Automobile casting and forging composite process method
Through the automotive casting and forging composite process, the process of combining squeeze casting and die forging is used to solve the common problems of shrinkage cavities and cracks in castings of automotive parts such as intake manifolds, and achieve high strength and high density manufacturing effects. .
Patent Information
- Application Number
- CN202410720631.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-05
- Publication Date
- 2024-10-01
AI Technical Summary
Existing automotive casting processes are difficult to produce parts with high strength, high density, and high fatigue life, such as automotive intake manifolds, which are prone to defects such as shrinkage cavities, cracks, and loose tissue.
The automotive casting and forging composite process method is adopted, including extrusion casting pre-forming of aluminum alloy liquid, followed by forging treatment in a die forging die, controlling the forging start time and forging pressure, combined with T6 heat treatment to ensure dense structure and plastic deformation.
It effectively avoids defects such as shrinkage cavities, cracks and loose tissue, and improves the mechanical properties of the parts.
Smart Images

Figure CN118720085A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of automobile processing, in particular to an automobile casting and forging composite process method. Background Art
[0002] With the acceleration of industrialization and energy development and utilization, the energy crisis has become a global concern. Environmental protection, energy saving, improvement of parts quality and production efficiency have become the main ways for enterprises to improve their benefits. Based on the above reasons, the research on material forming methods has become the main way to solve the above problems. There are many different material forming methods, but people always hope that the material processing method is easy to operate, has strong applicability, and has high quality of parts to meet the requirements of scientific and technological development on the shape, size and material properties of parts. Therefore, the research on forming technology has become the main way for enterprises to improve productivity and production efficiency. Castings and forgings play an important role in economic development. Such parts are widely used in the economy, such as automobiles, machinery, aviation, aerospace, etc., especially in the automotive field. New energy vehicles have become the trend of future development. The core of development is mainly concentrated on energy and environmental protection. Advanced automotive material technology dominated by lightweight automobiles is an important guarantee for achieving this goal. Therefore, lightweight new energy vehicles have become the main direction of future automotive technology development. Only by reducing the weight of various parts of the car can the car truly achieve the purpose of lightweight. In the past 10 years, steel parts in automobile castings are being replaced by aluminum parts. The conventional steel usage in automobiles is gradually decreasing, while the proportion of aluminum alloy castings in automobiles is increasing. Aluminum alloy castings are generally manufactured by gravity casting and other methods. Aluminum alloys are prone to shrinkage during solidification. Insufficient shrinkage compensation during casting crystallization, incorrect position of alloy liquid introduction, inappropriate temperature of various parts of the metal mold, and non-conformity with the sequential solidification principle may all form shrinkage cavities. In addition, metal mold gravity casting is also prone to cold shuts, which may occur when the mold temperature is too low, the aluminum liquid pouring temperature is too low, the pouring speed is inconsistent, the pouring system is poorly designed, and the number of internal gates is small. There are also methods such as low-pressure casting, melt casting, lost foam casting, metal mold casting, sand casting, etc. These molding methods are difficult to meet the requirements of some parts with high strength, high density, and high fatigue life, such as automobile intake manifolds and other parts with high performance requirements. Therefore, how to adjust the process parameters to optimize the manufacturing quality of automobile intake manifolds is a problem to be solved. Therefore, the present invention proposes an automobile casting and forging composite process method to solve the problems existing in the prior art. Summary of the invention
[0003] In view of the above problems, the present invention proposes an automobile casting and forging composite process method, which can effectively force shrinkage compensation and structural compaction of extrusion casting preforms and cause them to undergo plastic deformation, thereby avoiding the occurrence of defects such as shrinkage cavities, cracks and loose structure, and the mechanical properties of the parts are stronger.
[0004] To achieve the purpose of the present invention, the present invention is implemented by the following technical scheme: an automobile casting and forging composite process method comprises the following steps: S1: Melting the alloy material to prepare aluminum alloy liquid, measuring the chemical composition, and deriving the liquidus and solidus; S2: Prepare a molding die suitable for the automobile intake manifold and preheat the die to 250-300°C; S3: pouring aluminum alloy liquid into the forming mold, and controlling the punch injection speed to 50-60 mm / s; S4: Control the filling pressure to 130-150 MPa and maintain the pressure for 15-25 seconds, and obtain the extrusion casting preform after cooling; S5: heating the extrusion casting preform to its initial forging temperature, and then placing it into a die forging die, controlling the forging pressure to 110-130 MPa, and controlling the start forging time to 3-4 seconds; S6: Observe whether the upper die and the lower die of the die forging die are closed. After closing, open the die and lift up the forging blank; S7: Perform T6 heat treatment on the forging blank.
[0005] A further improvement is that: S1 comprises the following steps: S11: Raise the temperature of the medium frequency induction furnace to 300-400℃; S12: Add industrial pure aluminum, add A1-50%Cu master alloy and quick-dissolving silicon when the furnace temperature rises to 720°C, add A1-5%Ti-1%B at 730°C, and stir evenly; S13: After all the charge is melted, it is refined and degassed, allowed to stand, slag removed, a covering agent is added, and then a pure magnesium ingot wrapped with pure aluminum foil is added, stirred evenly, allowed to stand, and slag removed; S14: Take the alloy liquid with a spoon to measure the chemical composition, deduce the liquidus line and solidus line, and then keep the temperature at 750℃.
[0006] A further improvement is that: S2 comprises the following steps: S21: preparing a molding die adapted to the automobile intake manifold, the molding die being a pressure casting die; S22: Clean the inner surface of the molding die to remove dust and oil; S23: preheating the molding die to 250-300° C. through an electric heating tube; S24: The molding mold is kept warm until pouring begins.
[0007] A further improvement is that: S3 comprises the following steps: S31: connecting the punch head to the pouring port of the forming die, and introducing aluminum alloy liquid into the punch head; S32: Use piston to apply pressure and control the punch injection speed to 50-60mm / s; S33: During pouring, the pouring temperature is controlled to be 750°C.
[0008] A further improvement is that in S31, before pouring, the temperature of the aluminum alloy liquid is lowered to 30-60° C. above the liquidus temperature.
[0009] A further improvement is that: said S4 comprises the following steps: S41: After the aluminum alloy liquid cools down with the mold for 3-8 seconds, the die punch is driven by the slide of the extrusion casting press to apply a filling pressure of 130-150MPa to the aluminum alloy liquid in solidification and cooling; S42: Maintain pressure for 15-25 seconds, then release pressure and cool at room temperature; S43: Obtain an extrusion casting preform.
[0010] A further improvement is that: S5 comprises the following steps: S51: heating the squeeze casting preform to its initial forging temperature using a resistance furnace; S52: preheating the upper die and the lower die of the die forging die, and controlling the temperature to be 200° C.-250° C.; S53: placing the extrusion casting preform into a die forging die, and controlling the forging pressure to 110-130 MPa; S54: Control the forging start time to 3-4S and shorten the time error to 0.01S.
[0011] A further improvement is that in S6, when the upper die and the lower die are not closed, the upper die is driven by the press slider to strike rapidly at a frequency of 10 times / s-40 times / s, with a single strike deformation feed amount of 0.2mm-0.5mm, until the upper die and the lower die are closed.
[0012] A further improvement is that in S6, after the die is opened, the forging blank is processed, the flash generated during the die forging process is trimmed, and the surface is nitrided.
[0013] A further improvement is that: said S7 comprises the following steps: S71: The forging blank is solution treated at 530℃ for 3 h, and the heat treatment furnace is a box-type air circulation resistance furnace; S72: followed by water quenching, followed by artificial aging at 180°C for 6h, and finally air cooling.
[0014] The beneficial effects of the present invention are: 1. The present invention controls the start forging time to 3-4S and the applied forging pressure to 110-130MPa, which can effectively force the shrinkage of the extrusion casting preform and make it compact and cause it to produce plastic deformation, avoiding the generation of defects such as shrinkage holes, cracks and loose structure, and the mechanical properties of the parts are stronger.
[0015] 2. The present invention uses a press slider to drive the upper mold to strike quickly at a frequency of 10 times / s-40 times / s, with a single strike deformation feed amount of 0.2mm-0.5mm, until the upper mold and the lower mold are closed, so that the last solidified structure in the middle of the extrusion casting preform is flattened and compacted under the action of the forging pressure, undergoing plastic deformation, so that the structure of the ingot close to the lower mold is refined.
[0016] 3. The present invention controls the punch injection speed to 50-60 mm / s; controls the filling pressure to 130-150 MPa, and maintains the pressure for 15-25 seconds, so that the real-time pouring and filling is more compact, avoiding the occurrence of defects such as shrinkage cavities, cracks and loose structure. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 It is a flow chart of the present invention.
[0018] Figure 2 Schematic diagram of the microstructure of the squeeze casting preformed part before forging of the present invention; Figure 3 It is a schematic diagram of the microstructure of the extrusion casting preform after forging of the present invention. DETAILED DESCRIPTION
[0019] In order to deepen the understanding of the present invention, the present invention will be further described in detail below in conjunction with examples. The examples are only used to explain the present invention and do not constitute a limitation on the protection scope of the present invention. Example 1
[0020] according to Figure 1 As shown, this embodiment proposes a composite process for automotive casting and forging, comprising the following steps: S1: Melting the alloy material to prepare aluminum alloy liquid, measuring the chemical composition, and deriving the liquidus and solidus; S2: Prepare a molding die suitable for the automobile intake manifold and preheat the die to 250-300°C; S3: pouring aluminum alloy liquid into the forming mold, and controlling the punch injection speed to 50-60 mm / s; S4: Control the filling pressure to 130-150 MPa and maintain the pressure for 15-25 seconds, and obtain the extrusion casting preform after cooling; S5: heating the extrusion casting preform to its initial forging temperature, and then placing it into a die forging die, controlling the forging pressure to 110-130 MPa, and controlling the start forging time to 3-4 seconds; S6: Observe whether the upper die and the lower die of the die forging die are closed. After closing, open the die and lift up the forging blank; S7: Perform T6 heat treatment on the forging blank.
[0021] The invention controls the start forging time to 3-4S and the applied forging pressure to 110-130MPa, which can effectively force shrinkage compensation and compact the structure of the extrusion casting preform and cause it to produce plastic deformation, avoiding the generation of defects such as shrinkage cavities, cracks and loose structure. In addition, the invention controls the punch injection speed to 50-60mm / s; controls the filling pressure to 130-150MPa, and maintains the pressure for 15-25S, so that the real-time pouring and filling are more compact, avoiding the generation of defects such as shrinkage cavities, cracks and loose structure. Example 2
[0022] according to Figure 1 , 2 As shown in , 3, this embodiment proposes an automobile casting and forging composite process method, comprising the following steps: The alloy material is melted to prepare aluminum alloy liquid, and the chemical composition is determined, and the liquidus and solidus are derived; the specific steps are as follows: the temperature of the medium frequency induction furnace is increased to 300°C; industrial pure aluminum is added, and when the furnace temperature is increased to 720°C, A1-50%Cu master alloy and quick-dissolving silicon are added, and when the furnace temperature is 730°C, A1-5%Ti-1%B is added, and then stirred evenly; after all the furnace materials are melted, they are refined and degassed, allowed to stand, slag is removed, and after adding a covering agent, pure magnesium ingots wrapped with pure aluminum foil are added, stirred evenly, allowed to stand and slag is removed; the alloy liquid is taken with a material spoon for chemical composition determination, and the liquidus and solidus are derived, and then the temperature is kept at 750°C; according to the characteristics of the automobile intake manifold, 6061 aluminum alloy is prepared. 6061 aluminum alloy is a typical heat-treatable and strengthened aluminum alloy. Al-Mg-Si alloy has good plasticity, corrosion resistance, weldability, low quenching sensitivity coefficient and good forming performance, and is more suitable for forging. Its forgings are mainly used in automobiles, motorcycles and yachts. However, for some parts with complex structures, 6061 aluminum alloy belongs to deformed aluminum alloy and has poor casting performance. Generally, it is difficult to produce it by traditional casting processes such as metal mold casting, low-pressure casting and high-pressure casting. This is mainly because it often has defects such as coarse grains, uneven structure and component segregation. Therefore, the process method of the present invention has been verified to effectively force shrinkage compensation and compact structure of squeeze casting preforms and cause them to produce plastic deformation, thereby avoiding defects such as shrinkage cavities, cracks and loose structure.
[0023] Prepare a molding die for the automobile intake manifold and preheat the mold to 250°C; specifically include the following steps: prepare a molding die for the automobile intake manifold, the molding die is a pressure casting mold; clean the inner surface of the molding die to remove dust and oil; preheat the molding die to 250-300°C through an electric heating tube; keep the molding die warm until the pouring starts; preheat in advance to avoid the influence of the cold mold on the pouring material; The aluminum alloy liquid is poured into the forming mold, and the punch injection speed is controlled to be 50 mm / s; specifically, the following steps are included: before pouring, the temperature of the aluminum alloy liquid is reduced to 30-60°C above the liquidus temperature, the punch head is connected to the pouring port of the forming mold, and the aluminum alloy liquid is introduced into the punch head; a piston is used to apply pressure, and the punch injection speed is controlled to be 50 mm / s; during pouring, the pouring temperature is controlled to be 750°C; when the punch injection speed is 50 mm / s, when the inertia force is large, the liquid flows in a turbulent manner, and the viscous force effectively restricts the longitudinal pulsating flow of the metal liquid particles, thereby effectively curbing the turbulence of the liquid; The filling pressure is controlled to be 130MPa, and the pressure is maintained for 15S, and an extrusion casting preform is obtained after cooling; specifically, the following steps are included: after the aluminum alloy liquid cools with the mold for 5S, the mold punch is driven by the slider of the extrusion casting press to apply a filling pressure of 130MPa to the aluminum alloy liquid in solidification and cooling; the pressure is maintained for 15S, and then the pressure is released, and the extrusion casting preform is obtained; the filling pressure is controlled to be 130MPa, so that the metal liquid between the dendrites fills and flows, and has the characteristics of metal liquid flow in filling rheology. The existence of high pressure conditions during the metal liquid filling process is more conducive to the realization of such extrusion filling, so as to achieve complete filling and eliminate holes. For metals that shrink during solidification, pressurization during solidification is conducive to the solidification of such alloys, that is, more atomic groups participate in nucleation in the metal liquid; The extrusion casting preform is heated to its initial forging temperature, and then placed in the die forging die, the forging pressure is controlled to 110MPa, and the start forging time is controlled to 3S; the specific steps include: heating the extrusion casting preform to its initial forging temperature with a resistance furnace; preheating the upper die and the lower die of the die forging die, and controlling the temperature to 200℃; placing the extrusion casting preform in the die forging die, and controlling the forging pressure to 110MPa; controlling the start forging time to 3S, and shortening the time error to 0.01S; the present invention controls the start forging time to 3-4S, controls the applied forging pressure to 110-130MPa, can effectively force the extrusion casting preform to be shrinkage-compensated and compacted and cause it to produce plastic deformation, avoids the generation of defects such as shrinkage cavities, cracks and loose tissue, and can be seen by comparison. Figure 2 , 3 ; Observe whether the upper die and the lower die of the die forging die are closed. When the upper die and the lower die are not closed, the upper die is driven by the slider of the press to strike quickly at a frequency of 10 times / s, and the deformation feed amount of a single strike is 0.2mmmm, until the upper die and the lower die are closed; after closing, the die is opened to lift the forging blank. After opening the die, the forging blank is processed, the flash generated during the die forging process is trimmed, and the surface is nitrided; the upper die is driven by the slider of the press to strike quickly at a frequency of 10 times / s, and the deformation feed amount of a single strike is 0.2mm, until the upper die and the lower die are closed, so that the last solidified structure in the middle of the extrusion casting preform is flattened and compacted under the action of the forging pressure, plastic deformation occurs, and the structure of the part of the billet close to the lower die is refined; The forging blank is subjected to T6 heat treatment, which specifically includes the following steps: the forging blank is solution treated at 530°C for 3 h, and a box-type air circulation resistance furnace is selected as the heat treatment furnace; then water quenching, followed by artificial aging at 180°C for 6 h, and finally air cooling. Example 3
[0024] according to Figure 1 , 2 As shown in , 3, this embodiment proposes an automobile casting and forging composite process method, comprising the following steps: The alloy material is melted to prepare aluminum alloy liquid, and the chemical composition is determined, and the liquidus and solidus are derived; the specific steps are as follows: the temperature of the medium frequency induction furnace is increased to 400°C; industrial pure aluminum is added, and when the furnace temperature is increased to 720°C, A1-50%Cu master alloy and quick-dissolving silicon are added, and when the furnace temperature is 730°C, A1-5%Ti-1%B is added, and then stirred evenly; after all the furnace materials are melted, they are refined and degassed, allowed to stand, slag is removed, and after adding a covering agent, pure magnesium ingots wrapped with pure aluminum foil are added, stirred evenly, allowed to stand and slag is removed; the alloy liquid is taken with a material spoon for chemical composition determination, and the liquidus and solidus are derived, and then the temperature is kept at 750°C; according to the characteristics of the automobile intake manifold, 6061 aluminum alloy is prepared. 6061 aluminum alloy is a typical heat-treatable and strengthened aluminum alloy. Al-Mg-Si alloy has good plasticity, corrosion resistance, weldability, low quenching sensitivity coefficient and good forming performance, and is more suitable for forging. Its forgings are mainly used in automobiles, motorcycles and yachts. However, for some parts with complex structures, 6061 aluminum alloy belongs to deformed aluminum alloy and has poor casting performance. Generally, it is difficult to produce it by traditional casting processes such as metal mold casting, low-pressure casting and high-pressure casting. This is mainly because it often has defects such as coarse grains, uneven structure and component segregation. Therefore, the process method of the present invention has been verified to effectively force shrinkage compensation and compact structure of squeeze casting preforms and cause them to produce plastic deformation, thereby avoiding defects such as shrinkage cavities, cracks and loose structure.
[0025] Prepare a molding die for the automobile intake manifold and preheat the mold to 300°C; specifically include the following steps: prepare a molding die for the automobile intake manifold, which is a pressure casting mold; clean the inner surface of the molding die to remove dust and oil; preheat the molding die to 00°C through an electric heating tube; keep the molding die warm until the pouring starts; preheat in advance to avoid the influence of the cold mold on the pouring material; The aluminum alloy liquid is poured into the forming mold, and the punch injection speed is controlled to be 60 mm / s; specifically, the following steps are included: before pouring, the temperature of the aluminum alloy liquid is reduced to 30-60°C above the liquidus temperature, the punch head is connected to the pouring port of the forming mold, and the aluminum alloy liquid is introduced into the punch head; a piston is used to apply pressure, and the punch injection speed is controlled to be 60 mm / s; during pouring, the pouring temperature is controlled to be 750°C; when the punch injection speed is 60 mm / s, when the inertia force is large, the liquid flows in a turbulent manner, and the viscous force effectively restricts the longitudinal pulsating flow of the metal liquid particles, thereby effectively curbing the turbulence of the liquid; The filling pressure is controlled to be 150MPa, and the pressure is maintained for 25S, and an extrusion casting preform is obtained after cooling; specifically, the following steps are included: after the aluminum alloy liquid cools with the mold for 5S, the mold punch is driven by the slider of the extrusion casting press to apply a filling pressure of 150MPa to the aluminum alloy liquid in solidification and cooling; the pressure is maintained for 25S, and then the pressure is released, and the extrusion casting preform is obtained; the filling pressure is controlled to be 150MPa, so that the metal liquid between the dendrites fills and flows, and has the characteristics of metal liquid flow in filling rheology. The existence of high pressure conditions during the metal liquid filling process is more conducive to the realization of such extrusion filling, so as to achieve complete filling and eliminate holes. For metals that shrink during solidification, pressurization during solidification is conducive to the solidification of such alloys, that is, more atomic groups participate in nucleation in the metal liquid; The extrusion casting preform is heated to its initial forging temperature, and then placed in the die forging die, the forging pressure is controlled to 130MPa, and the start forging time is controlled to 4S; the specific steps include: heating the extrusion casting preform to its initial forging temperature with a resistance furnace; preheating the upper die and the lower die of the die forging die, and controlling the temperature to 250°C; placing the extrusion casting preform in the die forging die, and controlling the forging pressure to 130MPa; controlling the start forging time to 4S, and shortening the time error to 0.01S; the present invention controls the start forging time to 4S, controls the applied forging pressure to 130MPa, can effectively force the extrusion casting preform to be shrinkage-compensated and compacted and cause it to undergo plastic deformation, and avoids the generation of defects such as shrinkage cavities, cracks and loose tissue. By comparison, it can be seen that Figure 2 , 3 ; Observe whether the upper die and the lower die of the die forging die are closed. When the upper die and the lower die are not closed, the upper die is driven by the slider of the press to strike quickly at a frequency of 40 times / s, and the deformation feed amount of a single strike is 0.5mm, until the upper die and the lower die are closed; after closing, the die is opened to lift the forging blank. After opening the die, the forging blank is processed, the flash generated during the die forging process is trimmed, and the surface is nitrided; the upper die is driven by the slider of the press to strike quickly at a frequency of 40 times / s, and the deformation feed amount of a single strike is 0.5mm, until the upper die and the lower die are closed, so that the last solidified structure in the middle of the extrusion casting preform is flattened and compacted under the action of the forging pressure, and plastic deformation occurs, so that the structure of the part of the billet close to the lower die is refined; The forging blank is subjected to T6 heat treatment, which specifically includes the following steps: the forging blank is solution treated at 530°C for 3 h, and a box-type air circulation resistance furnace is selected as the heat treatment furnace; then water quenching, followed by artificial aging at 180°C for 6 h, and finally air cooling.
[0026] Verification example:
[0027]
[0028] The automobile casting and forging composite process method controls the start forging time to 3-4S, controls the applied forging pressure to 110-130MPa, can effectively force shrinkage compensation and organization density of the extrusion casting preform and make it plastically deformed, avoids the occurrence of defects such as shrinkage holes, cracks and loose organization, and has stronger mechanical properties of the product. In addition, the present invention drives the upper mold to strike quickly at a frequency of 10 times / s-40 times / s through the press slider, and the single strike deformation feed amount is 0.2mm-0.5mm until the upper mold and the lower mold are closed, so that the last solidified organization in the middle of the extrusion casting preform is flattened and compacted under the action of the forging pressure, and plastic deformation occurs, so that the organization of the part of the billet close to the lower mold is refined. At the same time, the present invention controls the punch injection speed to 50-60mm / s; controls the filling pressure to 130-150MPa, and maintains the pressure for 15-25S, so that the real-time pouring and filling is more compact, avoiding the occurrence of defects such as shrinkage holes, cracks and loose organization.
[0029] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention. The scope of protection of the present invention is defined by the attached claims and their equivalents.
Claims
1. Automobile casting and forging composite process method, It is characterized in that The following steps are involved: S1: Melting the alloy material to prepare aluminum alloy liquid, measuring the chemical composition, and deriving the liquidus and solidus; S2: Prepare a molding die suitable for the automobile intake manifold and preheat the die to 250-300°C; S3: pouring aluminum alloy liquid into the forming mold, and controlling the punch injection speed to 50-60 mm / s; S4: Control the filling pressure to 130-150 MPa and maintain the pressure for 15-25 seconds, and obtain the extrusion casting preform after cooling; S5: heating the extrusion casting preform to its initial forging temperature, and then placing it into the die forging die, controlling the forging pressure to 110-130 MPa, and controlling the start forging time to 3-4 seconds; S6: Observe whether the upper die and the lower die of the die forging die are closed. After closing, open the die and lift up the forging blank; S7: Perform T6 heat treatment on the forging blank.
2. The automotive casting and forging composite process according to claim 1, Features: The S1 comprises the following steps: S11: Raise the temperature of the medium frequency induction furnace to 300-400℃; S12: Add industrial pure aluminum, add A1-50%Cu master alloy and quick-dissolving silicon when the furnace temperature rises to 720°C, add A1-5%Ti-1%B at 730°C, and stir evenly; S13: After all the charge is melted, it is refined and degassed, left to stand, slag removed, a covering agent is added, and then a pure magnesium ingot wrapped with pure aluminum foil is added, stirred evenly, and left to stand to remove slag; S14: Take the alloy liquid with a spoon to measure the chemical composition, deduce the liquidus line and solidus line, and then keep it warm at 750℃.
3. The automotive casting and forging composite process according to claim 2, Features: The S2 comprises the following steps: S21: preparing a molding die adapted to the automobile intake manifold, the molding die being a pressure casting die; S22: Clean the inner surface of the molding die to remove dust and oil; S23: preheating the molding die to 250-300° C. through an electric heating tube; S24: The molding mold is kept warm until pouring begins.
4. The automotive casting and forging composite process according to claim 3, Features: The S3 comprises the following steps: S31: connecting the punch head to the pouring port of the forming die, and introducing aluminum alloy liquid into the punch head; S32: Use piston to apply pressure and control the punch injection speed to 50-60mm / s; S33: During pouring, the pouring temperature is controlled to be 750°C.
5. The automotive casting and forging composite process according to claim 4, Features: In S31, before pouring, the temperature of the aluminum alloy liquid is lowered to 30-60° C. above the liquidus temperature.
6. The automotive casting and forging composite process according to claim 5, Features: The S4 comprises the following steps: S41: After the aluminum alloy liquid cools down with the mold for 3-8 seconds, the die punch is driven by the slide of the extrusion casting press to apply a filling pressure of 130-150MPa to the aluminum alloy liquid in solidification and cooling; S42: Maintain pressure for 15-25 seconds, then release pressure and cool at room temperature; S43: Obtain an extrusion casting preform.
7. The automotive casting and forging composite process according to claim 6, Features: The S5 comprises the following steps: S51: heating the squeeze casting preform to its initial forging temperature using a resistance furnace; S52: preheating the upper die and the lower die of the die forging die, and controlling the temperature to be 200° C.-250° C.; S53: placing the extrusion casting preform into a die forging die, and controlling the forging pressure to 110-130 MPa; S54: Control the forging start time to 3-4S and shorten the time error to 0.01S.
8. The automotive casting and forging composite process according to claim 7, Features: In S6, when the upper die and the lower die are not closed, the upper die is driven by the press slide to strike rapidly at a frequency of 10 times / s-40 times / s, with a single strike deformation feed amount of 0.2mm-0.5mm, until the upper die and the lower die are closed.
9. The automotive casting and forging composite process according to claim 8, Features: In S6, after the die is opened, the forging blank is processed, the flash generated during the die forging process is trimmed, and the surface is nitrided.
10. The automotive casting and forging composite process according to claim 9, Features: The S7 comprises the following steps: S71: The forging blank is solution treated at 530℃ for 3 h, and the heat treatment furnace is a box-type air circulation resistance furnace; S72: followed by water quenching, followed by artificial aging at 180°C for 6h, and finally air cooling.
Citation Information
Cited By
Aluminum alloy wheel forging process based on automatic control and digital simulation
CN119304088A