using the coal flotation aid according to claim 1, characterized in that, The time for primary emulsification and dispersion is 1-30 minutes, and the time for secondary emulsification and dispersion is 1-20 minutes.

6. The method of using the coal flotation aid according to claim 1, characterized in that, The water content should not exceed 50% during a single emulsification.

7. The method of using the coal flotation aid according to claim 1, characterized in that, The proportion of coal flotation aids during secondary emulsification shall not be less than 50%.

8. The method of using the coal flotation aid according to claim 1, characterized in that, The emulsion should be allowed to stand for 1-30 minutes at a time.

9. The method of using the coal flotation aid according to claim 1, characterized in that, The flotation feed coal slime is low-rank coal, and the amount of coal flotation aid per ton of dry coal slime is no more than 2 kg / t, and less than or equal to the amount of non-polar hydrocarbon oil.

Citation Information

Patent Citations

  • Floatation method of difficult-to-float coal

    CN101015820A

  • Coal compound flotation agent

    CN104259011A